A centrifugal spinning aerogel fiber, preparation method and application thereof

The preparation of aerogel fibers by centrifugal spinning solves the problems of slow speed and low yield in existing technologies, and realizes efficient aerogel fiber preparation, which is suitable for applications such as thermal insulation and catalyst support.

CN114481352BActive Publication Date: 2024-11-15SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210090933.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-26
Publication Date
2024-11-15
Estimated Expiration
2042-01-26

AI Technical Summary

Technical Problem

Existing methods for preparing aerogel fibers are slow, have low yields, and are difficult to scale up for mass production.

Method used

Aerogel fibers were prepared by centrifugal spinning. Hydrogel fibers were obtained in a coagulation bath by a high-speed centrifugal spinning device, followed by solvent replacement and drying to obtain centrifugally spun aerogel fibers.

Benefits of technology

It improves spinning speed, simplifies the process, and enables large-scale production of aerogel fibers. The fibers have high specific surface area and low thermal conductivity, making them suitable for thermal insulation, catalyst support, and gas separation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114481352B_ABST
    Figure CN114481352B_ABST
Patent Text Reader

Abstract

The present invention discloses a centrifugally spun aerogel fiber, a preparation method and application thereof. The preparation method comprises: providing a polymer solution or a polymer dispersion, injecting the polymer solution or the polymer dispersion into a rotating coagulation bath under high-speed rotation through a high-speed centrifugal spinning device, and centrifugally spinning to obtain a hydrogel fiber; performing solvent replacement on the hydrogel fiber, and then drying the replaced hydrogel fiber to obtain a centrifugally spun aerogel fiber. The shaped fiber product obtained by large-scale preparation of the centrifugally spun aerogel fiber of the present invention has an adjustable macroporous structure and low thermal conductivity. The centrifugally spun aerogel fiber of the present invention has low density, high specific surface area, good thermal insulation performance and good thermal insulation effect, and provides a new aerogel fiber spinning method. The preparation method used is simple, the spinning speed is fast, and the reaction conditions are mild. At the same time, it provides a new idea for the preparation of aerogel thermal insulation flocculants.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a centrifugal spinning aerogel fiber, in particular to a centrifugal spinning aerogel fiber, a preparation method and application thereof, and belongs to the technical field of functional nanofiber preparation. Background Art

[0002] Aerogel is a porous material with low density and high specific surface area, which shows great potential in applications such as catalysis and thermal insulation. At present, there are not many methods for preparing aerogel fibers, and there are many reports on preparing aerogels by wet spinning. Such as graphene aerogel phase change smart fibers prepared by wet spinning (Adv. Mater. 2018, 30, 1801754), Kevlar aerogel fibers with high mechanical strength and super thermal insulation properties prepared by wet spinning (ACS Nano 2019, 13, 5703-5711). In addition, for aerogel fibers with more complex processes, such as polyimide aerogel fibers, in addition to the reported freeze-spinning process, a gel-limited transition (SGCT) strategy has been developed for preparing polyimide aerogel fibers (ACSNano 2021, 15, 3, 4759-4768). However, the above-mentioned methods for preparing aerogel fibers all have the characteristics of slow speed and low yield, and how to increase the spinning speed of aerogel fibers is also a problem that needs to be solved.

[0003] A study has dissolved aramid in concentrated sulfuric acid to prepare a polymer solution, gelled it in a coagulation bath, and collected a large number of formed aramid nanofibers after drying at normal pressure (Matter 3, 742–758, September 2, 2020). Although water was used as a coagulation bath in this study, the fiber formation was essentially caused by the evaporation of the solvent during the high-speed spinning of the fiber. Summary of the invention

[0004] The main purpose of the present invention is to provide a centrifugal spinning aerogel fiber and a preparation method thereof, which at least solves one of the technical problems existing in the prior art.

[0005] Another object of the present invention is to provide an application of the centrifugally spun aerogel fiber.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0007] An embodiment of the present invention provides a method for preparing centrifugal spinning aerogel fibers, which comprises:

[0008] Providing a polymer solution or a polymer dispersion;

[0009] The polymer solution or polymer dispersion is injected into a rotating coagulation bath under high-speed rotation by a high-speed centrifugal spinning device to perform centrifugal spinning to obtain hydrogel fibers;

[0010] The hydrogel fibers are subjected to solvent replacement, and then the replaced hydrogel fibers are dried to obtain centrifugally spun aerogel fibers.

[0011] In some embodiments, the high-speed centrifugal spinning device includes a centrifugal rotating mechanism and a mechanical stirring device, the centrifugal rotating mechanism is fixedly connected to the mechanical stirring device, and the centrifugal rotating mechanism is provided with an opening.

[0012] In some embodiments, the preparation method includes: injecting the polymer solution or polymer dispersion into the centrifugal rotating mechanism, and under high-speed rotation, the polymer solution or polymer dispersion is ejected from the opening of the centrifugal rotating mechanism and enters a rotating coagulation bath to obtain hydrogel fibers.

[0013] The embodiment of the present invention also provides centrifugal spinning aerogel fibers prepared by the above method.

[0014] Furthermore, the centrifugally spun aerogel fiber is a nanoporous structure material mainly composed of mesopores with a pore size of 2 to 50 nm, micropores with a pore size of less than 2 nm, and macropores with a pore size greater than 50 nm. The density of the centrifugally spun aerogel fiber is 0.5 to 0.7 g / cm 3 , with a specific surface area of ​​100 to 1000 m 2 / g.

[0015] The embodiment of the present invention also provides the use of the centrifugally spun aerogel fiber in thermal insulation, catalyst carrier or gas separation carrier, etc.

[0016] The embodiment of the present invention further provides an aerogel fiber product, which is prepared from the aforementioned centrifugal spinning aerogel fiber, and the thermal conductivity of the aerogel fiber product is 0.2-0.5 W / m·K.

[0017] Compared with the prior art, the advantages of the present invention include:

[0018] (1) The centrifugally spun aerogel fiber provided by the present invention, wherein the construction of the disordered three-dimensional microscopic network and the macroscopic network makes the fiber product full of air and has a lower thermal conductivity;

[0019] (2) The preparation method of the centrifugal spinning aerogel fiber provided by the present invention has a simple process, a faster spinning speed than the traditional wet spinning method, and is easy to carry out large-scale production;

[0020] (3) The centrifugally spun aerogel fiber provided by the present invention has broad application prospects and can be used for thermal insulation, as well as as a catalyst carrier for catalytic reaction or as a carrier for gas separation. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 This is an optical photograph of a molded Kevlar centrifugal spun aerogel fiber prepared in a typical embodiment of the present invention.

[0023] Figure 2 It is a schematic diagram of the structure of a centrifugal spinning device used in a typical embodiment of the present invention.

[0024] Figure 3a , Figure 3b , Figure 3c They are respectively actual photos of the centrifugally spun aerogels obtained in Examples 1 to 3 of the present invention.

[0025] Figure 4a , Figure 4b These are actual photos of the centrifugally spun aerogels obtained in Examples 4 to 5 of the present invention.

[0026] Figure 5a , Figure 5b They are respectively a SEM image of the centrifugally spun aerogel fiber obtained in Example 6 of the present invention, a fiber diameter distribution bar graph, and a fitting curve graph.

[0027] Figure 6 This is an optical photograph of the centrifugally spun aerogel fiber state obtained in Example 7 of the present invention.

[0028] Figure 7a , Figure 7b They are respectively an optical photograph of the state of the centrifugally spun aerogel fiber obtained in Example 8 of the present invention and a nitrogen adsorption-desorption curve diagram.

[0029] Figure 8a , Figure 8b They are respectively an optical photograph of the state of the centrifugally spun aerogel fiber obtained in Example 9 of the present invention and a nitrogen adsorption-desorption curve diagram.

[0030] Figure 9a and Figure 9b This is a characterization result diagram of the thermal insulation performance of the molded Kevlar centrifugal spun aerogel.

[0031] Fig.10 This is a nitrogen adsorption-desorption curve of the centrifugally spun aerogel fiber obtained in Example 10 of the present invention.

[0032] Fig.11This is a nitrogen adsorption-desorption curve of the centrifugally spun aerogel fiber obtained in Example 11 of the present invention.

[0033] Description of the drawings: 1-mechanical stirring device, 2-centrifugal rotor, 3-magnetic stirrer. DETAILED DESCRIPTION

[0034] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution, its implementation process and principle will be further explained as follows.

[0035] Centrifugal spinning is a method for preparing micro / nano fibers. Compared with electrospinning, centrifugal spinning has advantages in terms of equipment and cost, such as no need to apply high-voltage power plant fields, and in terms of safety and pollution, such as the dangers caused by high voltage and polluting solvents or solutions. Centrifugal spinning can produce micro / nano fibers at high speed and low cost. The micro / nano fiber membrane prepared by centrifugal spinning has the advantages of large specific surface area, high porosity, and small pore diameter. At the same time, the centrifugal spinning equipment has a simple structure, mainly consisting of a motor, a spinning head, a collecting rod, etc. At present, there is no report on the strategy of using the centrifugal spinning method to prepare aerogels.

[0036] The present invention uses the centrifugal spinning method for the preparation of aerogel fibers for the first time, which increases the spinning speed compared to wet spinning or confined spinning, and also broadens the preparation ideas of aerogel fibers. The preparation of the present invention has a sol-gel process, and finally obtains centrifugal spinning aerogel fibers with a high specific surface area.

[0037] One aspect of an embodiment of the present invention provides a method for preparing a centrifugal spinning aerogel fiber, which comprises:

[0038] Providing a polymer solution or a polymer dispersion;

[0039] The polymer solution or polymer dispersion is injected into a rotating coagulation bath under high-speed rotation by a high-speed centrifugal spinning device to perform centrifugal spinning to obtain hydrogel fibers;

[0040] The hydrogel fibers are subjected to solvent replacement, and then the replaced hydrogel fibers are dried to obtain centrifugally spun aerogel fibers.

[0041] In some preferred embodiments, the preparation method comprises:

[0042] (1) Providing a polymer solution / dispersion of a certain concentration;

[0043] (2) injecting the polymer solution / dispersion of step (1) into a high-speed centrifugal spinning device to quickly obtain a large amount of hydrogel fibers in a coagulation bath;

[0044] (3) replacing the organic solvent from the hydrogel fiber obtained in step (2), and then replacing it with an aqueous solution of tert-butyl alcohol or anhydrous ethanol;

[0045] (4) The hydrogel obtained after the replacement in step (3) is dried to obtain the centrifugal spun aerogel fiber.

[0046] In some typical implementation cases, in step (1), the polymer solution or polymer dispersion includes any one or a combination of two or more of Kevlar dispersion, MCNT / Kevlar mixed solution, sodium alginate solution, nanocellulose solution, chitosan solution, etc., but is not limited thereto.

[0047] Furthermore, the concentration of the polymer in the polymer solution or polymer dispersion is 1.0 wt% to 5.0 wt%, preferably 1.0 wt% to 2.0 wt%.

[0048] For example, Kevlar dispersion is prepared by dissolving a certain weight of Kevlar short fibers in a dimethyl sulfoxide (DMSO) / potassium hydroxide solution or a dimethyl sulfoxide (DMSO) / potassium tert-butoxide solution, and stirring to obtain a Kevlar dispersion with a concentration of 1.0 wt% to 5.0 wt%.

[0049] In some embodiments, the polymer contained in the polymer solution or polymer dispersion includes any one or a combination of two or more of Kevlar, cellulose, sodium alginate, chitosan, etc., but is not limited thereto.

[0050] In some embodiments, in step (2), the high-speed centrifugal spinning device includes a centrifugal rotating mechanism (e.g., a centrifugal rotor) and a mechanical stirring device, the centrifugal rotating mechanism is fixedly connected to the mechanical stirring device, an opening is provided on the centrifugal rotating mechanism, and the rotation speed of the centrifugal rotating mechanism is 500 to 5000 r / min, preferably 1500 to 2500 r / min.

[0051] In some embodiments, the preparation method includes: injecting the polymer solution or polymer dispersion into the centrifugal rotating mechanism, and under high-speed rotation, the polymer solution or polymer dispersion is ejected from the opening of the centrifugal rotating mechanism and enters a rotating coagulation bath to obtain hydrogel fibers.

[0052] Furthermore, the spinning speed of the present invention is fast, and the speed of the centrifugal spinning is 2 to 20 m / s.

[0053] In some typical implementation cases, in step (2), the coagulation bath includes any one or a combination of two or more of deionized water, PVA aqueous solution, methyl cellulose aqueous solution, NaOH aqueous solution, CaCl2 solution, etc., but is not limited thereto.

[0054] In some typical implementation cases, step (3) includes: replacing the organic solvent in the obtained hydrogel fiber with deionized water 2 to 3 times until the organic solvent is removed, and then replacing it with a tert-butanol water mixed solution or anhydrous ethanol 1 to 2 times until the pores of the hydrogel fiber are filled with a uniform tert-butanol water mixed solution or anhydrous ethanol.

[0055] In some typical implementation cases, step (4) includes: drying the hydrogel fiber by vacuum freeze drying or supercritical drying to obtain the centrifugally spun aerogel fiber.

[0056] The spinning equipment adopted by the invention has a simple process, a centrifugal rotating mechanism and a mechanical stirring device are assembled into a centrifugal spinning equipment, and the production efficiency is high. In addition, the preparation method has a fast spinning speed, a simple spinning equipment process, and a high production efficiency.

[0057] Another aspect of the embodiments of the present invention further provides a centrifugal spun aerogel fiber prepared by the above method. The centrifugal spun aerogel fiber has a rich mesoporous and microporous structure.

[0058] Furthermore, the centrifugally spun aerogel fiber is a nanoporous structure material mainly composed of mesopores with a pore size of 2 to 50 nm, micropores with a pore size of less than 2 nm, and macropores with a pore size greater than 50 nm. The density of the centrifugally spun aerogel fiber is 0.5 to 0.7 g / cm 3 , with a specific surface area of ​​100 to 1000 m 2 / g.

[0059] Another aspect of the embodiments of the present invention further provides the application of the centrifugally spun aerogel fiber, which can be used for thermal insulation, and can also be used as a catalyst carrier for catalytic reactions or as a carrier for gas separation and the like.

[0060] Another aspect of the embodiments of the present invention further provides an aerogel fiber product, which is prepared from the centrifugally spun aerogel fiber.

[0061] Furthermore, the centrifugally spun aerogel fiber product provided by the present invention has an adjustable millimeter pore (macropore) structure and a low thermal conductivity of 0.2 to 0.5 W / m·K.

[0062] Furthermore, the present invention injects a polymer dispersion / solution into a high-speed centrifugal spinning rotor to quickly and efficiently obtain a large amount of hydrogel fibers in a coagulation bath, and obtains aerogel fibers after drying. The aerogel fibers are finished and formed to have thermal insulation properties.

[0063] Through the above technical scheme, the centrifugal spinning aerogel fiber provided by the present invention has a high spinning yield compared with the prior art, the equipment is simple and easy to operate, and the fiber regulation can be adjusted by controlling the process parameters; such as the rotation speed, spinning solution concentration, spinneret hole diameter, and collection distance to obtain the required fiber diameter and different specific surface areas. The fiber membrane can be directly used for oil-water separation, and can also be used as a catalyst carrier for catalytic reactions or as a sol-gel membrane carrier for gas separation.

[0064] The centrifugally spun aerogel fiber of the invention has low density, high specific surface area, good thermal insulation performance and excellent thermal insulation effect; a new aerogel fiber spinning method is provided, the preparation method used is simple, the spinning speed is fast, and the reaction conditions are mild, and a new idea is provided for the preparation of aerogel thermal insulation flocculants.

[0065] The technical solution of the present invention is further described in detail below through several embodiments and in combination with the accompanying drawings. However, the selected embodiments are only used to illustrate the present invention, but not to limit the scope of the present invention, and those skilled in the art may adjust according to actual conditions.

[0066] Example 1

[0067] The preparation method of centrifugal spinning aerogel fiber in this embodiment has the following specific steps:

[0068] (1) A certain amount of Kevlar staple fibers is weighed and dissolved in a dimethyl sulfoxide (DMSO) / potassium hydroxide or dimethyl sulfoxide (DMSO) / potassium tert-butoxide solution, and a 1.5 wt% Kevlar dispersion is obtained by mechanical stirring or magnetic stirring.

[0069] (2) Adoption Figure 2 The centrifugal spinning device shown in the figure performs centrifugal spinning, and the rotation speed is set to 500r / min. The speed of centrifugal spinning is about 5m / s. Deionized water is used as a coagulation bath, and the boundary of the coagulation bath is about 2cm away from the nozzle. A 1.5wt% (Kevlar) dispersion is injected into the centrifugal spinning rotor, and the coagulation bath is rotated to form a vortex, which is convenient for collecting and forming hydrogel fibers.

[0070] (3) The collected hydrogel fibers were replaced with deionized water twice, and then replaced with water and tert-butyl alcohol solution to shape them. They were placed in a vacuum freeze dryer and dried for 24 hours. The drying time was adjusted according to the fiber thickness to obtain centrifugal spinning aerogel fibers. The optical photos can be referred to Figure 3a .

[0071] (4) The collected aerogel fibers were subjected to nitrogen adsorption and desorption tests, and the specific surface area was found to be 210.8 m 2 / g.

[0072] (5) The collected aerogel fibers were subjected to a thermal conductivity test, and the thermal conductivity was 0.03452 W / m·k.

[0073] Figure 3a This is a photo of the actual state of the centrifugal aerogel fiber obtained in Example 1. The centrifugal device used for centrifugal spinning is shown in Figure 2, including a mechanical stirring device 1, a stainless steel centrifugal rotor 2, a collection container, and a magnetic stirrer 3. The centrifugal rotor 2 has a hole on the side, and the polymer dispersion / solution is rotated out of the hole at a high speed. When the coagulation bath is stationary, the liquid level is consistent. When rotating, the top of the vortex is higher than the centrifugal rotor opening, and the vortex diameter close to the centrifugal rotor is larger than the centrifugal rotor diameter. The speed of the cross-shaped magnetic stirring coagulation bath remains consistent each time. The polymer dispersion / solution rotated out of the centrifugal rotor quickly gels after contacting the coagulation bath to form hydrogel fibers, and rotates in the coagulation bath.

[0074] Example 2

[0075] The preparation method of centrifugal spinning aerogel fiber in this embodiment has the following specific steps:

[0076] (1) A certain amount of Kevlar staple fibers is weighed and dissolved in a dimethyl sulfoxide (DMSO) / potassium hydroxide or dimethyl sulfoxide (DMSO) / potassium tert-butoxide solution, and a 1.5 wt% Kevlar dispersion is obtained by mechanical stirring or magnetic stirring.

[0077] (2) Adoption Figure 2 The centrifugal spinning device shown in the figure performs centrifugal spinning, and the rotation speed is set to 2500r / min, and the centrifugal spinning speed is about 10m / s. Deionized water is used as a coagulation bath, and the boundary of the coagulation bath is about 2cm away from the nozzle. A 1.5wt% (Kevlar) dispersion is injected into the centrifugal spinning rotor, and the coagulation bath is rotated to form a vortex, which is convenient for collecting and forming hydrogel fibers.

[0078] (3) The collected hydrogel fibers were replaced with deionized water for three times, and then replaced with water and tert-butyl alcohol solution to shape them, and then placed in a vacuum freeze dryer for 24 hours. The drying time was increased or decreased according to the fiber thickness to obtain centrifugal spinning aerogel fibers.

[0079] (4) The collected aerogel fibers were subjected to nitrogen adsorption and desorption tests, and the specific surface area was found to be 223.5 m 2 / g.

[0080] (5) The collected aerogel fibers were subjected to a thermal conductivity test, and the thermal conductivity was 0.03364 W / m·k.

[0081] Figure 3b This is a photo of the actual state of the centrifugally spun aerogel fiber obtained in Example 2.

[0082] Example 3

[0083] The preparation method of centrifugal spinning aerogel fiber in this embodiment has the following specific steps:

[0084] (1) A certain amount of Kevlar staple fibers is weighed and dissolved in a dimethyl sulfoxide (DMSO) / potassium hydroxide or dimethyl sulfoxide (DMSO) / potassium tert-butoxide solution, and a 1.5 wt% Kevlar dispersion is obtained by mechanical stirring or magnetic stirring.

[0085] (2) Adoption Figure 2 The centrifugal spinning device is shown for centrifugal spinning, with a rotation speed of 5000 r / min and a centrifugal spinning speed of about 20 m / s. Deionized water is used as a coagulation bath, and the boundary of the coagulation bath is about 2 cm away from the nozzle. A 1.5 wt% (Kevlar) dispersion is injected into the centrifugal spinning rotor, and the coagulation bath is rotated to form a vortex, which is convenient for collecting and forming hydrogel fibers.

[0086] (3) The collected hydrogel fibers were replaced with deionized water twice, and then replaced with water and tert-butyl alcohol solution to shape them, and then placed in a vacuum freeze dryer for 24 hours. The drying time was increased or decreased according to the fiber thickness to obtain centrifugal spinning aerogel fibers.

[0087] (4) The collected aerogel fibers were subjected to nitrogen adsorption and desorption tests, and the specific surface area was found to be 248.2 m 2 / g.

[0088] (5) The collected aerogel fibers were subjected to a thermal conductivity test, and the thermal conductivity was 0.03233 W / m·k.

[0089] Figure 3c This is a photo of the actual state of the centrifugally spun aerogel fiber obtained in Example 3.

[0090] Example 4

[0091] The preparation method of centrifugal spinning aerogel fiber in this embodiment has the following specific steps:

[0092] (1) A certain amount of Kevlar staple fibers are weighed and dissolved in a dimethyl sulfoxide (DMSO) / potassium hydroxide or dimethyl sulfoxide (DMSO) / potassium tert-butoxide solution, and a 1.0 wt% Kevlar dispersion is obtained by mechanical stirring or magnetic stirring.

[0093] (2) Adoption Figure 2 The centrifugal spinning device shown in the figure performs centrifugal spinning, and the rotation speed is set to 500r / min, and the centrifugal spinning speed is about 2m / s. Deionized water is used as a coagulation bath, and the boundary of the coagulation bath is about 2cm away from the nozzle. A 1.0wt% (Kevlar) dispersion is injected into the centrifugal spinning rotor, and the coagulation bath is rotated to form a vortex, which is convenient for collecting and forming hydrogel fibers.

[0094] (3) The collected hydrogel fibers were replaced with deionized water twice, and then replaced with water and tert-butyl alcohol solution to shape them, and then placed in a vacuum freeze dryer for 24 hours. The drying time was increased or decreased according to the fiber thickness to obtain centrifugal spinning aerogel fibers.

[0095] (4) The collected aerogel fibers were subjected to nitrogen adsorption and desorption tests, and the specific surface area was found to be 220.3 m 2 / g.

[0096] (5) The collected aerogel fibers were tested for thermal conductivity, and the thermal conductivity was 0.03258 W / m·k

[0097] Figure 4a This is a photo of the centrifugally spun aerogel fiber obtained in Example 4.

[0098] Example 5

[0099] The preparation method of centrifugal spinning aerogel fiber in this embodiment has the following specific steps:

[0100] (1) A certain amount of Kevlar staple fibers are weighed and dissolved in a dimethyl sulfoxide (DMSO) / potassium hydroxide or dimethyl sulfoxide (DMSO) / potassium tert-butoxide solution, and a 2.0 wt% Kevlar dispersion is obtained by mechanical stirring or magnetic stirring.

[0101] (2) Adoption Figure 2 The centrifugal spinning device shown in the figure performs centrifugal spinning, and the rotation speed is set to 5000r / min, and the centrifugal spinning speed is about 20m / s. Deionized water is used as a coagulation bath, and the boundary of the coagulation bath is about 2cm away from the nozzle. A 2.0wt% (Kevlar) dispersion is injected into the centrifugal spinning rotor, and the coagulation bath is rotated to form a vortex, which is convenient for collecting and forming hydrogel fibers.

[0102] (3) The collected hydrogel fibers were replaced with deionized water twice, and then replaced with water and tert-butyl alcohol solution to shape them, and then placed in a vacuum freeze dryer for 24 hours. The drying time was increased or decreased according to the fiber thickness to obtain centrifugal spinning aerogel fibers.

[0103] (4) The collected aerogel fibers were subjected to nitrogen adsorption and desorption tests, and the specific surface area was found to be 200.6 m 2 / g.

[0104] (5) The collected aerogel fibers were subjected to a thermal conductivity test, and the thermal conductivity was 0.04286 W / m·k.

[0105] Figure 4b This is a photo of the centrifugally spun aerogel fiber obtained in Example 5.

[0106] Example 6

[0107] The preparation method of centrifugal spinning aerogel fiber in this embodiment has the following specific steps:

[0108] (1) A certain amount of Kevlar staple fibers is weighed and dissolved in a dimethyl sulfoxide (DMSO) / potassium hydroxide or dimethyl sulfoxide (DMSO) / potassium tert-butoxide solution, and a 1.5 wt% Kevlar dispersion is obtained by mechanical stirring or magnetic stirring.

[0109] (2) Adoption Figure 2 The centrifugal spinning device is shown for centrifugal spinning, and the rotation speed is set to 2500r / min, and the centrifugal spinning speed is about 10m / s. The coagulation bath is about 2cm away from the nozzle, and a 1.5wt% (Kevlar) dispersion is injected into the centrifugal spinning rotor. The coagulation bath is a 1.0% PVA solution, and the coagulation bath is rotated to form a vortex, which is convenient for collecting and forming hydrogel fibers.

[0110] (3) The collected hydrogel fibers were replaced with deionized water twice, and then replaced with water and tert-butyl alcohol solution to shape them, and then placed in a vacuum freeze dryer for 24 hours. The drying time was increased or decreased according to the fiber thickness to obtain centrifugal spinning aerogel fibers.

[0111] (4) The collected aerogel fibers were subjected to nitrogen adsorption and desorption tests, and the specific surface area was found to be 248.4 m 2 / g.

[0112] (5) The collected aerogel fibers were subjected to a thermal conductivity test, and the thermal conductivity was 0.04053 W / m·k.

[0113] Figure 5a , Figure 5b The SEM image of the centrifugally spun aerogel fiber obtained in this example, as well as the fiber diameter distribution bar graph and the fitting curve graph are shown.

[0114] Example 7

[0115] The preparation method of centrifugal spinning aerogel fiber in this embodiment has the following specific steps:

[0116] (1) A certain amount of Kevlar staple fibers is weighed and dissolved in a dimethyl sulfoxide (DMSO) / potassium hydroxide or dimethyl sulfoxide (DMSO) / potassium tert-butoxide solution, and a 1.5 wt% Kevlar dispersion is obtained by mechanical stirring or magnetic stirring.

[0117] (2) Adoption Figure 2 The centrifugal spinning device shown in the figure performs centrifugal spinning, and the rotation speed is set to 2500r / min, and the centrifugal spinning speed is about 10m / s. The coagulation bath is about 2cm away from the nozzle, and a 1.5wt% (Kevlar) dispersion is injected into the centrifugal spinning rotor. The coagulation bath is a 0.5% methylcellulose solution, and the coagulation bath is rotated to form a vortex, which is convenient for collecting and forming hydrogel fibers.

[0118] (3) The collected hydrogel fibers were replaced with deionized water twice, and then replaced with water and tert-butyl alcohol solution to shape them, and then placed in a vacuum freeze dryer for 24 hours. The drying time was increased or decreased according to the fiber thickness to obtain centrifugal spinning aerogel fibers.

[0119] (4) The collected aerogel fibers were subjected to nitrogen adsorption and desorption tests, and the specific surface area was found to be 235.3 m 2 / g.

[0120] (5) The collected aerogel fibers were subjected to a thermal conductivity test, and the thermal conductivity was 0.04028 W / m·k.

[0121] Figure 6 This is a photo of the centrifugally spun aerogel fiber obtained in this example.

[0122] Example 8

[0123] The preparation method of centrifugal spinning aerogel fiber in this embodiment has the following specific steps:

[0124] (1) Weigh a certain amount of Kevlar staple fibers, dissolve them in a dimethyl sulfoxide (DMSO) / potassium hydroxide or a dimethyl sulfoxide (DMSO) / potassium tert-butoxide solution, and obtain a 1.5 wt% Kevlar dispersion by mechanical stirring or magnetic stirring. Add 0.1% MCNT to the 1.5% wt% Kevlar dispersion to obtain a mixed dispersion.

[0125] (2) Adoption Figure 2 The centrifugal spinning device shown in the figure performs centrifugal spinning, and the rotation speed is set to 2500r / min, and the centrifugal spinning speed is about 10m / s. The coagulation bath is water, and the boundary is about 2cm away from the nozzle. The mixed dispersion is injected into the centrifugal spinning rotor, and the coagulation bath is rotated to form a vortex, which is convenient for collecting and forming hydrogel fibers.

[0126] (3) The collected hydrogel fibers were replaced with deionized water twice, and then replaced with water and tert-butyl alcohol solution to shape them, and then placed in a vacuum freeze dryer for 24 hours. The drying time was increased or decreased according to the fiber thickness to obtain centrifugal spinning aerogel fibers.

[0127] (4) The collected aerogel fibers were subjected to nitrogen adsorption and desorption tests, and the specific surface area was found to be 248.4 m 2 / g.

[0128] (5) The collected aerogel fibers were subjected to a thermal conductivity test, and the thermal conductivity was 0.03842 W / m·k.

[0129] Figure 7a , Figure 7b The optical photograph of the centrifugally spun aerogel fiber state obtained in this example and the nitrogen adsorption-desorption curve diagram are shown.

[0130] Example 9

[0131] The preparation method of centrifugal spinning aerogel fiber in this embodiment has the following specific steps:

[0132] (1) Weigh a certain amount of sodium alginate and dissolve it in water. Stir in a water bath at 60°C to obtain a 5% sodium alginate solution.

[0133] (2) Adoption Figure 2 The centrifugal spinning device shown in the figure performs centrifugal spinning, and the speed is set to 2500r / min, and the speed of centrifugal spinning is about 10m / s. The coagulation bath is a CaCl2 solution, which is about 2cm away from the nozzle. A 5% sodium alginate solution is injected into the centrifugal spinning rotor, and the coagulation bath is rotated to form a vortex, which is convenient for collecting and forming hydrogel fibers.

[0134] (3) The collected hydrogel fibers are replaced twice with deionized water, replaced with water and ethanol solutions, and then shaped, and then supercritically dried to obtain centrifugal spun aerogel fibers.

[0135] (4) The collected aerogel fibers were subjected to nitrogen adsorption and desorption tests, and the specific surface area was found to be 379.8 m 2 / g.

[0136] (5) The collected aerogel fibers were subjected to a thermal conductivity test, and the thermal conductivity was 0.03033 W / m·k.

[0137] Figure 8a , Figure 8b The optical photograph of the centrifugally spun aerogel fiber state obtained in this example and the nitrogen adsorption-desorption curve diagram are shown. Figure 9a and Figure 9b This is a characterization result diagram of the thermal insulation performance of molded Kevlar centrifugal spinning aerogel.

[0138] Example 10

[0139] The preparation method of centrifugal spinning aerogel fiber in this embodiment has the following specific steps:

[0140] (1) A certain amount of cotton was weighed and dissolved in an ionic liquid, and stirred in a water bath at 80° C. to obtain a 2% nanocellulose solution.

[0141] (2) Adoption Figure 2 The centrifugal spinning device is shown for centrifugal spinning, with a rotation speed of 2500 r / min and a centrifugal spinning speed of about 10 m / s. The coagulation bath is a deionized water solution, about 2 cm away from the nozzle, and a 2% nanocellulose solution is injected into the centrifugal spinning rotor, and the coagulation bath is rotated to form a vortex, which is convenient for collecting and forming hydrogel fibers.

[0142] (3) The collected hydrogel fibers are replaced twice with deionized water, replaced with water and ethanol solutions, and then shaped, and then supercritically dried to obtain centrifugal spun aerogel fibers.

[0143] (4) The collected aerogel fibers were subjected to nitrogen adsorption and desorption tests, and the specific surface area was found to be 302.6 m 2 / g.

[0144] (5) The collected aerogel fibers were subjected to a thermal conductivity test, and the thermal conductivity was 0.03328 W / m·k.

[0145] Fig.10 The nitrogen adsorption-desorption curve of the centrifugal spun aerogel fiber obtained in this example is shown.

[0146] Embodiment 11

[0147] The preparation method of centrifugal spinning aerogel fiber in this embodiment has the following specific steps:

[0148] (1) Weigh a certain amount of chitosan and dissolve it in formic acid solution, and stir it in a water bath at 60° C. to obtain a 2% chitosan solution.

[0149] (2) Adoption Figure 2 The centrifugal spinning device is shown for centrifugal spinning, with a rotation speed of 2500 r / min and a centrifugal spinning speed of about 10 m / s. The coagulation bath is a deionized water solution, about 2 cm away from the nozzle, and a 2% chitosan solution is injected into the centrifugal spinning rotor, and the coagulation bath is rotated to form a vortex, which is convenient for collecting and forming hydrogel fibers.

[0150] (3) The collected hydrogel fibers are replaced twice with deionized water, replaced with water and ethanol solutions, and then shaped, and then supercritically dried to obtain centrifugal spun aerogel fibers.

[0151] (4) The collected aerogel fibers were subjected to nitrogen adsorption and desorption tests, and the specific surface area was found to be 159.2 m 2 / g.

[0152] (5) The collected aerogel fibers were subjected to a thermal conductivity test, and the thermal conductivity was 0.03887 W / m·k.

[0153] Fig.11 The nitrogen adsorption-desorption curve of the centrifugal spun aerogel fiber obtained in this example is shown.

[0154] Through Examples 1-11, it can be found that the centrifugal spinning aerogel fiber obtained by the above technical solution of the present invention has a simple preparation process, strong universality, high specific surface area, and can be used for heat insulation and thermal insulation functions.

[0155] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.

[0156] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made and that elements of the described embodiments may be substituted with substantial equivalents without departing from the spirit and scope of the present invention. In addition, many modifications may be made to adapt a particular situation or material to the teachings of the present invention without departing from the scope of the present invention. Therefore, it is not intended herein to limit the present invention to the specific disclosed embodiments for carrying out the present invention, but rather it is intended that the present invention will include all embodiments within the scope of the appended claims.

Claims

1. A method for preparing centrifugal spinning aerogel fibers, characterized in that: include: Providing a polymer solution or a polymer dispersion; The polymer solution or polymer dispersion is injected into a rotating coagulation bath under high-speed rotation by a high-speed centrifugal spinning device to perform centrifugal spinning to obtain hydrogel fibers; Performing solvent replacement on the hydrogel fiber, and then drying the replaced hydrogel fiber to obtain centrifugal spinning aerogel fiber; The polymer solution or polymer dispersion includes any one of Kevlar dispersion, nanocellulose solution, sodium alginate solution, chitosan solution, or a combination of two or more thereof; The concentration of the polymer in the polymer solution or polymer dispersion is 1.0wt% to 5.0wt%; The high-speed centrifugal spinning device comprises a centrifugal rotor and a mechanical stirring device, wherein the centrifugal rotor is fixedly connected to the mechanical stirring device; an opening is arranged on the centrifugal rotor, and the diameter of the eddy current near the centrifugal rotor is larger than the diameter of the centrifugal rotor; Injecting the polymer solution or polymer dispersion into the centrifugal rotor, and in a high-speed rotating state, the polymer solution or polymer dispersion is ejected from the opening of the centrifugal rotor and enters the rotating coagulation bath to obtain hydrogel fibers; The centrifugal spinning speed is 2-20 m / s; The rotation speed of the centrifugal rotor is 500-5000 r / min.

2. The preparation method according to claim 1, characterized in that: The rotation speed of the centrifugal rotor is 1500-2500 r / min.

3. The preparation method according to claim 1, characterized in that: The coagulation bath includes any one of deionized water, PVA aqueous solution, methyl cellulose aqueous solution, NaOH aqueous solution, and CaCl2 solution, or a combination of two or more thereof.

4. The preparation method according to claim 1, characterized in that: The preparation method of the Kevlar dispersion comprises: dissolving Kevlar short fibers in a dimethyl sulfoxide / potassium hydroxide solution or a dimethyl sulfoxide / potassium tert-butoxide solution, and stirring to obtain the Kevlar dispersion.

5. The preparation method according to claim 1, characterized in that: The concentration of the polymer in the polymer solution or polymer dispersion is 1.0 wt % to 2.0 wt %.

6. The preparation method according to claim 1, characterized in that: include: The organic solvent in the obtained hydrogel fiber is replaced 2-3 times with deionized water, and then replaced 1-2 times with a tert-butanol-water mixed solution or anhydrous ethanol, until the pores of the hydrogel fiber are filled with a uniform tert-butanol-water mixed solution or anhydrous ethanol; Afterwards, the hydrogel fiber is dried by vacuum freeze drying or supercritical drying to obtain the centrifugally spun aerogel fiber.

7. A centrifugally spun aerogel fiber prepared by the method of any one of claims 1 to 6, wherein the centrifugally spun aerogel fiber is a nanoporous structure material mainly composed of mesopores with a pore size of 2 to 50 nm, micropores with a pore size of less than 2 nm, and macropores with a pore size greater than 50 nm, and the density of the centrifugally spun aerogel fiber is 0.5 to 0.7 g / cm 3 , with a specific surface area of ​​160~380m 2 / g.

8. Use of the centrifugally spun aerogel fiber according to claim 7 in thermal insulation, catalyst carrier or gas separation carrier.