A method for preparing a solder bar
By using specific proportions of tin powder, copper powder, chromium powder and nickel powder in the solder bar, and adding functional flux, the problems of welding firmness and short service life are solved, and the welding performance and production efficiency are improved. improve.
Patent Information
- Application Number
- CN202210252931.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-03-15
AI Technical Summary
The mechanical properties and quality of existing solder bars are insufficient, resulting in poor welding firmness and short service life. The spatter problem during the welding process is difficult to solve, affecting production efficiency.
Tin powder, copper powder, chromium powder and nickel powder are heated and melted according to a specific ratio, and flux is added, including film-forming agent, thixotropic agent, tartaric acid, triisopropanolamine, 2-mercaptobenzothiazole, and antioxidants. and functional additives (such as polyisobutylene or modified polyisobutylene), which are molded through stirring and pouring to remove oxide films and impurities, prevent spatter, and improve welding performance.
It significantly improves the firmness and mechanical properties of the solder joints after welding, reduces spatter adhesion, reduces the cleaning intensity of workers, improves production efficiency, and enhances the tensile strength and elongation of the tin bar.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solder bar research and development, and in particular to a method for preparing the solder bar. Background Art
[0002] Tin is a malleable metal with a wide range of uses. It can be mixed with many metals to synthesize alloy materials with different properties and uses. Commonly added synthetic elements include Ag, Cu, Zn, Bi, Sb, In, etc. Solder alloy powder is an important component of solder bars. The eutectic point temperature of solder alloy powder directly affects the reflow soldering process. In order to ensure the excellent performance of solder bars, most solder alloys are made of eutectic alloys and near-eutectic alloys.
[0003] In actual welding engineering applications, the surface of the metal material being welded has long been oxidized by the atmosphere, and an oxide film of uneven thickness has formed on its surface. It is precisely because of the existence of this oxide film that the molten solder flows on the surface of the pad, resulting in the occurrence of empty solder joints and unsightly solder joints. In the process of soldering, in order to prevent this phenomenon from happening, it is necessary to add a substance that can effectively remove the oxide film on the surface of the pad, accelerate the diffusion of the molten solder on its surface, help welding, and effectively reduce the surface tension between the molten solder and the surface of the metal pad. This material used in conjunction with the solder alloy is called flux.
[0004] A Chinese invention patent (application number: 201510850506.6) discloses a method for making a rosin solder bar, comprising the following steps: (1) crushing and screening metals, including metal nickel, metal copper, metal tin, metal lead and metal bismuth, and ultrafinely crushing the above metals and passing them through a 50-60 mesh sieve; (2) weighing solder bar powder;
[0005] (3) Weighing 10-15 parts of rosin, (4) Melting of solder bar, putting the weighed metal powder into a melting furnace, melting and stirring for the first time until it is completely melted, adding the rosin in step (3), melting and stirring for the second time, (5) casting and molding, pouring the mixture obtained in step (4) into a mold, casting and molding. The method for making rosin solder bar of the present invention is simple to operate, the process is easy to control, and the prepared solder bar has a low melting point, low cost and good use effect. However, this invention patent still does not solve how to improve the mechanical properties and quality of the tin bar itself. Therefore, the preparation process of the solder bar still needs to be improved to prepare high-quality tin bars and increase the service life. Summary of the invention
[0006] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing a solder bar.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0008] A method for preparing a solder bar comprises the following steps: weighing tin powder, copper powder, chromium powder and nickel powder according to weight parts and putting them into a furnace, heating and melting the materials in sequence according to the melting points of the materials, adding flux, stirring at 1000-3000 rpm for 5-15 minutes when all the materials are melted into liquid; removing impurities floating on the molten surface and continuing to stir for 10-30 minutes; pouring into a mold for casting and molding, and cyclic cooling to obtain the solder bar.
[0009] The mass ratio of the tin powder, copper powder, chromium powder, nickel powder and soldering flux is (90-95): (0.5-2): (1-7): (0.4-2): (2-8).
[0010] The soldering flux is composed of the following raw materials in percentage by mass: 20-40% of film former, 5-10% of thixotropic agent, 2-5% of tartaric acid, 2-5% of triisopropanolamine, 0.5-2% of 2-mercaptobenzothiazole, 0.2-1.0% of antioxidant, 5-12% of functional additive, and the balance is organic solvent.
[0011] At room temperature, the surface of the metal to be welded is covered with an oxide film of uneven thickness. This oxide film is relatively dense, and the molten solder itself does not have the ability to remove the oxide film, which hinders the atomic bonding between the molten solder and the metal to be welded. At the same time, because the molten solder and the metal base material to be welded at high temperature are also easily oxidized by the atmosphere, the flux plays an auxiliary role such as protection.
[0012] The activator is a combination of organic acid and organic amine. When the organic amine is used as an activator, the oxide film is removed through -NH. When it is mixed with the organic acid, a neutralization reaction will occur, and the unstable neutralization product will decompose rapidly at the welding temperature to regenerate the organic acid and organic amine. Under the condition of ensuring the original activity of the organic acid, the organic amine is used to neutralize the remaining organic acid, thereby reducing the acidity of the residue and reducing its corrosion to the base material to be welded.
[0013] The functional additive is polyisobutylene or modified polyisobutylene.
[0014] Although the flux used can play a protective role, due to the different melting points and expansion coefficients of the flux and the raw alloy in actual use, the molten droplets burst and produce large splashes during the welding process due to heat, which not only makes the solder joints after welding poorly firm, but also affects the overall mechanical properties of the tin bar; secondly, the splashed metal droplets adhere to the weld and the surrounding parent material, making it difficult to clean. In order to solve this problem, the inventor added a functional additive that can prevent liquid splashing during the welding process, which can effectively solve the problems of short service life caused by poor welding firmness, and can also reduce the time of manual cleaning and improve production efficiency.
[0015] The present invention utilizes polyisobutylene or modified polyisobutylene to significantly reduce the surface energy of the weldment, can effectively wrap impurities in the welding process, prevent the molten droplet from bursting and generating large splashes in the welding process, ensure excellent weld formation, and ensure good flow of weld metal after melting without defects such as local accumulation of weld nodules, incomplete penetration, incomplete fusion, cracks, etc., so that the firmness of the weld after welding is enhanced and the mechanical properties of the tin bar are improved; at the same time, the splash adhesion in the welding process is avoided or the adhesion force is reduced, the work intensity of workers in cleaning the splash is reduced, and the production efficiency is improved.
[0016] Specifically, S1, using polyisobutylene and allyl succinic anhydride as main raw materials, using boron trifluoride etherate as catalyst, and carrying out addition reaction under the condition of petroleum ether as solvent to obtain intermediate product I; S2, further subjecting intermediate product I to silanization modification to provide more effective functional groups to effectively encapsulate impurities, reduce the impurity content during processing, and improve the splash performance of the solution; S3, subjecting intermediate product II prepared in S2 to boronization, the modified polyisobutylene after boronization has good lubrication properties, effectively reduces the friction of the tin bar during welding, reduces welding resistance, and makes the flux have good flow properties, thereby indirectly improving the welding performance of the tin bar.
[0017] Preferably, the functional additive is modified polyisobutylene; the preparation method of the modified polyisobutylene is as follows:
[0018] S1. In a nitrogen environment, 10-30 parts by weight of polyisobutylene, 0.1-1 parts by weight of boron trifluoride ether and 15-30 parts by weight of petroleum ether are mixed, and stirred at room temperature and 500-700 rpm for 20-50 min; then heated to 60-90° C., 3-7 parts by weight of allyl succinic anhydride are added dropwise at a rate of 0.1-0.5 mL / min, and stirring is continued for 8-14 hours after the addition is complete, and distilled under reduced pressure to obtain intermediate product I;
[0019] S2. Under a nitrogen environment, 10-30 parts by weight of the intermediate product I and 15-30 parts by weight of petroleum ether are mixed, and stirred at 50-80°C and 500-700 rpm for 10-30 min; then 0.5-2 parts by weight of aminosilane are added, and the mixture is reacted at 80-120°C for 1.5-5 h, and the petroleum ether is removed by reduced pressure distillation to obtain modified polyisobutylene.
[0020] Preferably, the preparation method of the modified polyisobutylene is as follows:
[0021] S1. In a nitrogen environment, 10-30 parts by weight of polyisobutylene, 0.1-1 parts by weight of boron trifluoride ether and 15-30 parts by weight of petroleum ether are mixed, and stirred at room temperature and 500-700 rpm for 20-50 min; then heated to 60-90° C., 3-7 parts by weight of allyl succinic anhydride are added dropwise at a rate of 0.1-0.5 mL / min, and stirring is continued for 8-14 hours after the addition is complete, and distilled under reduced pressure to obtain intermediate product I;
[0022] S2. Under a nitrogen environment, 10-30 parts by weight of the intermediate product I and 15-30 parts by weight of petroleum ether are mixed, and stirred at 50-80° C. and 500-700 rpm for 10-30 min; 0.5-2 parts by weight of aminosilane are added, and the mixture is reacted at 80-120° C. for 1.5-5 h, and the petroleum ether is removed by reduced pressure distillation to obtain an intermediate product II;
[0023] S3, 12-30 parts by weight of the intermediate product II and 20-40 parts by weight of a 20-50 wt% dimethyl sulfoxide solution of 3-acrylamidophenylboronic acid are uniformly mixed, reacted at 80-110° C. and 300-500 rpm for 2-5 hours, distilled under reduced pressure to remove dimethyl sulfoxide, filtered, and obtained modified polyisobutylene.
[0024] The aminosilane is N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane and / or N-[β-(N,N-diacetoxy)aminoethyl]-γ-(N-acetoxy)aminopropyltrimethoxysilane; preferably, the aminosilane is composed of N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane and N-[β-(N,N-diacetoxy)aminoethyl]-γ-(N-acetoxy)aminopropyltrimethoxysilane in a mass ratio of (1-3):1.
[0025] The present invention utilizes the synergistic effect of N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyl triethoxysilane and / or N-[β-(N,N-diacetoxy)aminoethyl]-γ-(N-acetoxy)aminopropyl trimethoxysilane to effectively reduce the impurity content of the tin bar during the welding process and improve the welding firmness; the polyisobutylene amine modified by N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyl triethoxysilane has hydroxyl groups and molecular polar groups, which makes it easier to form a molecular protective film on the surface of the tin bar. The protective film can prevent deposits from gathering on the metal surface, reduce the mutual friction between the metal surfaces, play a role in reducing friction, and improve the firmness of the connection solder joints of the tin bar during the welding process; and the polyisobutylene amine modified by N-[β-(N,N-diacetoxy)aminoethyl]-γ-(N-acetoxy)aminopropyltrimethoxysilane has a carboxyl group, which can effectively remove the oxide film and other impurities on the surface during the welding process, so that the weld metal flows better after melting, without defects such as local incomplete penetration, incomplete fusion, and cracks, thereby improving the tensile strength and elongation of the tin bar.
[0026] The film-forming agent is any one of maleic rosin, polyethylene oxide, polyethylene glycol, acrylic resin, and rosin acid glyceride; the thixotropic agent is at least one of fatty acid amide, stearyl wax, and hydrogenated castor oil; the solvent is at least one of dipropylene glycol dimethyl ether, triethylene glycol, and tetrahydrofurfuryl alcohol; and the antioxidant is at least one of hydroquinone, alkylphenol disulfide oligomer, and butylated hydroxytoluene.
[0027] A solder bar is prepared by adopting the method.
[0028] Beneficial effects of the present invention:
[0029] 1. The present invention uses tin as the main metal component and copper, zinc and nickel as auxiliary materials to facilitate the formation of solder joints. At the same time, it can also effectively increase the toughness of the solder and the solder joints, and improve the strength of the solder joints. By using a film-forming agent, a thixotropic agent, tartaric acid, triisopropanolamine, 2-mercaptobenzothiazole, an antioxidant, and a functional additive as a soldering flux, during the welding process, oxides and impurities on the surface of the weldment and the pad can be effectively removed, providing a wetting effect for the liquid solder.
[0030] 2. The present invention adds polyisobutylene or modified polyisobutylene as a functional additive in the flux, so that the surface energy of the weldment can be significantly reduced, and impurities in the welding process can be effectively wrapped to prevent the molten droplet from bursting and producing large splashes during the welding process, so that the weld is well formed, the weld metal flows well after melting, and there are no defects such as local accumulation of weld nodules, incomplete penetration, incomplete fusion, and cracks, so that the firmness of the weld after welding is enhanced, and the mechanical properties and compactness of the tin bar are improved; at the same time, the spatter adhesion during the welding process is avoided or the adhesion is reduced, the work intensity of workers in cleaning the spatter is reduced, and the production efficiency is improved. DETAILED DESCRIPTION
[0031] The above content of the present invention is further described in detail below in conjunction with specific implementation modes, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following embodiments.
[0032] Introduction of some raw materials in this application:
[0033] Tin powder, purity 99.5%; copper powder, purity 99.8%; chromium powder, purity 99.9%; nickel powder, purity 99.8%.
[0034] Polyisobutylene was purchased from Jinan Xinwo Chemical Co., Ltd., item number: 2110.
[0035] Malay rosin was purchased from Shanghai Zhenxin Technology Co., Ltd., brand number: 115.
[0036] N-(3-Acryloyloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane, CAS number: 123198-57-2.
[0037] N-[β-(N,N-diacetoxy)aminoethyl]-γ-(N-acetoxy)aminopropyltrimethoxysilane, CAS number: 84127-79-7.
[0038] Example 1
[0039] A preparation method of a solder bar is as follows: 94 parts by weight of tin powder, 1 part by weight of copper powder, 2 parts by weight of chromium powder, and 1 part by weight of nickel powder are put into a furnace, and the materials are heated and melted in sequence according to the melting points of the materials. When all the materials are melted into liquid, 5 parts by weight of flux are added, and the mixture is stirred at 2000 rpm for 10 minutes; impurities floating on the molten surface are removed, and the mixture is stirred for 15 minutes; the mixture is poured into a mold for casting and cooling in a cycle to obtain the solder bar.
[0040] The soldering flux is composed of the following raw materials in percentage by mass: 35% of maleic rosin, 8% of hydrogenated castor oil, 4% of tartaric acid, 4% of triisopropanolamine, 1% of 2-mercaptobenzothiazole, 0.5% of dibutyl hydroxytoluene, 10% of functional additives, and the balance is dipropylene glycol dimethyl ether.
[0041] The functional additive is polyisobutylene.
[0042] Example 2
[0043] A preparation method of a solder bar is as follows: 94 parts by weight of tin powder, 1 part by weight of copper powder, 2 parts by weight of chromium powder, and 1 part by weight of nickel powder are put into a furnace, and the materials are heated and melted in sequence according to the melting points of the materials. When all the materials are melted into liquid, 5 parts by weight of flux are added, and the mixture is stirred at 2000 rpm for 10 minutes; impurities floating on the molten surface are removed, and the mixture is stirred for 15 minutes; the mixture is poured into a mold for casting and cooling in a cycle to obtain the solder bar.
[0044] The soldering flux is composed of the following raw materials in percentage by mass: 35% maleic rosin, 8% hydrogenated castor oil, 4% tartaric acid, 4% triisopropanolamine, 1% 2-mercaptobenzothiazole, 0.5% dibutyl hydroxytoluene, 10% functional additives, and the balance is dipropylene glycol dimethyl ether;
[0045] The functional additive is modified polyisobutylene, and the preparation method of the modified polyisobutylene is as follows:
[0046] In a nitrogen environment, 20 parts by weight of polyisobutylene, 0.3 parts by weight of boron trifluoride ether and 20 parts by weight of petroleum ether were mixed and stirred at room temperature and 600 rpm for 30 min; then heated to 80°C, 5 parts by weight of allyl succinic anhydride were added dropwise at a rate of 0.2 mL / min, and stirring was continued for 10 hours after the addition was completed. The petroleum ether was removed by reduced pressure distillation to obtain modified polyisobutylene.
[0047] Example 3
[0048] A preparation method of a solder bar is as follows: 94 parts by weight of tin powder, 1 part by weight of copper powder, 2 parts by weight of chromium powder, and 1 part by weight of nickel powder are put into a furnace, and the materials are heated and melted in sequence according to the melting points of the materials. When all the materials are melted into liquid, 5 parts by weight of flux are added, and the mixture is stirred at 2000 rpm for 10 minutes; impurities floating on the molten surface are removed, and the mixture is stirred for 15 minutes; the mixture is poured into a mold for casting and cooling in a cycle to obtain the solder bar.
[0049] The soldering flux is composed of the following raw materials in percentage by mass: 35% maleic rosin, 8% hydrogenated castor oil, 4% tartaric acid, 4% triisopropanolamine, 1% 2-mercaptobenzothiazole, 0.5% dibutyl hydroxytoluene, 10% functional additives, and the balance is dipropylene glycol dimethyl ether;
[0050] The functional additive is modified polyisobutylene, and the preparation method of the modified polyisobutylene is as follows:
[0051] S1. Under a nitrogen environment, 20 parts by weight of polyisobutylene, 0.3 parts by weight of boron trifluoride ether and 20 parts by weight of petroleum ether were mixed, and stirred at room temperature and 600 rpm for 30 min; then heated to 80°C, 5 parts by weight of allyl succinic anhydride were added dropwise at a rate of 0.2 mL / min, and stirring was continued for 10 h after the addition was completed, and petroleum ether was removed by vacuum distillation to obtain intermediate product I;
[0052] S2. Under a nitrogen environment, 20 parts by weight of the intermediate product I and 20 parts by weight of petroleum ether were mixed, and the mixture was stirred at 60°C and 600 rpm for 20 min. Then 1.5 parts by weight of N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane was added, and the mixture was reacted at 100°C for 2.5 h. The petroleum ether was removed by distillation under reduced pressure to obtain modified polyisobutylene.
[0053] Example 4
[0054] A preparation method of a solder bar is as follows: 94 parts by weight of tin powder, 1 part by weight of copper powder, 2 parts by weight of chromium powder, and 1 part by weight of nickel powder are put into a furnace, and the materials are heated and melted in sequence according to the melting points of the materials. When all the materials are melted into liquid, 5 parts by weight of flux are added, and the mixture is stirred at 2000 rpm for 10 minutes; impurities floating on the molten surface are removed, and the mixture is stirred for 15 minutes; the mixture is poured into a mold for casting and cooling in a cycle to obtain the solder bar.
[0055] The soldering flux is composed of the following raw materials in percentage by mass: 35% maleic rosin, 8% hydrogenated castor oil, 4% tartaric acid, 4% triisopropanolamine, 1% 2-mercaptobenzothiazole, 0.5% dibutyl hydroxytoluene, 10% functional additives, and the balance is dipropylene glycol dimethyl ether;
[0056] The functional additive is modified polyisobutylene, and the preparation method of the modified polyisobutylene is as follows:
[0057] S1. Under a nitrogen environment, 20 parts by weight of polyisobutylene, 0.3 parts by weight of boron trifluoride ether and 20 parts by weight of petroleum ether were mixed, and stirred at room temperature and 600 rpm for 30 min; then heated to 80°C, 5 parts by weight of allyl succinic anhydride were added dropwise at a rate of 0.2 mL / min, and stirring was continued for 10 h after the addition was completed, and petroleum ether was removed by vacuum distillation to obtain intermediate product I;
[0058] S2. Under a nitrogen environment, 20 parts by weight of the intermediate product I and 20 parts by weight of petroleum ether were mixed, and stirred at 60° C. and 600 rpm for 20 min; 1.5 parts by weight of N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane were added, and the mixture was reacted at 100° C. for 2.5 h, and the petroleum ether was removed by distillation under reduced pressure to obtain an intermediate product II;
[0059] S3. Evenly mix 15 parts by weight of the intermediate product II and 30 parts by weight of a 30 wt% dimethyl sulfoxide solution of 3-acrylamidophenylboronic acid, react at 100° C. and 400 rpm for 3 h, remove dimethyl sulfoxide by reduced pressure distillation, filter, and obtain modified polyisobutylene.
[0060] Example 5
[0061] A preparation method of a solder bar is as follows: 94 parts by weight of tin powder, 1 part by weight of copper powder, 2 parts by weight of chromium powder, and 1 part by weight of nickel powder are put into a furnace, and the materials are heated and melted in sequence according to the melting points of the materials. When all the materials are melted into liquid, 5 parts by weight of flux are added, and the mixture is stirred at 2000 rpm for 10 minutes; impurities floating on the molten surface are removed, and the mixture is stirred for 15 minutes; the mixture is poured into a mold for casting and cooling in a cycle to obtain the solder bar.
[0062] The soldering flux is composed of the following raw materials in percentage by mass: 35% maleic rosin, 8% hydrogenated castor oil, 4% tartaric acid, 4% triisopropanolamine, 1% 2-mercaptobenzothiazole, 0.5% dibutyl hydroxytoluene, 10% functional additives, and the balance is dipropylene glycol dimethyl ether;
[0063] The functional additive is modified polyisobutylene, and the preparation method of the modified polyisobutylene is as follows:
[0064] S1. Under a nitrogen environment, 20 parts by weight of polyisobutylene, 0.3 parts by weight of boron trifluoride ether and 20 parts by weight of petroleum ether were mixed, and stirred at room temperature and 600 rpm for 30 min; then heated to 80°C, 5 parts by weight of allyl succinic anhydride were added dropwise at a rate of 0.2 mL / min, and stirring was continued for 10 h after the addition was completed, and petroleum ether was removed by vacuum distillation to obtain intermediate product I;
[0065] S2. Under a nitrogen environment, 20 parts by weight of the intermediate product I and 20 parts by weight of petroleum ether were mixed, and stirred at 60° C. and 600 rpm for 20 min; 1.5 parts by weight of N-[β-(N,N-diacetoxy)aminoethyl]-γ-(N-acetoxy)aminopropyltrimethoxysilane were added, and the mixture was reacted at 100° C. for 2.5 h, and the petroleum ether was removed by distillation under reduced pressure to obtain an intermediate product II;
[0066] S3. Evenly mix 15 parts by weight of the intermediate product II and 30 parts by weight of a 30 wt% dimethyl sulfoxide solution of 3-acrylamidophenylboronic acid, react at 100° C. and 400 rpm for 3 h, remove dimethyl sulfoxide by reduced pressure distillation, filter, and obtain modified polyisobutylene.
[0067] Example 6
[0068] A preparation method of a solder bar is as follows: 94 parts by weight of tin powder, 1 part by weight of copper powder, 2 parts by weight of chromium powder, and 1 part by weight of nickel powder are put into a furnace, and the materials are heated and melted in sequence according to the melting points of the materials. When all the materials are melted into liquid, 5 parts by weight of flux are added, and the mixture is stirred at 2000 rpm for 10 minutes; impurities floating on the molten surface are removed, and the mixture is stirred for 15 minutes; the mixture is poured into a mold for casting and cooling in a cycle to obtain the solder bar.
[0069] The soldering flux is composed of the following raw materials in percentage by mass: 35% maleic rosin, 8% hydrogenated castor oil, 4% tartaric acid, 4% triisopropanolamine, 1% 2-mercaptobenzothiazole, 0.5% dibutyl hydroxytoluene, 10% functional additives, and the balance is dipropylene glycol dimethyl ether;
[0070] The functional additive is modified polyisobutylene, and the preparation method of the modified polyisobutylene is as follows:
[0071] S1. Under a nitrogen environment, 20 parts by weight of polyisobutylene, 0.3 parts by weight of boron trifluoride ether and 20 parts by weight of petroleum ether were mixed, and stirred at room temperature and 600 rpm for 30 min; then heated to 80°C, 5 parts by weight of allyl succinic anhydride were added dropwise at a rate of 0.2 mL / min, and stirring was continued for 10 h after the addition was completed, and petroleum ether was removed by vacuum distillation to obtain intermediate product I;
[0072] S2. Under a nitrogen environment, 20 parts by weight of the intermediate product I and 20 parts by weight of petroleum ether were mixed, and stirred at 60° C. and 600 rpm for 20 min; 1 part by weight of N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane and 0.5 parts by weight of N-[β-(N,N-diacetoxy)aminoethyl]-γ-(N-acetoxy)aminopropyltrimethoxysilane were added, and the mixture was reacted at 100° C. for 2.5 h, and the petroleum ether was removed by distillation under reduced pressure to obtain an intermediate product II;
[0073] S3. Evenly mix 15 parts by weight of the intermediate product II and 30 parts by weight of a 30 wt% dimethyl sulfoxide solution of 3-acrylamidophenylboronic acid, react at 100° C. and 400 rpm for 3 h, remove dimethyl sulfoxide by reduced pressure distillation, filter, and obtain modified polyisobutylene.
[0074] Test Example 1
[0075] Tensile strength and elongation test: The prepared solder bar was subjected to tensile strength and elongation test on Shimadzu precision electronic material universal testing machine (CMT4305), with a tensile speed of 0.5 mm / s, sample thickness: 1.0 mm, width 3.2 mm, parallel length 10 mm, gauge length 5 mm, and strain rate 10 -3 s -1Each sample was tested 5 times and the average value was taken. The results are shown in Table 1.
[0076] Tensile strength / MPa Elongation(%) Example 1 65.8 41 Example 2 76.1 45 Example 3 90.3 55 Example 4 98.4 59 Example 5 97.5 58 Example 6 101.3 62
[0077] From the above results, it can be seen that the tin bar prepared by the present invention has good tensile properties and elongation. The present invention uses polyisobutylene or modified polyisobutylene to significantly reduce the surface energy of the weldment, can effectively wrap impurities in the welding process, prevent the molten droplet from bursting and producing large splashes during the welding process, so that the weld is well formed, the weld metal flows well after melting, and there are no defects such as local accumulation of weld nodules, incomplete welding, incomplete fusion, cracks, etc., so that the firmness of the solder joint after welding is enhanced, and the mechanical properties of the tin bar are improved; at the same time, the splash adhesion or reduced adhesion during the welding process is avoided, the work intensity of workers cleaning splashes is reduced, and production efficiency is improved. The modified polyisobutylene after boronization has good lubrication properties, effectively reduces the friction of the tin bar during the welding process, reduces welding resistance, and makes the flux have good flow properties, which indirectly improves the welding performance of the tin bar.
[0078] Example 6 The synergistic effect of N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane and / or N-[β-(N,N-diacetoxy)aminoethyl]-γ-(N-acetoxy)aminopropyltrimethoxysilane is used to effectively reduce the impurity content of the tin bar during the welding process and improve the firmness of the welding; the polyisobutylene amine modified by N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane has hydroxyl groups and molecular polar groups, which makes it easier to form a molecular protective film on the surface of the tin bar. This layer The protective film can prevent deposits from gathering on the metal surface, reduce the mutual friction between the metal surfaces, play a role in reducing friction, and improve the firmness of the connection solder joints of the tin bar during the welding process; and the polyisobutylene amine modified by N-[β-(N,N-diacetoxy)aminoethyl]-γ-(N-acetoxy)aminopropyltrimethoxysilane has a carboxyl group, which can effectively remove the oxide film and other impurities on the surface during the welding process, so that the weld metal flows better after melting, without defects such as local incomplete penetration, incomplete fusion, and cracks, thereby improving the tensile strength and elongation of the tin bar.
[0079] Test Example 2
[0080] Void rate test: Reflow soldering and X-ray detection method are used to perform void rate test, where void rate = (S1-S2) / S1, where S1 is the solderable area of the chip and S2 is the actual soldering area of the chip.
[0081] Void rate (%) Example 1 19.2 Example 2 12.5 Example 6 5.1
[0082] The present invention can effectively reduce the impurity content in the welding process by adding flux during the soldering process. The prepared tin bar can not only effectively reduce the phenomenon of poor welding quality caused by excessive welding residues and welding "voids", but also effectively reduce the oxidation rate of metal raw materials, thereby ensuring the welding quality.
Claims
1. A method for preparing a solder bar, characterized in that: The method comprises the following steps: putting tin powder, copper powder, chromium powder and nickel powder into a furnace, heating and melting the materials in turn according to their melting points, and adding flux and stirring when all the materials are melted into liquid; Remove impurities floating on the molten surface; Pour the mixture into a mold, cast it, and cool it in a cycle to obtain the solder bar; The soldering flux is composed of the following raw materials in percentage by weight: 20-40% of a film former, 5-10% of a thixotropic agent, 2-5% of tartaric acid, 2-5% of triisopropanolamine, 0.5-2% of 2-mercaptobenzothiazole, 0.2-1.0% of an antioxidant, 5-12% of a functional additive, and the balance is an organic solvent; The functional additive is modified polyisobutylene; The preparation method of the modified polyisobutylene is as follows: S1. In a nitrogen environment, 10-30 parts by weight of polyisobutylene, 0.1-1 parts by weight of boron trifluoride ether and 15-30 parts by weight of petroleum ether are mixed and stirred at room temperature; 3-7 parts by weight of allyl succinic anhydride are added dropwise at 60-90° C., stirring is continued for 8-14 hours after the addition is complete, and distillation is performed under reduced pressure to obtain intermediate product I; S2. Under a nitrogen environment, 10-30 parts by weight of the intermediate product I and 15-30 parts by weight of petroleum ether are mixed, and stirred at 50-80° C.; 0.5-2 parts by weight of aminosilane are added, and the mixture is reacted at 80-120° C. for 1.5-5 hours, and distilled under reduced pressure to obtain an intermediate product II; S3, 12-30 parts by weight of the intermediate product II and 20-40 parts by weight of a dimethyl sulfoxide solution of 3-acrylamidophenylboronic acid are uniformly mixed, reacted at 80-110° C. for 2-5 hours, distilled under reduced pressure, filtered, and modified polyisobutylene is obtained; The mass ratio of the tin powder, copper powder, chromium powder, nickel powder and soldering flux is (90-95): (0.5-2): (1-7): (0.4-2): (2-8).
2. The method for preparing a solder bar according to claim 1, characterized in that: The aminosilane is N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane and / or N-[β-(N,N-diacetoxy)aminoethyl]-γ-(N-acetoxy)aminopropyltrimethoxysilane.
3. The method for preparing a solder bar according to claim 1, characterized in that: The mass fraction of the dimethyl sulfoxide solution of 3-acrylamidophenylboronic acid is 20-50wt%.
4. The method for preparing a solder bar according to claim 1, characterized in that: The film-forming agent is any one of maleic rosin, polyethylene oxide, polyethylene glycol, acrylic resin, and rosin acid glyceride; the thixotropic agent is at least one of fatty acid amide, stearyl wax, and hydrogenated castor oil; the solvent is at least one of dipropylene glycol dimethyl ether, triethylene glycol, and tetrahydrofurfuryl alcohol; and the antioxidant is at least one of hydroquinone, alkylphenol disulfide oligomer, and butylated hydroxytoluene.
5. A solder bar, characterized in that: The method is prepared by any one of claims 1 to 4.