A composite scraper online casting molding mold and molding process
Through online casting molding molds and processes, the full-wrap casting of non-metallic materials of composite scrapers is achieved, which solves the problems of structural strength and wear resistance, improves service life and lightweighting effect, and reduces production costs.
Patent Information
- Application Number
- CN202110956392.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-06-18
- Filing Date
- 2021-08-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-08-19
AI Technical Summary
After use, the existing composite scrapers have low structural strength and poor wear resistance, resulting in poor transportation, severe local wear and tear, and short service life, making it difficult to meet the lightweight demand of coal machinery equipment.
The online casting molding mold and process are adopted to achieve full-wrap casting molding of non-metallic materials through the cooperation of special core inserts and molds, which improves the structural strength and wear resistance of the composite scraper and reduces its own weight.
It improves the service life and wear resistance of composite scrapers, meets the lightweight demand of coal machinery equipment, reduces supporting equipment transformation and tool customization, and reduces production costs.
Smart Images

Figure CN114454401B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite scraper processing and forming, in particular to an online casting and forming mold and a forming process for a composite scraper. Background Art
[0002] Scraper conveyor equipment is a continuous conveying machine that fixes the scraper on the chain as a traction component to transport materials in the middle trough. It has the advantages of large transportation capacity, wide adaptability to the environment and simple maintenance, and is widely used in coal mine fully mechanized working faces. In the scraper conveyor equipment, the scraper and the pressure plate, bolts, nuts and chains form the scraper chain, which is the direct actuator that drives the transported materials to move.
[0003] At present, in coal mining machinery and transportation equipment, the scrapers are all integral forged structures of low-alloy steel, and the manufacturing process is: die forging → machining → heat treatment. The material used is generally 40Mn2 or 27SiMn. As a result, the coal mining machinery and transportation equipment itself is heavy, and a large part of the motor load energy consumption is consumed by the coal mining machinery and transportation equipment itself, which limits the transportation capacity of the coal mining machinery and transportation equipment and even the production efficiency of the entire set of coal mining equipment; at the same time, due to the large wear of the steel scraper assembly on the bottom of the coal mining machinery and transportation equipment, the complete set of equipment is seriously damaged, with a short life and low production efficiency.
[0004] As an improvement, a large number of researchers in the coal mining equipment industry are also studying how to improve metal scrapers into composite types of non-metallic materials and metal core plates. The production process has been changed from the original forging machine processing to placing the forged metal core plate in a mold and directly pouring non-metallic materials to form it, thereby reducing the installed load of scraper conveying equipment for coal mines, and to a large extent, it has indeed met the development requirements of lightweight coal mining equipment, but the use effect is not ideal. For example, the composite scraper itself has a low structural strength, and it often needs to operate in harsh installation environments and complex extreme load conditions. After a period of use, its tensile strength, wear resistance, flame retardancy, antistatic properties, etc. will be further reduced, and it is often accompanied by poor transportation operation and severe local wear. In severe cases, it may even cause the chain to break, resulting in a service life that is seriously less than expected. Summary of the invention
[0005] In view of this, the technical problem to be solved by the present invention is: the first aspect is to provide an online casting and molding mold for a composite scraper, so that after the composite scraper is cast and molded, it can not only efficiently meet the development requirements of lightweight coal machinery equipment, but also ensure its use effect after long-term use, thereby improving the service life of the composite scraper.
[0006] In order to solve the above-mentioned technical problem of the first aspect, the present invention provides an online casting molding mold for a composite scraper, including a lower mold and an upper mold, the lower mold including a main groove and end grooves connected to the left and right ends of the main groove, the upper mold including a main cavity and end cavities located at the left and right ends of the main cavity, a vertical joint portion is opened in the main cavity near the end cavity, and groove protection frames are arranged on the front and rear sides of the main cavity in a downwardly protruding manner, the main groove includes a first stepped groove adapted to the groove protection frame, and after the upper mold is locked and connected with the lower mold, the groove protection frame is buckled in the first stepped groove to form a molding chamber.
[0007] Preferably, the main groove further includes a second stepped groove arranged closely to the inner side of the first stepped groove, and the second stepped groove is communicated with the end groove.
[0008] Preferably, a plurality of positioning plugs are fixedly arranged in the second stepped groove.
[0009] Preferably, the main cavity is provided with a plurality of top member holes penetrating upward, and the projections of the top member holes and the positioning plug on the horizontal plane do not overlap each other.
[0010] Preferably, a downwardly protruding pressure plate seat, a flat chain seat and a vertical chain seat are provided in the main cavity, a first escape space is formed between the pressure plate seat and the groove protection frame, and a second escape space is enclosed between the flat chain seat and the vertical chain seat.
[0011] Preferably, the main chamber further comprises at least one of the following arrangements:
[0012] 1) The top member hole is opened through the pressure plate seat;
[0013] 2) The pressure plate seat includes an extension section that passes through the vertical joint along its length direction and extends to the end cavity, the first avoidance space passes through the vertical joint and includes a third avoidance space formed between the extension section and the groove protection frame, and the third avoidance space is connected to the end cavity;
[0014] 3) The flat chain seat and the vertical chain seat are both arranged closely against the inner side wall of the groove protection frame, and the downward protruding height of the vertical chain seat is higher than the downward protruding height of the groove protection frame and constitutes a reinforced groove frame of the groove protection frame.
[0015] Preferably, the casting mold further includes a sealing strip, and the lower mold is provided with sealing grooves adapted to the sealing strip at any one or more locations corresponding to the outer peripheral side of the groove protection frame, the lower end of the vertical joint, and the second stepped groove.
[0016] Preferably, the end cavity is open upward, and the casting mold further comprises an upper mold cover, which is used to cover the opening of the end cavity after the upper mold is buckled.
[0017] Preferably, the molding chamber at least includes a first molding cavity distributed at both ends of the casting molding mold, the first molding cavity includes a bottom end face, a first inclined end face, a second inclined end face, a tail arc face, a third inclined end face, an upper end face, and a vertical joint face which are sequentially connected head to tail, the vertical joint face is arranged tightly against the outer wall surface of the vertical joint part, a first opening is formed between the vertical joint face and the bottom end face, and the tail arc face is arranged on opposite sides of the first opening.
[0018] The technical problem to be solved by the present invention is also: the second aspect proposes an online casting and molding process for a composite scraper, so that after the composite scraper is cast and molded, it can not only efficiently meet the development requirements of lightweight coal machinery equipment, but also ensure its use effect after long-term use, thereby improving the service life of the composite scraper.
[0019] In order to solve the above-mentioned second technical problem, the present invention proposes an online casting process for a composite scraper, comprising the following steps:
[0020] S1: Start the temperature-controlled casting machine, remove the upper mold, move the preheated special core insert into the lower mold and place it on the lower mold for preheating and heat preservation;
[0021] S2: Move the upper mold to just above the lower mold and quickly close the mold;
[0022] S3: pouring the polyurethane mixed liquid from the open part of the upper mold, and quickly closing the upper mold cover after pouring;
[0023] S4: Complete the curing molding under the preheating temperature condition and normal pressure static state;
[0024] S5: Remove the upper mold cover and the upper mold to demould the composite scraper product;
[0025] S6: After trimming, the composite scraper products are subjected to secondary batch aging, qualified inspection, packaging and storage.
[0026] Compared with the prior art, the composite scraper online casting molding die and molding process described in the present invention have the following beneficial effects:
[0027] 1) After the composite scraper is formed, it can not only efficiently meet the development requirements of lightweight coal mining equipment, but also ensure its use effect after long-term use, thereby increasing the service life of the composite scraper;
[0028] 2) After the composite scraper is formed, it can be better adapted to the original matching assembly parts such as chains, pressure plates, bolts, etc., which helps to reduce the modification of related supporting equipment and the customized purchase of related special installation tools, thereby reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The accompanying drawings, which constitute part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention. In the accompanying drawings:
[0030] Figure 1 It is a cross-sectional schematic diagram of the main structure of a composite scraper in the prior art described in a specific embodiment of the present invention;
[0031] Figure 2 It is a schematic diagram of the three-dimensional structure of an online casting mold for a composite scraper described in Example 1 of the present invention in a mold-closing state;
[0032] Figure 3 It is a schematic diagram of the explosion structure of an online casting mold for a composite scraper described in Example 1 of the present invention in a working state;
[0033] Figure 4 This is a schematic diagram of the three-dimensional structure of an upper mold described in Example 1 of the present invention;
[0034] Figure 5 This is a schematic diagram of a top view of an upper mold described in Example 1 of the present invention;
[0035] Figure 6 This is a schematic diagram of the three-dimensional structure of a lower mold described in Example 1 of the present invention;
[0036] Figure 7 This is a schematic diagram of the three-dimensional structure of a special core insert described in Example 1 of the present invention;
[0037] Figure 8 It is a bottom view structural schematic diagram of a special core insert described in Example 1 of the present invention;
[0038] Fig. 9 It is an exploded schematic diagram of a front view half-section structure of an online casting mold for a composite scraper described in Example 1 of the present invention;
[0039] Fig.10 It is a partially enlarged schematic diagram of the three-dimensional cross-sectional structure of a first molding cavity described in Example 1 of the present invention.
[0040] Description of reference numerals:
[0041] 100-body, 101-bolt hole, 102-flat chain groove, 200-end body, 300-core insert, 400-cladding layer;
[0042] 1-lower die, 11-main groove, 111-first step groove, 112-second step groove, 1121-positioning plug, 113-avoidance part, 12-end groove, 2-upper die, 21-main cavity, 211-top piece hole, 212-third avoidance space, 213-pressing plate seat, 214-flat chain seat, 215-vertical chain seat, 216-first avoidance space, 217-second avoidance space, 22-end cavity, 221-open, 23- Vertical joint, 24-groove protection frame, 241-reinforced groove frame, 25-opening groove, 3-molding chamber, 31-first molding cavity, 311-vertical joint surface, 312-bottom end surface, 313-first inclined end surface, 314-tail arc surface, 315-second inclined end surface, 316-third inclined end surface, 317-upper end surface, 318-first opening, 32-second molding cavity, 4-sealing strip, 41-sealing groove, 5-upper mold cover;
[0043] 6-special core insert, 61-main body, 611-weight reduction groove, 612-strengthening rib, 613-first bolt hole, 614-pressure plate groove, 615-vertical chain groove, 616-support foot, 62-wing body. DETAILED DESCRIPTION
[0044] In order to make the above-mentioned purpose, technical scheme and advantages of the present invention more clear and easy to understand, the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments of the present invention described herein only constitute part of the embodiments of the present invention, which are only used to explain the present invention and do not constitute a limitation of the present invention. In the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other.
[0045] like Figure 1 As shown, a composite scraper in the prior art includes a body 100 and end bodies 200 located at the left and right ends of the body 100. The body 100 is provided with a plurality of bolt holes 101 from top to bottom, and a plurality of flat chain grooves 102 are provided at the bottom of the body 100 to facilitate the composite scraper and the chain to be assembled into a scraper chain after being pressed and assembled by a pressing plate, bolts, and nuts. When the composite scraper is processed and formed, it is cast and formed by two groups of materials, a core insert 300 and a coating layer 400, wherein the core insert 300 is a metal material, usually low alloy steel, and the coating layer 400 is a non-metallic material, usually wear-resistant resin.
[0046] Example 1
[0047] like Figure 2-10As shown, the present invention provides an online casting molding mold for a composite scraper, including a lower mold 1 and an upper mold 2, wherein the lower mold 1 includes a main groove 11 and end grooves 12 connected to the left and right ends of the main groove 11, and the upper mold 2 includes a main cavity 21 and end cavities 22 located at the left and right ends of the main cavity 21, and a vertical joint 23 is opened in the main cavity 21 near the end cavity 22, and groove protection frames 24 are distributed on the front and rear sides of the main cavity 21 and protrude downward, and the main groove 11 includes a first stepped groove 111 adapted to the groove protection frame 24, and after the upper mold 2 is locked and connected with the lower mold 1, the groove protection frame 24 is buckled in the first stepped groove 111 to form a molding chamber 3.
[0048] Specifically, Figure 1 As shown, when the composite scraper is operated in a harsh installation environment and complex extreme load conditions, the traction force at the joint between the flat chain groove 102 and the chain is the largest and is most susceptible to chain wear, thereby causing the vertical chain groove ( Figure 1 Not shown, please refer to Figure 8 The joints between the vertical chain groove 615 and the chain, and the joints between the lower part of the bolt hole 101 and the pressure plate, bolts, and nuts are also subject to greater wear. In the prior art, due to the unreasonable casting method of the composite scraper during processing and forming, the structural strength of the composite scraper itself is relatively low. The composite scraper is excessively lightweight by sacrificing the necessary structural strength of the composite scraper itself. It is this excessive exchange that leads to its unsatisfactory use effect.
[0049] Research and experiments have shown that the scraper's own weight can be reduced by 33% to 40% simply by fully wrapping the end body 200 through compression molding or casting. When the end body 200 is fully wrapped with non-metallic materials such as wear-resistant resin, a moderate decrease in its various performances (excluding size) will not affect the use of the scraper, and there will be no phenomena such as "poor conveying operation, severe local wear, and even chain breakage in severe cases."
[0050] More specifically, when the composite scraper is cast by the casting mold of the present invention, the core insert 300 used in the casting process will be specially designed to match the casting mold, such as Figure 7-8As shown, it is a structural schematic diagram of a special core insert 6 in the present invention. When the special core insert 6 is designed, the main body 61 of the special core insert 6 can be reserved and designed with reference to the original structural dimensions of the main body 100 of the traditional low-alloy steel scraper. Therefore, when the composite scraper is cast, the special core insert 6 will first be placed in the lower mold 1 in reverse, and the main body 61 of the special core insert 6 will fall into the main groove 11, and its wing body 62 will remain in the tilted state in the end groove 12. Then, after the upper mold 2 is locked and connected with the lower mold 1, the vertical joint 23 provides a vertical downward tight press fit to the main body 61, and the main cavity 21 covers most or all of the main body 61, and the groove protection frame 24 encloses the main body 61 in the front and rear directions. Under the action of the vertical joint 23, the special core insert 6, and the groove guard frame 24 tightly pressing and enclosing together, most or all of the main cavity 21 will be completely separated from the end cavity 22. At this time, the part of the molding chamber 3 corresponding to the end cavity 22, that is, the first molding cavity 31 enclosed by the end cavity 22, the end groove 12, the vertical joint 23, and the main body 61 will also be divided into an upper and lower part by the wing body 62, and the upper and lower parts are only connected at the tail end and fully wrap at least the entire wing body 62. When the composite scraper is processed and formed, non-metallic material casting can be performed only on the first molding cavity 31, thereby realizing that after the composite scraper is processed and formed, a non-metallic material fully wrapped coating layer 400 is formed only on the end body 200.
[0051] Of course, according to the specific opening position of the vertical joint 23, the first molding cavity 31 can also fully wrap a small part of the main body 61. Therefore, after the composite scraper is only cast and molded with non-metallic materials in the first molding cavity 31, it can also simultaneously form a non-metallic material fully wrapped coating layer 400 for a small part of the main body 100. At the same time, since the small part of the main body 100 is located outside the flat chain groove 102, its requirements for tensile strength and wear resistance are relatively low, which also helps to further reduce the weight of the composite scraper without affecting the use effect of the composite scraper.
[0052] As can be seen from the above, through the above-mentioned setting of the casting mold, the composite scraper can at least only need to fully wrap the wing body 62 of the special core insert 6 during processing and forming. After the composite scraper is formed, the structural strength of its body 100 will remain unchanged, thereby not only efficiently meeting the development requirements of lightweight coal machinery equipment, but also greatly improving the structural strength of the composite scraper itself, ensuring its use effect after long-term use, and thus improving the service life of the composite scraper. In addition, after the composite scraper is formed, since its body 100 can retain the original structural size design of the low-alloy steel scraper, it can better adapt to the original matching assembly parts such as chains, pressure plates, bolts, etc., which helps to reduce the modification of related supporting equipment and the customized purchase of related special installation tools, and reduce production costs.
[0053] Preferably, the main groove 11 further includes a second stepped groove 112 arranged closely to the inner side of the first stepped groove 111 , and the second stepped groove 112 is communicated with the end groove 12 .
[0054] Specifically, when the composite scraper is in operation, the upper part of the bolt hole 101 does not need to be in direct contact with the chain, that is, corresponding to the upper area of the main body 100 of the composite scraper, the tensile strength and wear resistance of this area do not need to be designed to be very superior, and the coating layer 400 can be completely formed by casting of non-metallic composite materials, thereby achieving further weight reduction of the composite scraper.
[0055] More specifically, through the provision of the second stepped groove 112, the dedicated core insert 6 can also be provided with a weight-reducing groove 611 and reinforcing ribs 612 located on both sides of the weight-reducing groove 611. Thus, when the composite scraper is cast and molded, when the dedicated core insert 6 is reversely placed in the lower mold 1, the main body 61 of the dedicated core insert 6 will still fall into the main groove 11, but at the same time, the reinforcing ribs 612 will be reversely placed in the second stepped groove 112 and form abutment with the first stepped groove 111, and then after the upper mold 2 and the lower mold 1 are locked and connected, the groove guard 24 will be buckled downward in the first stepped groove 111 and still provide enclosure for the main body 61 in the front-to-back direction. At this time, under the support of the reinforcing ribs 612, the part of the molding chamber 3 corresponding to the weight-reducing groove 611, that is, between the second stepped groove 112 and the weight-reducing groove 611, will also enclose and form a second molding cavity 32, and the second molding cavity 32 will be connected with the first molding cavity 31. When the composite scraper is being cast, the second molding cavity 32 can also be cast with non-metallic materials to further reduce the weight of the composite scraper without affecting the overall structural strength of the composite scraper. At the same time, the structural setting of the second molding cavity 32 will greatly facilitate the casting of non-metallic materials such as wear-resistant resins. Non-metallic materials such as wear-resistant resins can flow from the first molding cavity 31 to the second molding cavity 32.
[0056] Preferably, a plurality of positioning plugs 1121 are fixedly disposed in the second stepped groove 112 .
[0057] Specifically, Figure 1As shown, after the composite scraper is cast, its body 100 needs to be penetrated from top to bottom with a number of bolt holes 101, so as to facilitate the composite scraper and the chain to be assembled into a scraper chain after being pressed and assembled by a pressure plate, bolts, and nuts. When a number of positioning plugs 1121 are also fixedly provided in the second step groove 112, when the composite scraper is cast, the special core insert 6 itself will also be provided with a first bolt hole 613 for the positioning plug 1121 to pass through. The positioning plug 1121 is used to position and place the special core insert 6, which can greatly improve the assembly accuracy and assembly efficiency of the special core insert 6 and the lower mold 1; at the same time, when the composite scraper is cast in the second molding cavity 32, it will also greatly facilitate the one-time molding of the composite scraper after casting, avoiding the subsequent drilling of the composite scraper. More specifically, after the composite scraper is cast and successfully demolded, the composite scraper falls off and separates from the positioning plug 1121, and the coating layer 400 cast by non-metallic material will form a second bolt hole below the first bolt hole 613, and the second bolt hole and the first bolt hole 613 will together constitute the bolt hole 101 of the composite scraper.
[0058] Preferably, a plurality of top member holes 211 are formed through the main cavity 21 upwardly, and the projections of the top member holes 211 and the positioning plugs 1121 on the horizontal plane do not overlap each other.
[0059] Specifically, after the composite scraper is cast, the coating layer 400 cast by the non-metallic composite material will fill the first molding cavity 31, and the upper mold 2 may have difficulty in opening the mold. The setting of the top piece hole 211 will greatly facilitate the composite scraper to be properly reversed by the top piece tool after casting, so that the upper mold 2 can be easily separated from the composite scraper.
[0060] Preferably, a mold opening groove 25 is formed on the outer side of the upper mold 2 close to the end cavity 22 .
[0061] Specifically, the mold opening groove 25 can cooperate with the top piece hole 211 to greatly facilitate the mold opening process under various extreme mold opening conditions.
[0062] Preferably, a downwardly protruding pressure plate seat 213, a flat chain seat 214, and a vertical chain seat 215 are provided in the main cavity 21, a first escape space 216 is formed between the pressure plate seat 213 and the groove protection frame 24, and a second escape space 217 is enclosed between the flat chain seat 214 and the vertical chain seat 215.
[0063] Specifically, after the composite scraper is formed, in order to facilitate the assembly into a scraper chain after being pressed and assembled with the chain through a pressure plate, bolts and nuts, a flat chain groove 102, a vertical chain groove 615 and a pressure plate groove 614 are respectively opened at the lower part of the composite scraper body 100. The arrangement of the pressure plate seat 213, the flat chain seat 214, the vertical chain seat 215, the first avoidance space 216 and the second avoidance space 217 can make the main cavity 21 form a fixed limit for the special core insert 6 at least between the vertical joints 23 after the upper mold 2 and the lower mold 1 are locked and connected, so as to avoid the special core insert 6 from shifting during the casting process, and also prevent the high-temperature casting liquid from continuing to flow into the main cavity 21 from the vertical joint 23 under extreme working conditions, so as not to affect the molding quality of the composite scraper.
[0064] Preferably, the main cavity 21 further includes at least one of the following configurations:
[0065] 1) The top member hole 211 is formed through the pressure plate seat 213;
[0066] 2) The pressure plate seat 213 includes an extension section that passes through the vertical joint 23 along its length direction and extends to the end cavity 22. The first avoidance space 216 passes through the vertical joint 23 and includes a third avoidance space 212 formed between the extension section and the groove protection frame 24. The third avoidance space 212 is connected to the end cavity 22.
[0067] 3) The flat chain seat 214 and the vertical chain seat 215 are both arranged close to the inner side wall of the groove protection frame 24 . The downward protrusion height of the vertical chain seat 215 is higher than the downward protrusion height of the groove protection frame 24 and constitutes a reinforcing groove frame 241 of the groove protection frame 24 .
[0068] Specifically, the pressure plate seat 213 is adapted to the pressure plate groove 614 of the dedicated core insert 6. When the top piece hole 211 is opened through the pressure plate seat 213, the force of the top piece will be located in the center of the composite scraper, which is conducive to the smooth separation of the upper mold 2 and the composite scraper. As for the further setting of the vertical joint 23 and the pressure plate seat 213, the first avoidance space 216 and the third avoidance space 212, when the composite scraper is cast, the pressure plate groove 614 of the special core insert 6 or the support legs 616 on both sides of the pressure plate groove 614 can be a non-through setting, and then the third avoidance space 212 will also be filled with the cast non-metallic material. Then after the composite scraper is formed, the pressure plate groove 614 will be set through along the length direction of its body 100, which is conducive to the tight fit between the composite scraper and the chain. At the same time, the coating layer 400 cast in the third avoidance space 212 is located on the outside of the flat chain groove 102, and its requirements for tensile strength and wear resistance are relatively low. It will not affect the use effect of the composite scraper while helping to further reduce the weight of the composite scraper. The setting of the reinforcing groove frame 241 not only makes the reinforcing groove frame 241 more tightly enclose the special core insert 6 in the front-back direction, but also makes it easier for the groove frame 24 to buckle in the first step groove 111 in the vertical direction, thereby making the main cavity 21 more secure in the tight pressing of the special core insert 6 in the vertical direction. At this time, an avoidance portion 113 can also be provided on the transition platform between the first step groove 111 and the second step groove 112. The avoidance portion 113 is used to snap-fit with the reinforcing groove frame 241, so that the vertical chain seat 215 can complete the tight enclosement of the special core insert 6 at its vertical chain groove 615, thereby ensuring the fixed limit of the main groove 11 on the special core insert 6, avoiding the displacement of the special core insert 6 during the casting process, and also preventing the high-temperature casting liquid from the reinforcing rib 612 through the vertical chain groove 615 to continue to overflow the second step groove 112 under extreme working conditions, so as not to affect the molding quality of the composite scraper.
[0069] Preferably, the casting mold also includes a sealing strip 4 , and the lower mold 1 is provided with a sealing groove 41 adapted to the sealing strip 4 at any one or more locations corresponding to the outer peripheral side of the groove protection frame 24 , the lower end of the vertical joint 23 , and the second stepped groove 112 .
[0070] Specifically, in the casting process of the composite scraper, in order to prevent the high-temperature casting liquid in the first molding cavity 31 and / or the second molding cavity 32 from penetrating in other directions, the casting mold further includes a sealing strip 4, which is installed in the sealing groove 41 and is used to expand at high temperature to prevent the high-temperature casting liquid in the first molding cavity 31 and / or the second molding cavity 32 from penetrating in other directions. More specifically, the sealing groove 41 is used to prevent the high-temperature casting liquid in the molding cavity 3 from penetrating in the circumferential direction, the high-temperature casting liquid in the first molding cavity 31 from continuing to penetrate into the main cavity 21 from the vertical joint 23, and the high-temperature casting liquid in the second molding cavity 32 from continuing to penetrate into the outside of the second step groove 112 from the vertical chain groove 615 of the dedicated core insert 6 and even the reinforcing rib 612.
[0071] Preferably, the end cavity 22 is open upward, and the casting mold further comprises an upper mold cover 5 , and the upper mold cover 5 is used to cover the opening 221 of the end cavity 22 after the upper mold 2 is buckled.
[0072] Specifically, during the pouring process, the opening 221 can be used as a pouring port, and the high-temperature pouring liquid can flow from the pouring port through the first molding cavity 31 into the first molding cavity 32 until the liquid level in the first molding cavity 31 reaches a preset liquid level, then the pouring is stopped and the upper mold cover 5 is closed for pressure-maintaining cooling and shaping.
[0073] Preferably, the molding chamber 3 at least includes a first molding cavity 31 distributed at both ends of the casting molding mold, the first molding cavity 31 includes a bottom end face 311, a first inclined end face 312, a second inclined end face 313, a tail arc face 314, a third inclined end face 315, an upper end face 316, and a vertical joint face 317 which are connected in sequence from head to tail, the vertical joint face 317 is arranged close to the outer wall surface of the vertical joint part 23, and a first opening 318 is formed between the vertical joint face 317 and the bottom end face 311, and the tail arc face 314 and the first opening 318 are arranged on opposite sides.
[0074] Specifically, in the casting mold, when the dedicated core insert 6 is placed in reverse, it usually means that the casting mold is in the casting process. At this time, the first opening 318 will be blocked by the main body 61 of the dedicated core insert 6, and the first molding cavity 31 will be divided into upper and lower parts by the wing body 62 of the dedicated core insert 6, and the upper and lower parts are connected only at the tail end and fully wrap the wing body 62, which also means that the first molding cavity 31 is completely activated under the action of the dedicated core insert 6. The above multi-faceted design of the first molding cavity 31 is conducive to improving the bonding wrapping area and bonding wrapping strength between the coating layer 400 and the dedicated core insert 6 of the composite scraper after casting, thereby enhancing the overall structural strength of the composite scraper, and at the same time ensuring that the coating layer 400 at the end body 200 of the composite scraper can have sufficient thickness and length, so as to increase the thickness of the wear-resistant resin layer and ensure the wear resistance of the contact surface with the middle groove while reducing the weight to the maximum extent and adapting to the middle groove, and ensuring that the composite scraper has sufficient service strength.
[0075] Preferably, each joint surface of the molding cavity 3 is processed with a smooth arc.
[0076] When smooth arc treatment is further adopted between each joint surface, on the one hand, when the end body 200 of the composite scraper is being cast, the interface bonding wrapping area of the coating layer 400 can be further increased, thereby effectively ensuring the bonding strength with non-metallic materials such as wear-resistant resin; on the other hand, after the composite scraper is cast, the stress shearing effect of the special core insert 6 on the coating layer 400 can be effectively reduced, thereby reducing or delaying the probability or occurrence time of falling off at the interface bonding wrapping after long-term use.
[0077] Preferably, the molding chamber 3 also includes a second molding cavity 32 located in the middle of the casting mold and connected to the first molding cavity 31, and the bottom end surface 311 extends inward in a horizontal direction until the first molding cavities 31 distributed at both ends of the casting mold are connected through the second stepped groove 112.
[0078] Specifically, in the casting mold, when the special core insert 6 with the weight-reducing groove 611 is placed in reverse, the main body 61 of the special core insert 6 does not need to completely block the first opening 318, and a small gap can be selected to be left at the lower part of the first opening 318, so that the small gap can be surrounded by the reinforcing ribs 612 in the front and rear directions and can be connected with the weight-reducing groove 611 in the left and right directions. At this time, the second molding cavity 32 will also be completely activated under the action of the special core insert 6, and connected with the first molding cavity 31 through the small gap, thereby achieving further weight reduction of the composite scraper without affecting the overall structural strength of the composite scraper, and will also greatly facilitate the high-temperature casting liquid to flow toward the second molding cavity 32 in time during casting.
[0079] At the same time, it should be noted here that since the pressure plate seat 213 and its extension section are only arranged in the center of the main cavity 21, a first avoidance space 216 and a third avoidance space 212 will be formed between it and the groove protection frame 24. At the same time, although the extension section of the pressure plate seat 213 passes through the vertical joint 23 along the length direction and extends to the end cavity 22, it cannot block the first opening 318 in the vertical direction. It only occupies a certain physical space in the first molding cavity 31 to facilitate the further weight reduction of the composite scraper body 100 here after molding and cast it into a fully through pressure plate groove 614.
[0080] Example 2
[0081] The present invention also provides an online casting process for a composite scraper, which uses an online casting mold for a composite scraper, and comprises the following steps:
[0082] S1: Start the temperature-controlled casting machine, remove the upper mold 2, move the preheated special core insert 6 into the lower mold 1 for preheating and heat preservation;
[0083] S2: Move the upper mold 2 to the top of the lower mold 1 and close the mold quickly;
[0084] S3: pouring the polyurethane mixed liquid from the opening 221 of the upper mold 2, and quickly closing the upper mold cover 5 after the pouring is completed;
[0085] S4: Complete the curing molding under the preheating temperature condition and normal pressure static state;
[0086] S5: Remove the upper mold cover 5 and the upper mold 2 to demould the composite scraper product;
[0087] S6: After trimming, the composite scraper products are subjected to secondary batch aging, qualified inspection, packaging and storage.
[0088] Specifically, the preheating and heat preservation temperature in step S1 can be 80℃~120℃, and the polyurethane mixed liquid in step S3 is composed of a polyurethane prepolymer composed of polyester or polyether polyol and polyisocyanate as the resin matrix of the wear-resistant resin layer, supplemented by a chain extender, a reinforcing agent, a wear-resistant agent, an antistatic agent, a flame retardant and other functional additives. The material has excellent oil resistance, corrosion resistance and wear resistance, good buffering, energy absorption and noise reduction and mechanical strength, which can effectively reduce the weight of a single scraper, reduce the wear of the scraper and the middle groove, thereby reducing the equipment maintenance cost and improving the service life and production efficiency of the equipment.
[0089] Preferably, before step S1, the process further comprises the following steps:
[0090] ST1: Derust and clean the casting mold, apply release agent, and preheat;
[0091] ST2: Derusting and cleaning of the special core insert 6, shot blasting, sand blasting, secondary cleaning, surface activation, and glue preheating;
[0092] ST3: Use hot air circulation system to preheat the polyurethane prepolymer and perform vacuum degassing treatment;
[0093] ST4: After quantitatively mixing the functional additives including chain extender, reinforcing agent, anti-wear agent, antistatic agent and flame retardant, preheating and vacuum degassing are performed;
[0094] ST5: Apply mold release agent to the main groove 11, the end groove 12, the main cavity 21, and the end cavity 22.
[0095] Specifically, the preheating temperature in step ST1 may be 90°C to 140°C, the preheating temperature in step ST3 may be 60°C to 100°C, and the preheating temperature in step ST4 may be 60°C to 140°C.
[0096] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A composite scraper online casting mold, characterized in that: The invention comprises a lower mold (1) and an upper mold (2), wherein the lower mold (1) comprises a main groove (11) and end grooves (12) connected to the left and right ends of the main groove (11), and the upper mold (2) comprises a main cavity (21) and end cavities (22) located at the left and right ends of the main cavity (21). A vertical joint portion (23) is provided in the main cavity (21) near the end cavity (22). Groove protection frames (24) are provided on the front and rear sides of the main cavity (21) and are protruding downward. The main groove (11) comprises a first stepped groove (111) adapted to the groove protection frame (24). After the upper mold (2) is locked and connected with the lower mold (1), the groove protection frame (24) is buckled in the first stepped groove (111) to form a molding chamber (3); during the casting and molding of the composite scraper online casting and molding mold, the following steps are included: S1: starting the temperature-controlled casting machine, removing the upper mold (2), moving the preheated special core insert (6) into the lower mold (1) and placing it on the lower mold (1) for preheating and heat preservation; S2: Move the upper mold (2) to the top of the lower mold (1) and quickly close the mold; S3: pouring the polyurethane mixed liquid from the opening (221) of the end cavity (22) of the upper mold (2), and quickly closing the upper mold cover (5) after the pouring is completed; S4: Complete the curing molding under the preheating temperature condition and normal pressure static state; S5: removing the upper mold cover (5) and the upper mold (2) to demould the composite scraper product; S6: After trimming, the composite scraper products are subjected to secondary batch curing, qualified inspection, packaging and storage; the special core insert (6) includes a main body (61) and a wing body (62). When the composite scraper is cast, the special core insert (6) is placed in the lower mold (1) in reverse, and the main body (61) falls into the main groove (11). The wing body (62) remains in a tilted state in the end groove (12). After the upper mold (2) and the lower mold (1) are locked and connected, the vertical joint (23) provides a vertical downward tight pressing for the main body (61), and the main cavity (21) covers most or all of the main body (61). At the same time, the groove protection frame (24) encloses the main body (61) in the front and rear directions; at the vertical joint (23), the special core insert (6), and the groove protection frame (24) Under the action of tight pressing and enclosing of the frame (24), most or all of the main cavity (21) will be completely separated from the end cavity (22), and the molding chamber (3) corresponds to the part of the end cavity (22). The end cavity (22), the end groove (12), the vertical joint (23) and the main body (61) enclose a first molding cavity (31). The wing body (62) divides the first molding cavity (31) into two upper and lower parts, and the upper and lower parts are connected only at the rear end and fully wrap at least the entire wing body (62); the end cavity (22) is open upward, and the casting molding mold also includes an upper mold cover (5), which is used to cover the opening (221) of the end cavity (22) after the upper mold (2) is buckled.
2. The composite scraper online casting mold according to claim 1, characterized in that: The main groove (11) further comprises a second stepped groove (112) arranged closely on the inner side of the first stepped groove (111), and the second stepped groove (112) is connected to the end groove (12).
3. The composite scraper online casting mold according to claim 2, characterized in that: A plurality of positioning plugs (1121) are also fixedly arranged in the second stepped groove (112).
4. The composite scraper online casting mold according to claim 3, characterized in that: The main cavity (21) is provided with a plurality of top member holes (211) penetrating upward, and the projections of the top member holes (211) and the positioning plug (1121) on the horizontal plane do not overlap each other.
5. The composite scraper online casting mold according to claim 4, characterized in that: The main cavity (21) is provided with a downwardly protruding pressure plate seat (213), a flat chain seat (214), and a vertical chain seat (215); a first escape space (216) is formed between the pressure plate seat (213) and the groove protection frame (24); and a second escape space (217) is enclosed between the flat chain seat (214) and the vertical chain seat (215).
6. The composite scraper online casting mold according to claim 5, characterized in that: The main chamber (21) further comprises at least one of the following arrangements: 1) The top member hole (211) is opened through the pressure plate seat (213); 2) the pressure plate seat (213) includes an extension section that passes through the vertical joint (23) along its length direction and extends to the end cavity (22); the first avoidance space (216) passes through the vertical joint (23) and includes a third avoidance space (212) formed between the extension section and the groove protection frame (24); the third avoidance space (212) is connected to the end cavity (22); 3) The flat chain seat (214) and the vertical chain seat (215) are both arranged closely against the inner side wall of the groove protection frame (24); the downward protruding height of the vertical chain seat (215) is higher than the downward protruding height of the groove protection frame (24) and constitutes a reinforcing groove frame (241) of the groove protection frame (24).
7. A composite scraper online casting mold according to any one of claims 2-6, characterized in that: The casting mold also includes a sealing strip (4), and the lower mold (1) is provided with a sealing groove (41) adapted to the sealing strip (4) at any one or more locations corresponding to the outer peripheral side of the groove protection frame (24), the lower end of the vertical joint (23), and the second stepped groove (112).
8. A composite scraper online casting mold according to any one of claims 1-6, characterized in that: The molding chamber (3) at least comprises a first molding cavity (31) distributed at both ends of the casting molding mold, the first molding cavity (31) comprising a bottom end surface (311), a first oblique end surface (312), a second oblique end surface (313), a tail arc surface (314), a third oblique end surface (315), an upper end surface (316), and a vertical joint surface (317) which are sequentially connected head to tail, the vertical joint surface (317) being arranged in close contact with the outer wall surface of the vertical joint portion (23), a first opening (318) being formed between the vertical joint surface (317) and the bottom end surface (311), and the tail arc surface (314) and the first opening (318) being arranged on opposite sides.
Citation Information
Patent Citations
Non-metallic material and metal core plate composite type scraper used for coal mine and manufacturing process
CN105173546A
Pressing plate for scraper conveyor and production method thereof
CN106429211A
Handle seat injection mold
CN205202032U
Injection mold of mirror callus on sole
CN208392532U
Injection mold for injection molding of IBF products
CN209718459U