A welding method for aluminum-scandium target and aluminum alloy back plate
Electron beam welding with tailored parameters addresses the inefficiencies of conventional welding methods for aluminum-scandium targets, achieving high bonding rates and low energy consumption.
Patent Information
- Application Number
- CN202210238571.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-03-11
AI Technical Summary
Existing technologies for welding aluminum-scandium targets face challenges such as poor wetting effect, high energy consumption, and inefficiency in mass production, particularly when preparing aluminum-scandium alloy targets with high scandium content.
The method employs electron beam welding with specific parameters tailored to scandium content, including multiple passes, beam current, focal depth, and linear speed to achieve stable and efficient bonding.
This approach enables automated production with high bonding rates (>99%) and low energy consumption, addressing the inefficiencies of conventional methods.
Smart Images

Figure BDA0003543331320000061 
Figure BDA0003543331320000071 
Figure BDA0003543331320000081
Abstract
Description
Technical Field
[0001] The invention belongs to the field of target material manufacturing, relates to an aluminum-scandium target material, and in particular to a welding method of the aluminum-scandium target material and an aluminum alloy back plate. Background Art
[0002] Aluminum-scandium alloy materials, while maintaining the same electrical conductivity and heat resistance as high-purity aluminum, can improve the electron migration and stress displacement of thin film materials several times; in the field of wireless communication equipment, as the signal frequency requirements continue to increase, the filter is upgraded from SW devices to FBAR devices, and the piezoelectric film material is also transitioning from aluminum nitride piezoelectric film to aluminum-scandium nitride piezoelectric film. Compared with aluminum nitride piezoelectric film, aluminum-scandium nitride piezoelectric film has a higher piezoelectric constant, better piezoelectric performance and perfect semiconductor process compatibility, and is increasingly valued.
[0003] The welding of aluminum-scandium is mostly done by welding an aluminum-scandium target and an aluminum alloy back plate (mostly a high-strength aluminum-copper alloy or an aluminum-magnesium-silicon alloy). The aluminum-scandium alloy target with a scandium content between 5-43at% is used, and the commonly used target has a scandium content of ≤20at%.
[0004] The existing conventional brazing preparation process technology has the following problems: 1. As the Sc content of aluminum-scandium alloy increases, the wetting effect becomes worse and the preparation efficiency is low; 2. The preparation process consumes a lot of energy; 3. It is not conducive to mass automated production.
[0005] CN 112894111A discloses a method for diffusion welding of a high-scB content aluminum-scB alloy target and a prepared welding assembly, comprising: a first step, ultrasonic cleaning, ultrasonic cleaning of the high-scB content aluminum-scB alloy target blank to be diffused welded; a second step, surface roughening treatment, surface roughening treatment of the welding surface of the aluminum-scB alloy target blank obtained in the first step; a third step, cold spraying, cold spraying Al alloy or Cu alloy backing plate on the welding surface of the aluminum-scB alloy target blank after the second step of roughening treatment; a fourth step, low-temperature heat treatment, low-temperature heat treatment of the aluminum-scB alloy target after the third step of spraying, promoting the diffusion of the AlSc alloy target blank and the sprayed backing plate, and increasing the welding strength of the AlSc alloy target; a fifth step, mechanical processing, lathing the heat-treated aluminum-scB alloy target to obtain a crack-free high-Sc content AlSc alloy target diffusion welding assembly. Although the method has a good welding effect, the welding process is complicated, and the target and the backing plate surface need to be processed in multiple steps, which is not conducive to industrial production.
[0006] CN 112877653A discloses an aluminum-scandium alloy diffusion welding target material and its preparation method and application, comprising an aluminum-scandium alloy target blank, an aluminum-based alloy back plate, and an intermediate layer located between the aluminum-scandium alloy target blank and the aluminum-based alloy back plate, wherein the intermediate layer is an aluminum layer, and the intermediate layer and the aluminum-scandium alloy target blank, and the intermediate layer and the aluminum-based alloy back plate are both diffusely welded. The preparation method comprises: step 1: performing aluminum film plating treatment on the welding surface of the aluminum-scandium alloy target blank to obtain an aluminum-scandium alloy target blank having an aluminum layer on the welding surface; step 2: stacking the aluminum-based alloy back plate and the aluminum-scandium alloy target blank having an aluminum layer, so that the aluminum layer is located between the aluminum-scandium alloy target blank and the aluminum-based alloy back plate, performing hot pressing diffusion welding, and obtaining an aluminum-scandium alloy diffusion welding target material. This method requires adding an intermediate layer between the target material and the back plate, which not only increases the welding cost, but also is not conducive to the thinning of the target material. Summary of the invention
[0007] In order to solve the technical problems existing in the prior art, the present invention provides a welding method for an aluminum-scandium target and an aluminum alloy back plate. The welding method adopts electron beam welding, and the preparation of an aluminum-scandium alloy target is convenient for automated production, the welding process and quality are more stable, the energy consumption is low, and the production efficiency is high.
[0008] In order to achieve the above technical effects, the present invention adopts the following technical solutions:
[0009] The invention provides a welding method for an aluminum-scandium target material and an aluminum alloy back plate. The welding method is electron beam welding, the number of passes of the electron beam welding is ≥3, and the content of scandium in the aluminum-scandium target material is ≤20at%.
[0010] Among them, the number of electron beam welding passes can be 3, 4, 5, 6, 7, 8, 9 or 10, and the scandium content in the aluminum-scandium target can be 0.5at%, 1at%, 2at%, 5at%, 8at%, 10at%, 12at%, 15at% or 18at%, but is not limited to the listed values, and other unlisted values within the above numerical ranges are also applicable.
[0011] In the present invention, when the scandium content of the aluminum-scandium alloy is less than 25%, it is mainly composed of Al phase and Al3Sc phase. When the scandium content is ≥20%, the proportion of Al phase is very small, and it is difficult to achieve effective welding of the aluminum-scandium alloy and the aluminum alloy back plate by electron beam welding. Electron beam welding is not recommended for welding. When the scandium content is less than 20%, effective welding can be achieved by electron beam welding, and with the increase of scandium content, the Al3Sc phase increases, and welding becomes difficult. In order to improve the welding bonding rate, it is necessary to increase the number of welding passes and beam current.
[0012] As a preferred technical solution of the present invention, the scandium content in the aluminum-scandium target is 5 to 10 at%, such as 5.5 at%, 6 at%, 6.5 at%, 7 at%, 7.5 at%, 8 at%, 8.5 at%, 9 at% or 9.5 at%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0013] As a preferred technical solution of the present invention, the beam current of the electron beam welding is 20-40mA, such as 22mA, 25mA, 28mA, 30mA, 32mA, 35mA or 38mA, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0014] Preferably, the focal depth of the electron beam welding is 515-560mA, such as 520mA, 525mA, 530mA, 535mA, 540mA, 545mA, 550mA or 555mA, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0015] As a preferred technical solution of the present invention, the linear speed of the electron beam welding is 10 to 15 mm / s, such as 10.5 mm / s, 11 mm / s, 11.5 mm / s, 12 mm / s, 12.5 mm / s, 13 mm / s, 13.5 mm / s, 14 mm / s or 14.5 mm / s, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0016] As a preferred technical solution of the present invention, the scandium content in the aluminum-scandium target is 10-15at%, excluding 10at%, such as 10.5at%, 11at%, 11.5at%, 12at%, 12.5at%, 13at%, 13.5at%, 14at% or 14.5at%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] As a preferred technical solution of the present invention, after the welding gun of the electron beam welding is aligned with the weld position, it is biased toward one side of the aluminum-scandium target by 0 to 1 mm, excluding 0, such as 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm or 0.9 mm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] Preferably, the number of electron beam welding passes is ≥ 4, such as 4, 5, 6, 7, 8, 9 or 10, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] As a preferred technical solution of the present invention, the beam current of the electron beam welding is 20-50mA, such as 25mA, 30mA, 35mA, 40mA or 45mA, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] Preferably, the focal depth of the electron beam welding is 515-560mA, such as 520mA, 525mA, 530mA, 535mA, 540mA, 545mA, 550mA or 555mA, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, the linear speed of the electron beam welding is 10 to 15 mm / s, such as 10.5 mm / s, 11 mm / s, 11.5 mm / s, 12 mm / s, 12.5 mm / s, 13 mm / s, 13.5 mm / s, 14 mm / s or 14.5 mm / s, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] As a preferred technical solution of the present invention, the scandium content in the aluminum-scandium target is 15-20at%, excluding 15at%, such as 15.5at%, 16at%, 16.5at%, 17at%, 17.5at%, 18at%, 18.5at%, 19at% or 19.5at%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] As a preferred technical solution of the present invention, after the welding gun of the electron beam welding is aligned with the weld position, it is biased toward one side of the aluminum-scandium target by 1 to 1.5 mm, excluding 1, such as 1.1 mm, 1.2 mm, 1.3 mm or 1.4 mm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, the number of electron beam welding passes is ≥5, such as 5, 6, 7, 8, 9 or 10, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] As a preferred technical solution of the present invention, the beam current of the electron beam welding is 20-60mA, such as 25mA, 30mA, 35mA, 40mA, 45mA, 50mA or 55mA, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the focal depth of the electron beam welding is 515-560mA, such as 520mA, 525mA, 530mA, 535mA, 540mA, 545mA, 550mA or 555mA, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, the linear speed of the electron beam welding is 10 to 15 mm / s, such as 10.5 mm / s, 11 mm / s, 11.5 mm / s, 12 mm / s, 12.5 mm / s, 13 mm / s, 13.5 mm / s, 14 mm / s or 14.5 mm / s, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] In the present invention, since the content of scandium element has a direct influence on the welding properties of aluminum-scandium alloy, different welding conditions, such as welding passes and the position of welding gun, are adopted for aluminum-scandium targets with different scandium contents during electron beam welding, so as to achieve the best welding effect.
[0029] In the present invention, the limitation of the welding passes is the total number of welding passes when electron beam welding is performed. For example, if the welding passes are 3, it includes the first welding pass, the second welding pass and the third welding pass; if the welding passes are 4, it includes the first welding pass, the second welding pass, the third welding pass and the fourth welding pass; if the welding passes are 5, it includes the first welding pass, the second welding pass, the third welding pass, the fourth welding pass and the fifth welding pass, and so on.
[0030] Compared with the prior art, the present invention has at least the following beneficial effects:
[0031] The present invention provides a method for welding an aluminum-scandium target and an aluminum alloy back plate. The welding method adopts electron beam welding, and the preparation of the aluminum-scandium alloy target is convenient for automated production, the welding process and quality are more stable, the energy consumption is low, the production efficiency is high, the overall bonding rate is greater than 99%, and the single defect rate is less than 0.5%. DETAILED DESCRIPTION
[0032] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0033] Example
[0034] An embodiment of the present invention provides a method for welding an aluminum-scandium target and an aluminum alloy back plate. The specific welding conditions are shown in Table 1.
[0035] Table 1
[0036]
[0037]
[0038] Comparative Example 1
[0039] In this comparative example, except that the content of scandium in the aluminum-scandium target is 25 at %, other conditions are the same as those of Example 5.
[0040] Comparative Example 2
[0041] Except that the number of welding passes is 3, the other conditions of this comparative example are the same as those of Example 5.
[0042] Comparative Example 3
[0043] This comparative example has the same conditions as those of Example 5 except that the welding gun is not biased toward the aluminum-scandium target after being aligned with the weld.
[0044] Comparative Example 4
[0045] This comparative example adopts a brazing method to weld the aluminum-scandium target material and the aluminum alloy back plate in Example 4. The brazing solder is indium solder, the thickness of the brazing layer is 0.2 mm, and the temperature is 180°C.
[0046] Comparative Example 5
[0047] In this comparative example, the aluminum-scandium target material in Example 6 is welded to the aluminum alloy back plate by a brazing method. The brazing solder is indium solder, the thickness of the brazing solder layer is 0.2 mm, and the temperature is 280°C.
[0048] The back plates used in Examples 2-6 and Comparative Examples 1-5 are aluminum-magnesium alloy (model: 2024), and the back plates used in Example 1 are aluminum-magnesium-silicon alloy (model: 6061).
[0049] The welding bonding rates of the targets after welding in Examples 1-6 and Comparative Examples 1-5 were tested. The welding effect was verified by C-SCAN detection, and the detection conditions are shown in Table 2, and the results are shown in Table 3.
[0050] Table 2
[0051] Test conditions product Probe 10MHZ Sensitivity 36dB Material sound velocity 4000m / s Water distance 85.38mm X-axis spacing 0.2mm Y axis spacing 0.2mm Scan speed 100mm / s Scan range / Scan direction YX Threshold TH=60
[0052] Table 3
[0053]
[0054]
[0055] It can be seen from the test results in Table 3 that the welding method of the aluminum-scandium target material and the aluminum alloy back plate provided in Examples 1-6 of the present invention can ensure that the welding bonding rate is above 99% and the single defect rate is below 0.5%. In Comparative Example 1, electron beam welding is performed on an aluminum-scandium target material with a scandium content of 25at%, but since this type of target material is not suitable for electron beam welding, the welding bonding rate is greatly reduced. In Comparative Example 2, fewer passes of electron beam welding are used, resulting in a decrease in the welding bonding rate. In Comparative Example 3, the position of the welding gun is not adjusted, which also causes a decrease in the welding bonding rate. Comparative Examples 4 and 5 use brazing for welding, and their welding effects are significantly lower than the welding methods provided in the present application.
[0056] The applicant declares that the present invention illustrates the detailed process equipment and process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for welding an aluminum-scandium target and an aluminum alloy back plate, characterized in that: The welding method is electron beam welding, The content of scandium in the aluminum-scandium target is 5 to 10 at%, and the number of passes of the electron beam welding is ≥3; Or the content of scandium in the aluminum-scandium target is 10 to 15 at%, excluding 10 at%, and the number of passes of the electron beam welding is ≥ 4; Or the scandium content in the aluminum-scandium target is 15-20at%, excluding 15at%, and after the welding gun of the electron beam welding is aligned with the weld position, it deviates to one side of the aluminum-scandium target by 1-1.5mm, excluding 1; the number of passes of the electron beam welding is ≥5.
2. The welding method according to claim 1, characterized in that: The content of scandium in the aluminum-scandium target is 5-10 at%, and the beam current of the electron beam welding is 20-40 mA.
3. The welding method according to claim 1, characterized in that: The content of scandium in the aluminum-scandium target is 5-10 at%, and the focus depth of the electron beam welding is 515-560 mA.
4. The welding method according to claim 1, characterized in that: The content of scandium in the aluminum-scandium target is 5-10 at%, and the linear speed of the electron beam welding is 10-15 mm / s.
5. The welding method according to claim 1, characterized in that: The scandium content in the aluminum-scandium target is 10-15at%, excluding 10at%. After the welding gun of the electron beam welding is aligned with the weld position, it is deviated to one side of the aluminum-scandium target by 0-1mm, excluding 0.
6. The welding method according to claim 1, characterized in that: The content of scandium in the aluminum-scandium target is 10 to 15 at%, excluding 10 at%, and the beam current of the electron beam welding is 20 to 50 mA.
7. The welding method according to claim 1, characterized in that: The content of scandium in the aluminum-scandium target is 10-15 at%, excluding 10 at%, and the focus depth of the electron beam welding is 515-560 mA.
8. The welding method according to claim 1, characterized in that: The content of scandium in the aluminum-scandium target is 10 to 15 at%, excluding 10 at%, and the linear speed of the electron beam welding is 10 to 15 mm / s.
9. The welding method according to claim 1, characterized in that: The content of scandium in the aluminum-scandium target is 15 to 20 at%, excluding 15 at%, and the beam current of the electron beam welding is 20 to 60 mA.
10. The welding method according to claim 1, characterized in that: The content of scandium in the aluminum-scandium target is 15-20 at%, excluding 15 at%, and the focus depth of the electron beam welding is 515-560 mA.
11. The welding method according to claim 1, characterized in that: The content of scandium in the aluminum-scandium target is 15 to 20 at%, excluding 15 at%, and the linear speed of the electron beam welding is 10 to 15 mm / s.
Citation Information
Patent Citations
Aluminum-scandium alloy diffusion welding target material and preparation method and application thereof
CN112877653A
Diffusion welding method for high-scandium-content aluminum-scandium alloy target material and prepared welding assembly.
CN112894111A
Connection method of aluminum target material as sputtering target material and aluminum alloy backboard
CN104646817A
Aluminum-scandium alloy target blank and preparation method and application thereof
CN107841639A
Al-Sc alloy target material forming method
CN108097722A