A preparation method and application of carbon quantum dot polylactic acid oligomer

By using carbon quantum dot polylactic acid oligomers as toughening fillers or crosslinking agents in polylactic acid materials, the problem of low elongation of breaking polylactic acid materials is solved, and its mechanical properties and thermal stability are improved while maintaining the The color and dispersion of the materials are suitable for packaging and medical fields.

CN114410093BActive Publication Date: 2024-11-15SHENZHEN FAYMO TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210155621.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-18
Publication Date
2024-11-15
Estimated Expiration
2042-02-18

AI Technical Summary

Technical Problem

The low elongation of polylactic acid materials in breaking limits its application in some fields. In addition, carbon nanotubes have poor dispersion and great influence on color in PLA substrates, making it difficult to meet the requirements of packaging and medical applications.

Method used

Carbon quantum dots are prepared by cutting carbon nanotubes into mixed acids of concentrated sulfuric acid and concentrated nitric acid, and mixing them uniformly with lactic acid to control reaction temperature and gas protection, carbon quantum dot polylactic acid oligomers are prepared as toughening fillers or The crosslinking agent is mixed with polylactic acid material to increase its elongation of break.

Benefits of technology

It significantly improves the elongation of the break of polylactic acid materials from the original 10% to 100%-200%, and keeps the color of the material's matrix unchanged, enhancing its mechanical properties and thermal stability, and avoiding carbon quantum dots falling off .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114410093B_ABST
    Figure CN114410093B_ABST
Patent Text Reader

Abstract

The invention belongs to the field of chemical material technology, and is specifically related to a method for preparing a carbon quantum dot polylactic acid oligomer and its application, wherein the method for preparing a carbon quantum dot polylactic acid oligomer includes adding carbon nanotubes to a mixed acid of concentrated sulfuric acid and concentrated nitric acid for reaction, and then filtering and dialyzing the reacted solution to obtain a carbon quantum dot aqueous solution containing carboxyl and hydroxyl groups; Lactic acid and the carbon quantum dot aqueous solution obtained in step one are mixed evenly, and then the water in the mixed solution is evaporated to obtain a carbon quantum dot lactic acid solution; A catalyst is added to the carbon quantum dot lactic acid solution and stirred evenly, and the reaction temperature is controlled to be 140-150°C, and an inert gas is passed through the entire reaction process for protection to obtain a carbon quantum dot polylactic acid oligomer crude product; Chloroform and acetone solution are added to the carbon quantum dot polylactic acid oligomer crude product, and carbon quantum dot polylactic acid oligomers are extracted. The preparation method is simple, and can be used as a toughening filler or crosslinking agent for polylactic acid materials to improve the elongation at break of polylactic acid materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical materials, and specifically relates to a preparation method of a carbon quantum dot polylactic acid oligomer and application thereof. Background Art

[0002] As people's environmental awareness continues to improve, the biodegradability of plastics has attracted more and more attention from researchers. Polylactic acid (PLA), as a relatively mature biodegradable plastic and biocompatible, is widely used in 3D printing consumables, packaging materials, medical devices, daily necessities and other fields. With the launch of products in the fields of 3D printing and packaging, the production of PLA has increased year by year, further expanding the application of PLA in biodegradable plastics.

[0003] PLA is a thermoplastic polymer material that can be processed by extrusion, blow molding, molding and other processing methods. It can replace the current petroleum-based polymer materials and solve the energy and environmental pollution problems. However, PLA is brittle and has a low elongation at break (less than 10%), which limits the application of PLA materials in some fields.

[0004] As an inorganic nanomaterial, carbon nanotubes have been widely used as conductive agents for lithium-ion batteries in recent years and have attracted much attention. Carbon nanotubes are a type of one-dimensional nanomaterial composed of carbon atoms in a six-membered ring and then curled up. They have excellent mechanical properties, conductivity and thermal stability, and can significantly improve the thermodynamic properties of PLA. Carbon nanotubes have a large aspect ratio and only contain a small amount of hydrophilic groups on the surface. Although they have good compatibility with PLA, there is a problem of dispersibility of carbon nanotubes in the PLA matrix that is difficult to solve. Modifying PLA with carbon nanotubes will affect the color of the PLA material, and in packaging, medical and other applications, there are high requirements for product color, powder loss and other issues. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a carbon quantum dot polylactic acid oligomer and application thereof, aiming to solve the technical problem of low elongation at break of PLA.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0007] On the one hand, the present invention provides a method for preparing carbon quantum dot polylactic acid oligomer, which comprises the following preparation steps:

[0008] Step 1: adding carbon nanotubes to a mixed acid of concentrated sulfuric acid and concentrated nitric acid for reaction, and then filtering and dialyzing the solution after the reaction to obtain a carbon quantum dot aqueous solution containing carboxyl and hydroxyl groups;

[0009] Step 2, uniformly mixing lactic acid and the carbon quantum dot aqueous solution obtained in step 1, and then evaporating the water in the mixed solution to obtain a carbon quantum dot lactic acid solution;

[0010] Step 3: Add a catalyst to the carbon quantum dot lactic acid solution and stir evenly, control the reaction temperature to 140-150° C., and pass an inert gas throughout the reaction for protection to obtain a carbon quantum dot polylactic acid oligomer crude product;

[0011] Step 4: Add chloroform and acetone solution to the crude carbon quantum dot polylactic acid oligomer product to extract the carbon quantum dot polylactic acid oligomer.

[0012] The preparation method of the carbon quantum dot polylactic acid oligomer of the present invention is simple. The prepared carbon quantum dot polylactic acid oligomer has high toughness and can be used as a polylactic acid toughening filler or a cross-linking agent. The carbon quantum dot polylactic acid oligomer is mixed with a polylactic acid material to effectively improve the elongation at break of the polylactic acid material, and the elongation at break of the polylactic acid material is increased from the original 10% to 100%-200%. The polylactic acid oligomer prepared by the preparation method of the present invention is compounded with the polylactic acid material without changing the matrix color of the polylactic acid material. In addition, since the carbon quantum dots are loaded with oligomeric polylactic acid, the interface with the polylactic acid matrix is ​​facilitated, so that the carbon quantum dots are not easy to fall off in the polylactic acid matrix.

[0013] Another aspect of the present invention provides an application of a carbon quantum dot polylactic acid oligomer, wherein the carbon quantum dot polylactic acid oligomer is melt-blended with polylactic acid to prepare a polylactic acid composite material.

[0014] By melt-mixing carbon quantum dot polylactic acid oligomers with polylactic acid materials, the prepared polylactic acid nanocomposite material has increased molecules, the carbon quantum dots play a certain cross-linking role, and the polylactic acid is partially cross-linked to form a branched structure. During the stretching process, the crystallinity is improved, and the mechanical properties and thermal stability of the composite material are improved. The elongation at break of the polylactic acid composite material is increased from the original 10% to 100%-200%.

[0015] Beneficial effects of the present invention:

[0016] The preparation method of the carbon quantum dot polylactic acid oligomer of the present invention is simple. The prepared carbon quantum dot polylactic acid oligomer has high toughness and can be used as a polylactic acid toughening filler or a cross-linking agent. The carbon quantum dot polylactic acid oligomer is mixed with a polylactic acid material to effectively improve the elongation at break of the polylactic acid material, and the elongation at break of the polylactic acid material is increased from the original 10% to 100%-200%. The polylactic acid oligomer prepared by the preparation method of the present invention is compounded with the polylactic acid material without changing the matrix color of the polylactic acid material. In addition, since the carbon quantum dots are loaded with oligomeric polylactic acid, the interface with the polylactic acid matrix is ​​facilitated, so that the carbon quantum dots are not easy to fall off in the polylactic acid matrix.

[0017] By melt-mixing carbon quantum dot polylactic acid oligomers with polylactic acid materials, the prepared polylactic acid nanocomposite material has increased molecules, the carbon quantum dots play a certain cross-linking role, and the polylactic acid is partially cross-linked to form a branched structure. During the stretching process, the crystallinity is improved, and the mechanical properties and thermal stability of the composite material are improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Schematic diagram of the grafting mechanism of carbon quantum dots and lactic acid molecules according to an embodiment of the present invention;

[0019] Figure 2 Schematic diagram of the mechanism of forming a polylactic acid composite material from carbon quantum dot polylactic acid oligomer and polylactic acid according to an embodiment of the present invention; DETAILED DESCRIPTION

[0020] In order to make the purpose, technical scheme and technical effect of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention is clearly and completely described. The embodiments described below are part of the embodiments of the present invention, rather than all of the embodiments. In conjunction with the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or the conditions recommended by the manufacturer; if the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0021] In the description of the present invention, the term "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.

[0022] In the description of the present invention, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple, respectively.

[0023] It should be understood that the weight of the relevant components mentioned in the embodiments of the present invention can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components in the embodiments of the present invention is proportionally enlarged or reduced, it is within the scope disclosed by the present invention. Specifically, the weight described in the embodiments of the present invention can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0024] In addition, unless the context clearly uses otherwise, the expression of the singular form of a word should be understood to include the plural form of the word. The term "includes" or "having" is intended to specify the existence of a feature, quantity, step, operation, element, part or combination thereof, but is not used to exclude the existence or possible addition of one or more other features, quantities, steps, operations, elements, parts or combinations thereof.

[0025] The embodiment of the present invention provides a method for preparing a carbon quantum dot polylactic acid oligomer, which comprises the following preparation steps:

[0026] Step 1: adding carbon nanotubes to a mixed acid of concentrated sulfuric acid and concentrated nitric acid for reaction, and then filtering and dialyzing the solution after the reaction to obtain a carbon quantum dot aqueous solution containing carboxyl and hydroxyl groups;

[0027] Step 2, uniformly mixing lactic acid and the carbon quantum dot aqueous solution obtained in step 1, and then evaporating the water in the mixed solution to obtain a carbon quantum dot lactic acid solution;

[0028] Step 3: Add a catalyst to the carbon quantum dot lactic acid solution and stir evenly, control the reaction temperature to 140-150° C., and pass an inert gas throughout the reaction for protection to obtain a carbon quantum dot polylactic acid oligomer crude product;

[0029] Step 4: Add chloroform and acetone solution to the crude carbon quantum dot polylactic acid oligomer product to extract the carbon quantum dot polylactic acid oligomer.

[0030] The carbon quantum dot polylactic acid oligomer preparation method of the present invention is simple. The prepared carbon quantum dot polylactic acid oligomer has high toughness and can be used as a toughening filler or crosslinking agent for polylactic acid. The carbon quantum dot polylactic acid oligomer is mixed with a polylactic acid material to effectively improve the elongation at break of the polylactic acid material, and the elongation at break of the polylactic acid material is increased from the original 10% to 100%-200%. The polylactic acid oligomer prepared by the preparation method of the present invention is compounded with the polylactic acid material without changing the matrix color of the polylactic acid material. In addition, since the carbon quantum dots are loaded with oligomeric polylactic acid, such as Figure 1 , which is conducive to the interface interaction with the polylactic acid matrix, making it difficult for the carbon quantum dots to fall off in the polylactic acid matrix.

[0031] The preparation method of the present invention first uses carbon nanotubes as a precursor, then uses a mixed acid of concentrated sulfuric acid and concentrated nitric acid as a cutting agent to cut the carbon nanotubes, so that the carbon nanotubes form smaller carbon quantum dots, then filters out the uncut carbon nanotubes, and removes excess acid by dialysis, so that the solution forms a carbon quantum dot aqueous solution containing carboxyl and hydroxyl groups with a pH value of 6-7. The carbon quantum dots prepared by the method have a high yield, a small size, and contain oxygen-containing functional groups such as carboxyl and hydroxyl groups, which are conducive to use as functionalization and cross-linking agents.

[0032] By uniformly mixing lactic acid and carbon quantum dot aqueous solution and then evaporating the water in the mixed solution, compared with directly mixing lactic acid with carbon quantum dots, the method of the present invention is more conducive to uniform mixing of lactic acid and carbon quantum dots, which is beneficial to the subsequent formation of polylactic acid and the reaction of carbon quantum dots and polylactic acid.

[0033] By adding a catalyst to the carbon quantum dot lactic acid solution and controlling the reaction temperature to 140-150°C, the reaction is facilitated to proceed smoothly and the reaction speed is accelerated. Stirring is conducive to the full reaction of carbon quantum dots, lactic acid and catalyst. The introduction of inert gas can, on the one hand, take away the moisture in the reaction system, accelerate the speed of the forward reaction, improve the synthesis efficiency of polylactic acid, and further promote the reaction of polylactic acid and carbon quantum dots. On the other hand, it can avoid the hydrolysis and oxidation of the generated polylactic acid. Step 4: After extracting the carbon quantum dot polylactic acid oligomer produced in step 3, the carbon quantum dot polylactic acid oligomer can be obtained, which can be used as a polylactic acid toughening filler or crosslinking agent.

[0034] In step 1, after the carbon nanotubes are added to the mixed acid and mixed, ultrasonic treatment is performed for 20-40 minutes. The carbon nanotubes and the mixed acid can be dispersed by ultrasonic treatment, which is conducive to the full progress of the reaction. Specifically, the ultrasonic power is 90-110W.

[0035] Among them, in step 1, when the carbon nanotubes and the mixed acid react, they are refluxed at 60-80°C for more than 24 hours. By controlling the temperature at 60-80°C, it is beneficial for the reaction to proceed smoothly and quickly, so that the carbon nanotubes are cut to form carbon quantum dots. When the temperature is too high, the reaction system is prone to boiling and the nitric acid will decompose.

[0036] Wherein, in step 1, the concentration of the concentrated sulfuric acid is greater than or equal to 98%, the concentration of the concentrated nitric acid is 14-15 mol / L, the mass ratio of concentrated sulfuric acid to concentrated nitric acid is 1-3:1, and every 0.5-1 g of carbon nanotubes is added to 100-500 mL of the mixed acid for reaction.

[0037] In step 2, after the lactic acid and the carbon quantum dot aqueous solution are mixed, ultrasonic treatment is performed for 20-40 minutes to disperse the lactic acid and the carbon nanotubes and mix them evenly, and the ultrasonic power is 90-110W.

[0038] In step 2, after the lactic acid and the carbon quantum dot aqueous solution are evenly mixed, the water in the mixed solution is evaporated by continuous vacuum at 60-70°C.

[0039] Wherein, in step 2, the mass ratio of lactic acid to carbon quantum dot aqueous solution is 5-20:2-10.

[0040] The catalyst is stannous octoate or stannous chloride. Specifically, the amount of the catalyst added is 0.1%-0.5% of the mass of the carbon quantum dot lactic acid solution.

[0041] Wherein, the inert gas is at least one of nitrogen and argon.

[0042] Wherein, in step three, the reaction time is 24-48h.

[0043] Wherein, in step 4, the amount of chloroform is 50-150 mL, the amount of acetone is 40-150 mL, and the carbon quantum dot polylactic acid oligomer is separated under the condition of 4000-6000 rpm.

[0044] Another aspect of the present invention provides an application of a carbon quantum dot polylactic acid oligomer, wherein the carbon quantum dot polylactic acid oligomer is melt-blended with polylactic acid to prepare a polylactic acid composite material.

[0045] Wherein, the mass ratio of the carbon quantum dot polylactic acid oligomer to polylactic acid is 1-20:100.

[0046] Wherein, the melting temperature is 170-180°C.

[0047] By melt-mixing carbon quantum dot polylactic acid oligomers and polylactic acid materials, the prepared polylactic acid nanocomposite molecules increase, the carbon quantum dots play a certain cross-linking role, and the polylactic acid is partially cross-linked to form a branched structure (such as Figure 2 ), during the stretching process, the crystallinity is improved, and the mechanical properties and thermal stability of the composite material are improved, and the elongation at break of the polylactic acid composite material is increased from the original 10% to 100%-200%.

[0048] In order to enable those skilled in the art to clearly understand the implementation details and operations of the present invention, and to significantly demonstrate the improved performance of the embodiments of the present invention, the above technical solutions are illustrated by multiple embodiments below.

[0049] Example 1

[0050] A method for preparing a carbon quantum dot polylactic acid oligomer comprises the following preparation steps:

[0051] Step 1, adding 0.5g of carbon nanotubes to a mixed acid of 100mL of concentrated sulfuric acid and concentrated nitric acid, then ultrasonicating for 20min at a power of 90W, then reacting and reflux at 60°C for more than 24h, then filtering and dialyzing the solution after the reaction to remove large particles and acid, and obtaining a carbon quantum dot aqueous solution containing carboxyl and hydroxyl groups; wherein the concentration of the concentrated sulfuric acid is equal to 98%, the concentration of the concentrated nitric acid is 14mol / L, and the mass ratio of the concentrated sulfuric acid to the concentrated nitric acid is 1:1;

[0052] Step 2: Place 25 g of lactic acid in an evaporating bottle of a rotary evaporator, and take 10 g of the carbon quantum dot aqueous solution obtained in step 1 and place it in the evaporating bottle, then ultrasonicate for 20 min at an ultrasonic power of 90 W to mix the solution evenly, then continue to vacuumize at 60 ° C to evaporate the water in the mixed solution to obtain a carbon quantum dot lactic acid solution;

[0053] Step 3: Add the above carbon quantum dot lactic acid solution to a 500 mL single-necked flask, add stannous octoate or stannous chloride catalyst, stir evenly with magnetic force, control the reaction temperature to 140 ° C, and pass nitrogen or argon inert gas throughout the reaction for protection. React for 24 hours to obtain a crude carbon quantum dot polylactic acid oligomer product; wherein the amount of the catalyst added is 0.1% of the mass of the carbon quantum dot lactic acid solution;

[0054] Step 4: Add 50 mL of chloroform and 40 mL of acetone solution to the crude carbon quantum dot polylactic acid oligomer product, separate and extract the carbon quantum dot polylactic acid oligomer at 4000 rpm, and place the separated carbon quantum dot polylactic acid oligomer in a 60°C vacuum drying oven for 24 hours to remove residual acetone, thereby obtaining the carbon quantum dot polylactic acid oligomer.

[0055] The above carbon quantum dot polylactic acid oligomer is applied by taking 1 g of the carbon quantum dot polylactic acid oligomer and 100 g of polylactic acid and melt-blending them at 170° C. until the torque is stable, then taking them out and performing compression molding to obtain a polylactic acid nanocomposite material.

[0056] Example 2

[0057] A method for preparing a carbon quantum dot polylactic acid oligomer comprises the following preparation steps:

[0058] Step 1, adding 0.75g of carbon nanotubes to a mixed acid of 300mL of concentrated sulfuric acid and concentrated nitric acid, then ultrasonicating for 30min at a power of 100W, then reacting and reflux at 70°C for more than 24h, then filtering and dialyzing the solution after the reaction to remove large particles and acid, and obtaining a carbon quantum dot aqueous solution containing carboxyl and hydroxyl groups; wherein the concentration of the concentrated sulfuric acid is equal to 98%, the concentration of the concentrated nitric acid is 14.5mol / L, and the mass ratio of concentrated sulfuric acid to concentrated nitric acid is 2:1;

[0059] Step 2: Place 57 g of lactic acid in an evaporating bottle of a rotary evaporator, and take 30 g of the carbon quantum dot aqueous solution obtained in step 1 and put it into the evaporating bottle, then ultrasonicate for 30 min at an ultrasonic power of 100 W to mix the solution evenly, then continue to vacuum at 65 ° C to evaporate the water in the mixed solution to obtain a carbon quantum dot lactic acid solution;

[0060] Step 3: Add the above carbon quantum dot lactic acid solution to a 500mL single-necked flask, add stannous octoate catalyst, stir evenly with magnetic force, control the reaction temperature to 145°C, and pass nitrogen or argon inert gas throughout the reaction for protection. React for 36 hours to obtain a crude carbon quantum dot polylactic acid oligomer product; wherein the amount of the catalyst added is 0.3% of the mass of the carbon quantum dot lactic acid solution;

[0061] Step 4: Add 100 mL of chloroform and 95 mL of acetone solution to the crude carbon quantum dot polylactic acid oligomer product, separate and extract the carbon quantum dot polylactic acid oligomer at 5000 rpm, and place the separated carbon quantum dot polylactic acid oligomer in a 60°C vacuum drying oven for 24 hours to remove residual acetone, thereby obtaining the carbon quantum dot polylactic acid oligomer.

[0062] The above carbon quantum dot polylactic acid oligomer is used. 10 g of the carbon quantum dot polylactic acid oligomer is melt-blended with 100 g of polylactic acid at 175° C. until the torque is stable, and then the mixture is taken out and compression molded to obtain a polylactic acid nanocomposite material.

[0063] Example 3

[0064] A method for preparing a carbon quantum dot polylactic acid oligomer comprises the following preparation steps:

[0065] Step 1, add 1g of carbon nanotubes to a mixed acid of 500mL of concentrated sulfuric acid and concentrated nitric acid, then ultrasonicate for 40min at a power of 110W, then reflux at 80°C for more than 24h, then filter and dialyze the solution after the reaction to remove large particles and acid, and obtain a carbon quantum dot aqueous solution containing carboxyl and hydroxyl groups; wherein the concentration of the concentrated sulfuric acid is equal to 98%, the concentration of the concentrated nitric acid is 15mol / L, and the mass ratio of concentrated sulfuric acid to concentrated nitric acid is 3:1;

[0066] Step 2: Place 100 g of lactic acid in an evaporating bottle of a rotary evaporator, and take 50 g of the carbon quantum dot aqueous solution obtained in step 1 and put it into the evaporating bottle, then ultrasonicate for 40 min at an ultrasonic power of 110 W to mix the solution evenly, and then continue to vacuumize at 70 ° C to evaporate the water in the mixed solution to obtain a carbon quantum dot lactic acid solution;

[0067] Step 3: Add the above carbon quantum dot lactic acid solution to a 500 mL single-necked flask, add stannous octoate or stannous chloride catalyst, stir evenly with magnetic force, control the reaction temperature to 150 ° C, and pass nitrogen or argon inert gas throughout the reaction for protection. React for 48 hours to obtain a crude carbon quantum dot polylactic acid oligomer product; wherein the amount of the catalyst added is 0.5% of the mass of the carbon quantum dot lactic acid solution;

[0068] Step 4: Add 150 mL of chloroform and 150 mL of acetone solution to the crude carbon quantum dot polylactic acid oligomer product, separate and extract the carbon quantum dot polylactic acid oligomer at 6000 rpm, and place the separated carbon quantum dot polylactic acid oligomer in a 60°C vacuum drying oven for 24 hours to remove residual acetone, thereby obtaining the carbon quantum dot polylactic acid oligomer.

[0069] The above carbon quantum dot polylactic acid oligomer is used. 20 g of the carbon quantum dot polylactic acid oligomer is melt-blended with 100 g of polylactic acid at 180° C. until the torque is stable, and then taken out and compression molded to obtain a polylactic acid nanocomposite material.

[0070] Performance Testing

[0071] The polylactic acid composite materials prepared in Examples 1-3 were cut into specimens of the same size, each of which was a 5 cm × 5 cm × 0.5 cm rectangular piece. Five specimens were prepared for each example, and then the tensile strength of the specimens of Examples 1-3 was tested under the same conditions, and then the average tensile strength of the specimens of Examples 1-3 was calculated.

[0072] After testing, the average tensile strength of the sample of Example 1 was 100%, the average tensile strength of the sample of Example 2 was 170%, and the average tensile strength of the sample of Example 3 was 200%.

[0073] It can be seen that the carbon quantum dot polylactic acid oligomer prepared by the preparation method of the present invention can effectively improve the tensile strength of the polylactic acid material, and can be used as a toughening agent for the polylactic acid material with a good toughening effect.

[0074] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing carbon quantum dot polylactic acid oligomer, characterized in that: The method comprises the following preparation steps: Step 1, adding carbon nanotubes to a mixed acid of concentrated sulfuric acid and concentrated nitric acid for reaction, and refluxing at 60-80° C. for more than 24 hours, wherein the mixed acid of concentrated sulfuric acid and concentrated nitric acid acts as a cutting agent to cut the carbon nanotubes to form carbon quantum dots during the reaction, and then filtering and dialyzing the solution after the reaction to filter out the uncut carbon nanotubes, thereby obtaining a carbon quantum dot aqueous solution containing carboxyl and hydroxyl groups; Step 2, uniformly mixing lactic acid and the carbon quantum dot aqueous solution obtained in step 1, and then evaporating the water in the mixed solution to obtain a carbon quantum dot lactic acid solution; Step 3: Add a catalyst to the carbon quantum dot lactic acid solution and stir evenly, control the reaction temperature to 140-150° C., and pass an inert gas throughout the reaction for protection to obtain a carbon quantum dot polylactic acid oligomer crude product; Step 4: Add chloroform and acetone solution to the crude carbon quantum dot polylactic acid oligomer product to extract the carbon quantum dot polylactic acid oligomer.

2. The method for preparing a carbon quantum dot polylactic acid oligomer according to claim 1, characterized in that: In step 1, carbon nanotubes are added to the mixed acid and then ultrasonicated for 20-40 minutes.

3. The method for preparing a carbon quantum dot polylactic acid oligomer according to claim 1, characterized in that: In step 2, lactic acid and the carbon quantum dot aqueous solution are mixed and ultrasonicated for 20-40 minutes.

4. The method for preparing a carbon quantum dot polylactic acid oligomer according to claim 1, characterized in that: In step 2, after the lactic acid and the carbon quantum dot aqueous solution are evenly mixed, the water in the mixed solution is evaporated by continuous vacuum at 60-70°C.

5. The method for preparing a carbon quantum dot polylactic acid oligomer according to claim 1, characterized in that: The catalyst is stannous octoate or stannous chloride.

6. The method for preparing a carbon quantum dot polylactic acid oligomer according to claim 1, characterized in that: The inert gas is at least one of nitrogen and argon.

7. The method for preparing a carbon quantum dot polylactic acid oligomer according to claim 1, characterized in that: In step 3, the reaction time is 24-48h.

8. Application of the carbon quantum dot polylactic acid oligomer prepared by any one of the preparation methods of claims 1 to 7, characterized in that: The carbon quantum dot polylactic acid oligomer is melt-blended with polylactic acid to prepare a polylactic acid composite material.

9. The use of a carbon quantum dot polylactic acid oligomer according to claim 8, characterized in that: The mass ratio of the carbon quantum dot polylactic acid oligomer to polylactic acid is 1-20:100.