A method for leaching lithium from spodumene

By using a low-temperature conversion and pressurized acid leaching method for spodumene, the problems of high energy consumption and equipment corrosion in the spodumene leaching process have been solved, achieving a low-energy, high-efficiency lithium extraction and an environmentally friendly production process.

CN114477241BActive Publication Date: 2024-11-19INST OF RESOURCES UTILIZATION & RARE EARTH DEV GUANGDONG ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210042075.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-14
Publication Date
2024-11-19
Estimated Expiration
2042-01-14

AI Technical Summary

Technical Problem

Existing spodumene leaching processes are energy-intensive, cause severe equipment corrosion, and have long process flows, making it difficult to effectively apply the sulfuric acid method to extract lithium from spodumene.

Method used

The method employs a low-temperature conversion of spodumene followed by pressurized acid leaching, which includes steps such as mixing and granulation, low-temperature roasting, pressurized leaching, and solid-liquid separation. This method avoids high-temperature roasting and combines low-temperature roasting with pressurized acid leaching, thereby reducing energy consumption and simplifying the process.

Benefits of technology

It reduces production energy consumption, minimizes equipment corrosion, shortens the process flow, and improves lithium extraction efficiency and environmental benefits.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the field of metallurgy technology, and specifically discloses a method for leaching lithium from spodumene. The method of the invention comprises the following steps: granulating spodumene concentrate and then roasting it at low temperature, ball milling the obtained roasted sand, and then boiling and pressurizing it in the presence of sulfuric acid to obtain lithium sulfate slurry, and then adding alkali for neutralization and purification to obtain lithium sulfate solution. The method can effectively reduce the roasting conversion temperature, reduce production energy consumption, reduce equipment corrosion, and improve the operating environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgy, and in particular to a method for leaching lithium from spodumene. Background Art

[0002] At present, the main methods for extracting lithium from lithium ore include limestone method, sulfuric acid method, sulfate method, chloride method and pressure cooking method. The sulfuric acid method is mature in technology and has the advantages of simple process, high lithium recovery rate and less waste residue. It is the mainstream method for producing lithium salt products from spodumene at home and abroad. The sulfate method is mainly used to treat lithium mica ore. It has the advantages of simple process flow, low roasting temperature, high lithium concentration in leachate, small evaporation and low energy consumption. However, this method is currently difficult to apply in spodumene mines. Chloride or fluoride needs to be added to roast spodumene to achieve better results, but chlorine (fluoride) compounds bring equipment corrosion and pollution control difficulties. High-pressure alkali cooking can reduce the roasting process, but it needs to be carried out under high pressure, with high alkali consumption and difficulty in solid-liquid separation. It is still in the research and development stage.

[0003] Natural α-spodumene is difficult to react with sulfuric acid (salt) to transform into soluble lithium sulfate. The sulfuric acid method requires high-temperature roasting to transform α-spodumene into β-spodumene, and transform the dense structure into a loose structure before it can be decomposed by sulfuric acid. In order to completely transform spodumene, the industrial roasting temperature is high, usually 1100-1200°C, which not only has high energy consumption and large carbon emissions, but also high-temperature rotary kiln roasting will cause the problem of melting and ringing of the furnace charge. In addition, the treatment of the roasted material by the sulfuric acid method includes two processes: acidification and leaching. The treatment process is relatively long, the acid gas volatilization is serious, the equipment is easily corroded, and the environmental protection treatment pressure is high.

[0004] Therefore, it is urgent to develop an effective spodumene leaching process to reduce energy consumption, shorten the process flow, and realize efficient and green resource production of spodumene. Summary of the invention

[0005] The main technical problem solved by the present invention is to provide a method for leaching lithium from spodumene. The method of the present invention has a low roasting conversion temperature, reduces production energy consumption, and reduces equipment corrosion.

[0006] In order to solve the above technical problems, the present invention provides a method for leaching lithium from spodumene, wherein the method adopts a method of low-temperature transformation of spodumene and then pressurized acid leaching to dissolve lithium, comprising the following steps:

[0007] S1, mixing-granulation: mixing spodumene concentrate, binder, sulfate and / or alkali compound, adding water to granulate, making wet granules with a particle size of 8-12 mm, and then drying;

[0008] S2, low temperature roasting: roasting the granular material obtained by drying in step S1 at a temperature lower than the phase transition temperature of α-spodumene, and cooling after roasting;

[0009] S3, pressure leaching: the roasted pellets obtained by roasting in step S2 are ball-milled with water to prepare slurry, the slurry is transferred to an autoclave, sulfuric acid and water are added, and the slurry is adjusted to obtain an initial leaching slurry; the initial leaching slurry is subjected to hot boiling and pressure leaching to obtain a lithium sulfate slurry;

[0010] S4, impurity removal and purification: the lithium sulfate slurry obtained in step S3 is neutralized with alkali, the pH value of the liquid is adjusted to ≥4.0, and the solid-liquid separation and impurity removal are carried out after stirring, and the obtained liquid phase is a lithium sulfate solution. The stirring is preferably carried out at room temperature, and the solid-liquid separation is carried out after stirring for 15 to 30 minutes to obtain a lithium sulfate solution, and the lithium leaching is completed.

[0011] The obtained lithium sulfate solution can be further processed by conventional industrial methods to prepare lithium salt products such as lithium carbonate.

[0012] As a preferred embodiment of the present invention, in step S1, the sulfate is sodium sulfate and / or potassium sulfate, and the addition amount is 2.0-10.0% of the mass of the spodumene concentrate.

[0013] In step S1, the alkali compound is caustic soda (NaOH) and / or soda ash (Na2CO3), and the added amount is 2.0-5.0% of the mass of the spodumene concentrate.

[0014] In step S1, the binder is an inorganic binder, preferably a mixture of any one or more of clay, water glass, and silica fume, and the added amount is 2.0-10.0% of the mass of the spodumene concentrate.

[0015] As a preferred embodiment of the present invention, in step S2, the calcination temperature is 820-900°C, and the calcination holding time is preferably 30-120 minutes.

[0016] As a preferred embodiment of the present invention, in step S3, the mass percentage concentration of the slurry is 50-60%.

[0017] The mass percentage concentration of the initial leaching pulp is 20-40%, and the concentration of sulfuric acid therein at the initial leaching is 1.0-1.5 mol / L.

[0018] The concentration of the sulfuric acid raw material used for leaching is 70% to 95% (w / w), and industrially recycled waste sulfuric acid can be used.

[0019] As a preferred embodiment of the present invention, in step S3, the leaching temperature is 180-230° C., the leaching pressure is 1.10-2.85 MPa, and the preferred leaching time is 60-150 min.

[0020] As a preferred embodiment of the present invention, in step S4, the alkali is an inorganic alkali, preferably any one or a combination of lime, caustic soda, calcium carbonate and sodium carbonate; further preferably, the pH value of the feed solution after neutralization is 4.0 to 7.0.

[0021] More preferably, in step S1, the sulfate is sodium sulfate or a mixture of sodium sulfate and potassium sulfate; and / or, the alkali compound is soda ash or caustic soda; and / or, the binder is clay, silica powder or water glass.

[0022] The method of the present invention is based on the composition characteristics of spodumene minerals and combines the existing lithium extraction methods to propose a fluorine-free and chlorine-free weak alkaline mixed salt low-temperature roasting method. The spodumene ore is roasted at a low temperature of 820°C to 900°C to reconstruct the physical phase of the spodumene ore, making it easy to be dissolved by acid leaching in the next step; the roasted sand obtained by roasting is pressurized and hot-boiled in an acidic environment to leach lithium in one step, and the leachate is purified to obtain a lithium sulfate solution. The lithium sulfate solution can then be prepared into lithium salt products such as lithium carbonate by conventional methods.

[0023] The method for extracting lithium from spodumene provided by the present invention, through the study of granulation process, adopts a suitable batching process to granulate the spodumene concentrate, and can be subjected to low-temperature roasting after granulation, that is, reacting at a temperature lower than the phase transition temperature of α-spodumene to generate a mineral that is easy to acid-leach. The method of the present invention avoids high-temperature roasting, reduces energy consumption, saves energy and reduces carbon, and then pressurizes acid leaching in one step, shortens the process flow, avoids acid gas volatilization, improves the operating environment, and improves production efficiency and environmental benefits. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is described in detail below through specific embodiments.

[0025] In the following examples, unless otherwise specified, the drugs used are all commercially available products. The concentrations or contents in each example are all in mass percentage.

[0026] Example 1

[0027] This embodiment provides a method for leaching lithium from spodumene, using spodumene concentrate, and the specific steps are:

[0028] Take 200g of spodumene concentrate (containing 5.77% Li2O), add 14.0g of sodium sulfate, 10.0g of sodium hydroxide and 10g of clay, mix well, add water to granulate, make small balls with a particle size of 8-10mm, and then dry at 150℃ for 30min;

[0029] The dry balls were placed in a muffle furnace and heated to 850°C for 90 min, then cooled;

[0030] The cold balls were crushed, and 200 mL of water was added to the balls to form a slurry, and the particle size was controlled to be ≤ 0.5 mm. The slurry with a concentration of 54.3% was obtained by ball milling;

[0031] Add 60 g of concentrated sulfuric acid with a concentration of 80% (w / w) to the slurry obtained by ball milling, then place it in an autoclave, add 170 mL of water, and obtain an initial leaching slurry with a concentration of 34.5%. The sulfuric acid concentration in the initial leaching slurry is 1.2 mol / L. Stir, heat to 220° C. for leaching, the leaching pressure is 2.4 MPa, and the temperature is kept for leaching for 60 min to obtain a leaching slurry;

[0032] The leached slurry is cooled to below 100°C, discharged into a beaker, stirred, and industrial caustic soda is added to neutralize and adjust the pH value of the slurry to 4.5. Stirring is stopped after 30 minutes. The neutralized slurry is separated into solid and liquid by vacuum filtration to obtain filter residue and filtrate.

[0033] The filter residue was countercurrent washed and dried three times, and the dry residue weighed 201.3 g and contained 0.29% Li2O. The filtrate (including the first washing water) was 495 mL, which was a lithium sulfate solution containing 20.21 g / L Li2O. Lithium carbonate and other lithium salt products could be extracted subsequently by conventional processes.

[0034] The Li2O leaching rate (calculated based on the Li2O content in the filter residue) of this embodiment is 94.94%.

[0035] Example 2

[0036] This embodiment provides a method for leaching lithium from spodumene, using spodumene concentrate, and the specific steps are:

[0037] Take 200g of spodumene concentrate (containing 5.77% Li2O), add 6.0g of sodium sulfate, 8.0g of sodium hydroxide, and 6.0g of silicon powder, mix well, add water to granulate, make small balls with a particle size of 8-10mm, and then dry at 150℃ for 30min;

[0038] The dry balls were placed in a muffle furnace and heated to 900°C for 60 min, then cooled;

[0039] The cold balls were crushed, and 200 mL of water was added to the balls to form a slurry, and the particle size was controlled to be ≤ 0.5 mm. The slurry with a concentration of 51.5% was obtained by ball milling;

[0040] Add 70 g of concentrated sulfuric acid with a concentration of 95% (w / w) to the slurry obtained by ball milling, place it in an autoclave, add 470 mL of water, and obtain an initial leaching slurry with a concentration of 22.5%. The sulfuric acid concentration in the initial leaching slurry is 1.0 mol / L. Stir, heat to 200°C for leaching, the leaching pressure is 1.6 MPa, and keep warm for 120 minutes to obtain a leached slurry;

[0041] The leached slurry is cooled to below 100°C, discharged into a beaker, stirred, and firstly lime is added to neutralize and adjust the pH value of the slurry to 2.0, and then sodium carbonate is added to adjust the pH value of the slurry to 5.0. Stirring is stopped after 30 minutes; the neutralized slurry is subjected to solid-liquid separation by vacuum filtration to obtain filter residue and filtrate;

[0042] The filter residue was countercurrent washed three times and dried, and the dry residue weighed 235.3 g and contained 0.21% Li2O. The filtrate (including the first washing water) was 795 mL, which was a lithium sulfate solution containing 13.64 g / L Li2O. Lithium carbonate and other lithium salt products could be extracted subsequently by conventional processes.

[0043] The Li2O leaching rate (calculated based on the Li2O content in the filter residue) of this embodiment is 95.72%.

[0044] Example 3

[0045] This embodiment provides a method for leaching lithium from spodumene, using spodumene concentrate, and the specific steps are:

[0046] Take 200g of spodumene concentrate (containing 5.77% Li2O), add 4.0g of sodium sulfate, 4.0g of potassium sulfate, 8.0g of sodium carbonate, and 6.0g of water glass, mix well, add water to granulate, and make small balls with a particle size of about 10-12mm, and then dry at 150℃ for 45min;

[0047] The dried granules were placed in a muffle furnace and heated to 820°C for 120 min and then cooled;

[0048] The cold balls were crushed, and 200 mL of water was added to the balls to form a slurry, and the particle size was controlled to be ≤ 0.5 mm. The slurry with a concentration of 51.8% was obtained by ball milling;

[0049] 60 g of concentrated sulfuric acid with a concentration of 70% (w / w) was added to the slurry obtained by ball milling, and the mixture was placed in an autoclave, and 100 mL of water was added to obtain an initial leaching slurry with a concentration of 37.4%, wherein the sulfuric acid concentration was 1.3 mol / L, and the mixture was stirred, heated to 185° C. for leaching, the leaching pressure was 1.2 MPa, and the leaching was carried out for 120 min under heat preservation to obtain a leached slurry;

[0050] The leached slurry is cooled to below 100°C, discharged into a beaker, stirred, and calcium carbonate is first added to neutralize and adjust the pH value of the slurry to 2.0, and then sodium carbonate is added to adjust the pH value of the slurry to 5.5. Stirring is stopped after 30 minutes; the neutralized slurry is subjected to solid-liquid separation by vacuum filtration to obtain filter residue and filtrate;

[0051] The filter residue was countercurrent washed three times and dried, and the dry residue weighed 226.4 g and contained 0.34% Li2O. The filtrate (including the first washing water) was 420 mL, which was a lithium sulfate solution containing 23.28 g / L Li2O. Lithium carbonate and other lithium salt products could be extracted subsequently by conventional processes.

[0052] The Li2O leaching rate (calculated based on the Li2O content in the filter residue) of this embodiment is 93.33%.

[0053] Example 4

[0054] This embodiment provides a method for leaching lithium from spodumene, using spodumene concentrate, and the specific steps are:

[0055] Take 200g of spodumene concentrate (containing 5.63% Li2O), add 10.0g of sodium sulfate and 10.0g of water glass, mix well, add water to granulate, make small balls with a particle size of 8-10mm, and then dry at 150℃ for 30min;

[0056] The dry balls were placed in a muffle furnace and heated to 860°C for 90 min and then cooled;

[0057] The cold balls were crushed, and 150 mL of water was added to make a slurry by ball grinding. The particle size was controlled to be ≤ 0.5 mm, and the slurry with a concentration of 58.3% was obtained by ball grinding.

[0058] The slurry obtained by ball milling was added with 50 g of concentrated sulfuric acid with a concentration of 95% (w / w), placed in an autoclave, and supplemented with 220 mL of water to obtain an initial leaching slurry with a concentration of 33.3%, wherein the concentration of sulfuric acid was 1.2 mol / L, stirred, heated to 220° C. for leaching, the leaching pressure was 2.4 MPa, and the leaching was carried out for 60 min under heat preservation to obtain a leaching slurry;

[0059] The leached slurry is cooled to below 100°C, discharged into a beaker, stirred, and sodium carbonate is first added to neutralize and adjust the pH value of the slurry to 1.5, and then caustic soda is added to adjust the pH value of the slurry to 6.0. Stirring is stopped after 30 minutes; the neutralized slurry is subjected to solid-liquid separation by vacuum filtration to obtain filter residue and filtrate;

[0060] The filter residue was countercurrent washed three times and dried, and the dry residue weighed 203.5 g and contained 0.23% Li2O. The filtrate (including the first washing water) was 505 mL, which was a lithium sulfate solution containing 19.43 g / L Li2O. Lithium carbonate and other lithium salt products could be extracted subsequently by conventional processes.

[0061] The Li2O leaching rate (calculated based on the Li2O content in the filter residue) of this embodiment is 95.84%.

[0062] Example 5

[0063] This embodiment provides a method for leaching lithium from spodumene, using spodumene concentrate, and the specific steps are:

[0064] Take 500g of spodumene concentrate (containing 5.63% Li2O), add 10.0g of sodium carbonate and 45.0g of water glass, mix well, add water to make balls, make small balls with a particle size of 8-10mm, and dry at 150℃ for 45min;

[0065] The dry balls were placed in a muffle furnace and heated to 880°C for 75 min and then cooled;

[0066] The cold balls were crushed, and 350 mL of water was added to make a slurry by ball grinding. The particle size was controlled to be ≤ 0.5 mm, and the slurry with a concentration of 59.8% was obtained by ball grinding.

[0067] The slurry obtained by ball milling was added with 130 g of concentrated sulfuric acid with a concentration of 93% (w / w), placed in an autoclave, and supplemented with 650 mL of water to obtain an initial leaching slurry with a concentration of 31.5%, wherein the sulfuric acid concentration was 1.2 mol / L, stirred, heated to 200°C for leaching, the leaching pressure was 1.6 MPa, and the leaching was carried out for 90 min at a heat preservation temperature to obtain a leached slurry;

[0068] The leached slurry is cooled to below 100°C, discharged into a beaker, stirred, and firstly lime is added to neutralize and adjust the pH value of the slurry to 2.0, and then sodium carbonate is added to adjust the pH value of the slurry to 5.2. Stirring is stopped after 30 minutes; the neutralized slurry is subjected to solid-liquid separation by vacuum filtration to obtain filter residue and filtrate;

[0069] The filter residue was countercurrent washed three times and dried, and the dry residue weighed 596.7 g and contained 0.23% Li2O. The filtrate (including the first washing water) was 1370 mL, which was a lithium sulfate solution containing 18.63 g / L Li2O. Lithium carbonate and other lithium salt products could be extracted subsequently by conventional processes.

[0070] The Li2O leaching rate (calculated based on the Li2O content in the filter residue) of this embodiment is 95.12%.

[0071] Although the present invention has been described in detail above by means of general description, specific implementation methods and tests, it is obvious to those skilled in the art that some modifications or improvements may be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A method for leaching lithium from spodumene, characterized in that: The method adopts a method of low-temperature transformation of spodumene and then pressurized acid leaching to dissolve lithium, comprising the following steps: S1, mixing-granulation: mixing spodumene concentrate, binder and sodium sulfate, adding water to granulate, making wet granules with a particle size of 8-12 mm, and then drying; the binder is clay, silica powder or water glass; the amount of sodium sulfate added is 2.0-10.0% of the mass of the spodumene concentrate; S2, low temperature roasting: roasting the granular material obtained by drying in step S1 at a temperature lower than the phase transition temperature of α-spodumene, and cooling after roasting; the roasting temperature is 820-900° C., and the roasting holding time is 30-120 min; S3, pressure leaching: the roasted pellets obtained by roasting in step S2 are ball-milled with water to prepare slurry, the slurry is transferred to an autoclave, sulfuric acid and water are added, and the slurry is adjusted to obtain an initial leaching slurry; the initial leaching slurry is subjected to hot boiling pressure leaching, the leaching temperature is 180-230°C, the leaching pressure is 1.10-2.85MPa, and the leaching time is 60-150min to obtain lithium sulfate slurry; S4, impurity removal and purification: the lithium sulfate slurry obtained in step S3 is neutralized with alkali, the pH value of the liquid is adjusted to ≥4.0, and the solid-liquid separation and impurity removal are carried out after stirring, and the obtained liquid phase is a lithium sulfate solution.

2. The method according to claim 1, characterized in that In step S1, the amount of the binder added is 2.0-10.0% of the mass of the spodumene concentrate.

3. The method according to claim 1 or 2, characterized in that: In step S3, the mass percentage concentration of the slurry is 50-60%; and / or the mass percentage concentration of the initial leaching slurry is 20-40%, wherein the concentration of sulfuric acid is 1.0-1.5 mol / L.

4. The method according to claim 1, characterized in that: In step S4, the alkali is selected from any one of caustic soda and sodium carbonate; the pH value of the feed solution after neutralization is 4.0-7.0.