A composite photocatalyst for treating organic pollutants in wastewater, and its preparation method and application
Through hydrothermal treatment of bismuth salt, copper salt and nickel salt and sodium silicate composite, composite photocatalysts are formed, which solves the problem of low utilization of existing photocatalysts and achieves efficient degradation of wastewater organic pollutants. The process is simple and cost-effective Low.
Patent Information
- Application Number
- CN202210310514.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-03-28
AI Technical Summary
The existing photocatalysts have low utilization of sunlight and fail to effectively combine the photocatalytic effects of Bi2O3 and bismuth silicate, making it difficult to efficiently treat organic pollutants in wastewater.
The bismuth salt, copper salt and nickel salt were dissolved into the alcohol solvent, and the urea was added to hydrothermal treatment to obtain bismuth oxide co-doped with copper and nickel, and stirred with sodium metasilicate aqueous solution and alkali solution and hydrothermal treatment to form a composite Photocatalysts improve their photocatalytic properties.
Through element doping and composite preparation, the photocatalytic performance and sunlight utilization rate of the photocatalyst are significantly improved, and the organic pollutants in the wastewater are effectively degraded, with a simple process and saving manpower and equipment costs.
Smart Images

Figure BDA0003567991230000071
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of wastewater treatment, and more specifically, relates to a composite photocatalyst for treating organic pollutants in wastewater, and a preparation method and application thereof. Background Art
[0002] With the deepening of industrialization, environmental pollution problems have become more serious. Photocatalysis technology is considered to be an effective way to solve this problem. Photocatalysis (PC) uses the combined action of light and catalysts. The catalyst is excited by light to generate photogenerated electron-hole pairs (e - -h + ), generating active groups with strong oxidizing ability, which can degrade organic pollutants. It is an advanced oxidation technology. Photocatalytic technology has the advantages of wide applicability, mild reaction conditions, and the use of sunlight. It meets the requirements of the "green chemistry" concept and has a very broad application prospect.
[0003] CN113797917A discloses a Bi / β-Bi2O3 heterojunction material, a sodium gluconate-assisted synthesis method and its application, wherein sodium gluconate is first dissolved in water, then added to a PEG4000 aqueous solution, then added to a Bi(NO3)3 aqueous solution, and then mixed with formamide, and a precursor material is obtained by a hydrothermal method; further, a Bi / β-Bi2O3 photocatalyst material is obtained by heat treatment in a nitrogen atmosphere. The Bi / β-Bi2O3 heterojunction prepared in the present invention is a bird's nest-shaped hierarchical micro-nano structure, and has excellent photocatalytic performance; it has a high photocatalytic degradation activity for rhodamine B and levofloxacin hydrochloride, and still has a high degradation rate after a cyclic photocatalytic reaction.
[0004] CN111013569A discloses a flower-shaped bismuth silicate / bismuth molybdate heterojunction photocatalyst and its preparation method and application. During the preparation, Bi(NO3)3·5H2O is first dissolved in ethylene glycol to obtain liquid A; then Na2SiO3·9H2O and Na2MoO4·2H2O are dissolved in water to obtain liquid B; liquid A and liquid B are mixed, and the pH of the solution is adjusted with alkali while stirring; then the mixed solution is transferred to a reactor and reacted at 170-190°C for 9-11h, and the collected products are washed three times with deionized water and ethanol respectively, and dried at 55-65°C to obtain the product; the preparation process of the invention is simple, the production process is green and environmentally friendly, and the raw materials are cheap and easy to obtain. The product has a controllable and uniform morphology, excellent activity in photocatalytic degradation of CIP, high stability, and can be reused, which meets the needs of industrial applications and has a large application prospect.
[0005] CN109046231A discloses a method and application for preparing mesoporous copper bismuth silicate nanocomposite materials by ultrasonic-assisted hydrothermal synthesis, and relates to the technical field of preparation of organic wastewater treatment agents. First, bismuth silicate is prepared by ultrasonic-assisted hydrothermal synthesis using silicon dioxide and bismuth nitrate, and then copper bismuth silicate, copper acetate and ammonia water are prepared by ultrasonic-assisted hydrothermal synthesis. The experiment found that the molar ratio of the initial raw materials and the length of the hydrothermal reaction time will affect the morphology and phase composition of the final product of the experiment; as the reaction time increases, the product changes from a hollow structure to a core-shell structure. Cu 2+ :Bi 2+ The sample with a molar ratio of 1:1 was selected as the adsorbent and catalyst to perform physical adsorption and tungsten light catalysis on the indigo solution. The experimental results showed that the degradation adsorption effect can basically reach more than 85%.
[0006] Although Bi2O3 and bismuth silicate have been studied as photocatalysts in the prior art, the utilization rate of sunlight by the above-mentioned photocatalysts is still relatively low, and there has been no research on the photocatalytic effect of combining the two. The applicant unexpectedly discovered that the photocatalyst obtained by the above-mentioned combination has excellent photocatalytic properties and has excellent degradation ability for organic pollutants in wastewater. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the defects and deficiencies in the prior art, and provide a composite photocatalyst for treating organic pollutants in wastewater, and a preparation method and application thereof. The composite photocatalyst is prepared by dissolving bismuth salt, copper salt and nickel salt into an alcohol solvent, then adding urea and continuing to stir, then hydrothermally treating, centrifuging the solid after the reaction, washing and drying, to obtain copper and nickel co-doped bismuth oxide; taking the prepared copper and nickel co-doped bismuth oxide and adding it to the alcohol solution of bismuth salt, taking a certain amount of sodium metasilicate aqueous solution and adding it to the alcohol solution of bismuth salt, magnetically stirring, slowly dropping an alkaline solution under stirring conditions to adjust the pH, continuing to stir, then hydrothermally treating, cooling to room temperature, washing, drying, to obtain a composite photocatalyst, and the composite photocatalyst prepared by element doping and composite preparation can effectively photodegrade organic pollutants in wastewater.
[0008] The purpose of the present invention is to provide a method for preparing a composite photocatalyst for treating organic pollutants in waste water.
[0009] Another object of the present invention is to provide a composite photocatalyst for treating organic pollutants in wastewater and its application.
[0010] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0011] A method for preparing a composite photocatalyst for treating organic pollutants in wastewater, the preparation method comprising the following steps:
[0012] (1) dissolving a bismuth salt, a copper salt and a nickel salt in an alcohol solvent, then adding urea and continuing stirring, then hydrothermally treating, and after the reaction, centrifuging the solid, washing and drying to obtain copper- and nickel-co-doped bismuth oxide;
[0013] (2) adding the copper and nickel co-doped bismuth oxide prepared in step 1) to an alcohol solution of bismuth salt, adding a certain amount of sodium metasilicate aqueous solution to the alcohol solution of bismuth salt, stirring magnetically, slowly adding alkaline solution dropwise under stirring to adjust the pH, continuing stirring, then hydrothermally treating, cooling to room temperature, washing, and drying to obtain a composite photocatalyst.
[0014] Preferably, in step (1), the bismuth salt is at least one of bismuth nitrate, bismuth chloride and bismuth acetate; the copper salt is at least one of copper nitrate, copper acetate and copper chloride; and the nickel salt is at least one of nickel nitrate, nickel acetate and nickel chloride.
[0015] Preferably, in step (1), the molar ratio of the bismuth salt to the copper salt and the nickel salt is 1:0.01-0.03:0.02-0.04; and the material ratio of bismuth to alcohol is 1 mol:60-70 mL.
[0016] Preferably, in step (1), the alcohol is one of ethanol, ethylene glycol and propylene glycol, and the molar ratio of the bismuth salt to urea is 1:3-5.
[0017] Preferably, in step (1), the stirring time is 20 to 40 minutes; the hydrothermal temperature is 140 to 160° C., and the hydrothermal time is 14 to 18 hours; and the drying is carried out at 80 to 100° C. for 10 to 16 hours.
[0018] Preferably, in step (2), the volume of the alcohol solution of the bismuth salt is 10 to 30 mL, and the concentration is 1 mol / L; the bismuth salt is at least one of bismuth nitrate, bismuth chloride, and bismuth acetate; the alcohol is one of ethanol, ethylene glycol, and glycerol; and the alkali solution is an aqueous solution of sodium hydroxide, potassium hydroxide, or ammonia.
[0019] Preferably, in step (2), the stirring time is 30 to 40 minutes; and the molar ratio of the bismuth salt to sodium metasilicate is 2:1.
[0020] Preferably, in step (2), the pH is 10; the stirring time is 30 to 50 minutes; the hydrothermal treatment is a hydrothermal reaction at 180 to 220° C. for 10 to 16 hours; and the drying is drying at 80 to 100° C. for 10 to 14 hours.
[0021] A composite photocatalyst is prepared based on the above-mentioned method for preparing a composite photocatalyst for treating organic pollutants in wastewater.
[0022] Based on the use of the composite photocatalyst described above, the composite photocatalyst is used to treat organic pollutants in wastewater.
[0023] The present invention has the following beneficial effects:
[0024] (1) By using a hydrothermal method, copper and nickel are in-situ doped into bismuth oxide, and the synergistic effect of the two elements is used to increase the utilization rate of sunlight by bismuth oxide and improve its photocatalytic performance.
[0025] (2) By using a hydrothermal method to in situ recombine bismuth silicate with doped bismuth oxide to form a heterojunction structure, the electron conductivity is improved, the effective separation of photogenerated electrons and holes is promoted, and the photocatalytic performance is improved, thereby promoting the effective removal of organic pollutants in wastewater.
[0026] (3) The preparation method of the present invention has simple process and convenient operation, and can effectively save manpower and equipment costs. DETAILED DESCRIPTION
[0027] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0028] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0029] Example 1
[0030] A method for preparing a composite photocatalyst for treating organic pollutants in wastewater, the preparation method comprising the following steps:
[0031] (1) 1 mol of bismuth nitrate, 0.02 mol of copper nitrate and 0.03 mol of nickel nitrate were dissolved in 65 mL of ethylene glycol solvent, and then 4 mol of urea was added and stirred for 30 min, and then hydrothermally reacted at 150° C. for 16 h. After the reaction, the solid was centrifuged, washed with deionized water 3 times, and dried at 90° C. for 13 h to obtain copper-nickel co-doped bismuth oxide;
[0032] (2) Add the copper and nickel co-doped bismuth oxide prepared in step 1) to 20 mL of a 1 mol / L bismuth nitrate ethylene glycol solution, add 10 mL of a 1 mol / L sodium metasilicate aqueous solution to the bismuth nitrate ethylene glycol solution, and stir magnetically for 35 min; slowly add a sodium hydroxide aqueous solution under stirring to adjust the pH to 10; continue stirring for 40 min; then react at 200° C. for 14 h; cool to room temperature, wash with deionized water three times, and dry at 90° C. for 12 h to obtain a composite photocatalyst.
[0033] Example 2
[0034] A method for preparing a composite photocatalyst for treating organic pollutants in wastewater, the preparation method comprising the following steps:
[0035] (1) 1 mol of bismuth acetate, 0.03 mol of copper chloride and 0.02 mol of nickel nitrate were dissolved in 70 mL of ethanol solvent, and then 5 mol of urea was added and stirred for 40 min, and then hydrothermally reacted at 160° C. for 14 h. After the reaction, the solid was centrifuged, washed with deionized water 3 times, and dried at 100° C. for 10 h to obtain copper and nickel co-doped bismuth oxide;
[0036] (2) Add the copper and nickel co-doped bismuth oxide prepared in step 1) to 30 mL of a 1 mol / L ethanol solution of bismuth chloride, add 15 mL of a 1 mol / L sodium metasilicate aqueous solution to the ethanol solution of bismuth chloride, and stir magnetically for 40 min; slowly add a potassium hydroxide aqueous solution under stirring to adjust the pH to 10; continue stirring for 50 min; then react at 220° C. for 10 h; cool to room temperature, wash with deionized water 3 times, and dry at 100° C. for 10 h to obtain a composite photocatalyst.
[0037] Example 3
[0038] A method for preparing a composite photocatalyst for treating organic pollutants in wastewater, the preparation method comprising the following steps:
[0039] (1) 1 mol of bismuth acetate, 0.01 mol of copper nitrate and 0.04 mol of nickel chloride were dissolved in 60 mL of glycerol solvent, and then 3 mol of urea was added and stirred for 20 min, and then hydrothermally reacted at 140° C. for 18 h. After the reaction, the solid was centrifuged, washed with deionized water 3 times, and dried at 80° C. for 16 h to obtain copper and nickel co-doped bismuth oxide;
[0040] (2) Add the copper and nickel co-doped bismuth oxide prepared in step 1) to 10 mL of a 1 mol / L bismuth acetate propylene glycol solution, add 5 mL of a 1 mol / L sodium metasilicate aqueous solution to the bismuth acetate propylene glycol solution, and stir magnetically for 30 min; slowly add an ammonia aqueous solution while stirring to adjust the pH to 10; continue stirring for 30 min; then react at 180° C. for 16 h; cool to room temperature, wash with deionized water 3 times, and dry at 80° C. for 14 h to obtain a composite photocatalyst.
[0041] Comparative Example 1
[0042] A method for preparing a composite photocatalyst for treating organic pollutants in wastewater, the preparation method comprising the following steps:
[0043] (1) dissolving 1 mol of bismuth nitrate and 0.05 mol of copper nitrate in 65 mL of ethylene glycol solvent, then adding 4 mol of urea and stirring for 30 min, and then hydrothermally reacting at 150° C. for 16 h. After the reaction, the solid was centrifuged, washed with deionized water 3 times, and dried at 90° C. for 13 h to obtain copper-doped bismuth oxide;
[0044] (2) Add the copper-doped bismuth oxide prepared in step 1) to 20 mL of a 1 mol / L bismuth nitrate ethylene glycol solution, add 10 mL of a 1 mol / L sodium metasilicate aqueous solution to the bismuth nitrate ethylene glycol solution, and stir magnetically for 35 min; slowly add a sodium hydroxide aqueous solution under stirring to adjust the pH to 10; continue stirring for 40 min; then react at 200° C. for 14 h; cool to room temperature, wash with deionized water 3 times, and dry at 90° C. for 12 h to obtain a composite photocatalyst.
[0045] Comparative Example 2
[0046] A method for preparing a composite photocatalyst for treating organic pollutants in wastewater, the preparation method comprising the following steps:
[0047] (1) dissolving 1 mol of bismuth nitrate and 0.05 mol of nickel nitrate in 65 mL of ethylene glycol solvent, then adding 4 mol of urea and stirring for 30 min, and then hydrothermally reacting at 150° C. for 16 h. After the reaction, the solid was centrifuged, washed with deionized water three times, and dried at 90° C. for 13 h to obtain nickel-doped bismuth oxide;
[0048] (2) Add the nickel-doped bismuth oxide prepared in step 1) to 20 mL of a 1 mol / L bismuth nitrate ethylene glycol solution, add 10 mL of a 1 mol / L sodium metasilicate aqueous solution to the bismuth nitrate ethylene glycol solution, and stir magnetically for 35 min; slowly add a sodium hydroxide aqueous solution under stirring to adjust the pH to 10; continue stirring for 40 min; then react at 200° C. for 14 h; cool to room temperature, wash with deionized water three times, and dry at 90° C. for 12 h to obtain a composite photocatalyst.
[0049] Comparative Example 3
[0050] A method for preparing a composite photocatalyst for treating organic pollutants in wastewater, the preparation method comprising the following steps:
[0051] (1) 1 mol of bismuth nitrate, 0.02 mol of copper nitrate and 0.03 mol of nickel nitrate were dissolved in 65 mL of ethylene glycol solvent, and then 4 mol of urea was added and stirred for 30 min, and then hydrothermally reacted at 150° C. for 16 h. After the reaction, the solid was centrifuged, washed with deionized water 3 times, and dried at 90° C. for 13 h to obtain copper-nickel co-doped bismuth oxide;
[0052] (2) taking 20 mL of a 1 mol / L bismuth nitrate ethylene glycol solution, taking 10 mL of a 1 mol / L sodium metasilicate aqueous solution and adding it to the bismuth nitrate ethylene glycol solution, and magnetically stirring for 35 min; slowly adding a sodium hydroxide aqueous solution under stirring to adjust the pH to 10; continuing stirring for 40 min; then reacting at 200° C. for 14 h; cooling to room temperature, washing with deionized water 3 times, and drying at 90° C. for 12 h to obtain bismuth silicate.
[0053] (3) Grind and mix the copper-nickel co-doped bismuth oxide obtained in step (1) and the bismuth silicate obtained in step (2) to obtain a composite photocatalyst.
[0054] Comparative Example 4
[0055] A method for preparing a photocatalyst for treating organic pollutants in wastewater, the preparation method comprising the following steps:
[0056] (1) 1 mol of bismuth nitrate, 0.02 mol of copper nitrate and 0.03 mol of nickel nitrate were dissolved in 65 mL of ethylene glycol solvent, and then 4 mol of urea was added and stirred for 30 min. Then, the mixture was hydrothermally reacted at 150° C. for 16 h. After the reaction, the solid was centrifuged, washed with deionized water three times, and dried at 90° C. for 13 h to obtain bismuth oxide co-doped with copper and nickel.
[0057] Comparative Example 5
[0058] A method for preparing a photocatalyst for treating organic pollutants in wastewater, the preparation method comprising the following steps:
[0059] Take 20 mL of 1 mol / L bismuth nitrate ethylene glycol solution, take 10 mL of 1 mol / L sodium metasilicate aqueous solution and add it to the bismuth nitrate ethylene glycol solution, and stir magnetically for 35 minutes; slowly add sodium hydroxide aqueous solution under stirring to adjust the pH to 10; continue stirring for 40 minutes; then react at 200°C for 14 hours; cool to room temperature, wash with deionized water 3 times, and dry at 90°C for 12 hours to obtain a photocatalyst.
[0060] The photocatalysts of Examples 1-3 and Comparative Examples 1-5 were used in photocatalytic degradation experiments. The specific method is as follows:
[0061] Take 15 mg of photocatalyst and add it to the aqueous solution of Rhodamine B (concentration is 10 -5 M), first stirred for 30 min in dark conditions, then stirred under irradiation of a xenon lamp (350 W), and the degradation rates were measured at 5 min and 10 min.
[0062] Take 15 mg of photocatalyst and add it to an aqueous solution of methyl orange (concentration of 10 -5 M), first stirred for 30 min in dark conditions, then stirred under irradiation of a xenon lamp (350 W), and the degradation rates were measured at 5 min and 10 min.
[0063]
[0064] By comparing Examples 1-3 with Comparative Examples 1-5, the composite photocatalyst is significantly improved by co-doping bismuth oxide with copper and nickel and then compounding it with bismuth silicate through hydrothermal treatment and utilizing the synergistic effect between the components.
[0065] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a composite photocatalyst for treating organic pollutants in wastewater, characterized in that: The preparation method comprises the following steps: (1) dissolving bismuth salt, copper salt and nickel salt in an alcohol solvent, then adding urea and continuing stirring, then hydrothermally treating, centrifuging the solid after the reaction, washing and drying to obtain copper and nickel co-doped bismuth oxide; the molar ratio of the bismuth salt to the copper salt and the nickel salt is 1:0.01-0.03:0.02-0.04; the material ratio of the bismuth salt to the alcohol solvent is 1 mol:60-70 mL; the stirring time is 20-40 min; the hydrothermal temperature is 140-160° C., the hydrothermal time is 14-18 h; the drying is performed at 80-100° C. for 10-16 h; (2) adding the copper and nickel co-doped bismuth oxide prepared in step (1) to an alcohol solution of bismuth salt, taking a certain amount of sodium metasilicate aqueous solution and adding it to the alcohol solution of bismuth salt, stirring magnetically, slowly adding alkaline solution under stirring to adjust the pH value, continuing stirring, then hydrothermally treating, cooling to room temperature, washing, and drying to obtain a composite photocatalyst; the pH value is 10; the stirring time is 30-50 minutes; the hydrothermal treatment is a hydrothermal reaction at 180-220° C. for 10-16 hours; the drying is drying at 80-100° C. for 10-14 hours; the magnetic stirring time is 30-40 minutes; and the molar ratio of bismuth salt to sodium metasilicate is 2:
1.
2. The method for preparing a composite photocatalyst for treating organic pollutants in wastewater according to claim 1, characterized in that: In step (1), the bismuth salt is at least one of bismuth nitrate, bismuth chloride, and bismuth acetate; the copper salt is at least one of copper nitrate, copper acetate, and copper chloride; and the nickel salt is at least one of nickel nitrate, nickel acetate, and nickel chloride.
3. The method for preparing a composite photocatalyst for treating organic pollutants in wastewater according to claim 1, characterized in that: In step (1), the alcohol solvent is one of ethanol, ethylene glycol and propylene glycol, and the molar ratio of the bismuth salt to urea is 1:3-5.
4. The method for preparing a composite photocatalyst for treating organic pollutants in wastewater according to claim 1, characterized in that: In step (2), the volume of the alcohol solution of the bismuth salt is 10-30 mL, and the concentration is 1 mol / L; the bismuth salt is at least one of bismuth nitrate, bismuth chloride, and bismuth acetate; the alcohol is one of ethanol, ethylene glycol, and glycerol; and the alkaline solution is an aqueous solution of sodium hydroxide, potassium hydroxide, or ammonia.
5. A composite photocatalyst prepared by the method for preparing a composite photocatalyst for treating organic pollutants in wastewater according to any one of claims 1 to 4.
6. The use of the composite photocatalyst according to claim 5, characterized in that: The composite photocatalyst is used for treating organic pollutants in wastewater.