Composite dielectric aluminum electrolytic capacitors
By using a composite oxide film and a voltage-resistant protective film doped with valve metal in aluminum electrolytic capacitors, combined with sodium oleate corrosion inhibitor, the problems of specific capacitance limit and corrosion failure are solved, resulting in higher capacitance and longer service life.
Patent Information
- Application Number
- CN202210182686.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-02-25
AI Technical Summary
The specific capacitance of existing aluminum electrolytic capacitors has reached its limit, and they are prone to corrosion failure.
A composite oxide film doped with valve metal is used as the medium, and micro-tunnels and voltage-resistant protective films are formed on the surface of the anode aluminum foil. Sodium oleate is used as a corrosion inhibitor, and the thickness of the release paper and the composition of the electrolyte are optimized.
This improves the specific capacitance of electrolytic capacitors, reduces leakage current and corrosion, extends service life, and enhances the safety and withstand voltage performance of capacitors.
Smart Images

Figure CN114496575B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of capacitors, and in particular to a composite dielectric aluminum electrolytic capacitor. Background Art
[0002] Aluminum electrolytic capacitors are known for their large capacitance per unit volume, small size, light weight and low price. They are widely used in electronic circuits for low-frequency filtering, audio coupling, DC isolation, energy storage, etc. At present, electrolytic capacitors are second only to ceramic capacitors in terms of quantity in the entire capacitor industry, and they occupy the first place in terms of output value, playing a pivotal role. Electrolytic capacitors are responsible for the task of large capacitance, but they are also difficult to integrate components. How to adapt to the development trend of light, thin and miniaturization has become an important issue for the future development of electrolytic capacitors. In recent years, with the rapid development of the information and energy industries, industries such as displays, fast charging power supplies, and automotive electronics have injected new vitality into the capacitor market. It can be predicted that the production and sales of aluminum electrolytic capacitors will not only not shrink for a long time in the future. Instead, they will have stronger vitality and broader development space. In order to adapt to the rapid development of electronic complete machines towards miniaturization and high-density assembly, researchers need to further study and explore solutions to reduce the size of capacitors, increase specific capacitance, extend life, and reduce equivalent series resistance.
[0003] The surface of the anode aluminum foil of traditional aluminum electrolytic capacitors is covered with a dense, non-porous aluminum oxide film, which is usually formed through electrochemical corrosion and chemical formation processes. This aluminum oxide film acts as a dielectric in the capacitor, which strongly affects the overall capacitance, withstand voltage and life of the aluminum electrolytic capacitor. Because the specific capacitance is inversely proportional to the distance between the electrodes, the thinner the oxide film means the shorter the distance between the two electrodes, which is conducive to the increase of specific capacitance. However, the technology of increasing the specific capacitance by expanding the surface area S of the anode foil and reducing the thickness d of the dielectric layer has reached its limit.
[0004] Figure 1 It is the mechanism of chloride ions penetrating oxide film in electrolytic corrosion. Due to the presence of a large number of oxygen vacancies in the aluminum oxide film lattice, corrosive anions and water molecules can easily pass through the oxide film layer to the oxide layer / metal interface through these oxygen vacancies, thereby further reacting with metal atoms to cause pitting corrosion to occur. In other words, the control step of pitting corrosion initiation is not determined by the process of chloride ions and water molecules passing through the oxide film, but by the high defect concentration and highly active aluminum atoms contained in the aluminum oxide film / metal aluminum interface. The dissolution rate and the rate at which aluminum complexes migrate from the aluminum oxide film / metal aluminum interface to the main solution.
[0005] In addition, in an electrolyte containing corrosive anions, the aluminum oxide film is in an unstable state. When the potential of the aluminum foil electrode changes suddenly, the unstable aluminum oxide film is prone to chemical reaction and electrostriction with the electrolyte, which will lead to residual stress in the aluminum oxide film. Furthermore, the residual stress will cause cracks on the aluminum oxide film, that is, the aluminum oxide film will be broken down. At the point where the oxide film is broken down, the electrolyte will directly contact the aluminum atoms, and at the same time, the chloride ions and oxygen atoms in the water molecules will compete with the aluminum atoms, causing the growth of pitting corrosion.
[0006] In addition, aluminum electrolytic capacitors often fail due to corrosion, especially those with high voltages above 400 V. The main reason for the failure is that the anode is severely corroded under high temperature load, which causes the capacitor to fail. Anode corrosion refers to the phenomenon that the aluminum rivets connecting the anode lead strip and the cover assembly are gradually electrochemically corroded after a period of time under certain load conditions, resulting in product failure. Summary of the invention
[0007] In view of the above technical problems, the present invention provides a composite dielectric aluminum electrolytic capacitor to solve the problem that the existing aluminum electrolytic capacitor specific capacitance technology has reached its limit and electrolytic capacitor corrosion failure often occurs.
[0008] Other features and advantages of the present disclosure will become apparent from the following detailed description, or may be learned in part by the practice of the present disclosure.
[0009] A composite dielectric aluminum electrolytic capacitor comprises a core package, a packaging container covering the core package, and a packaging cover plate sealing the packaging container;
[0010] The core package is formed by winding a cathode aluminum foil and an anode aluminum foil with a separator paper sandwiched between them, wherein the separator paper is impregnated with a liquid electrolyte mixed with a corrosion inhibitor, and the thickness of the separator paper is 0.014 μm-0.9 μm;
[0011] The anode aluminum foil is connected to an anode lead bar, and a voltage-resistant protective film is formed on the surface of the anode lead bar;
[0012] The surface of the anode aluminum foil is provided with tiny tunnels formed by an etching process, and the surface of the anode aluminum foil is formed with a composite oxide film uniformly composed of aluminum oxide doped with valve metal oxides, and the valve metal includes one or more of Hf, Zr, and Ti.
[0013] Furthermore, the composite oxide film is a layer or multiple layers of thin films formed by alternately pulse contacting the anode aluminum foil with a gas-phase precursor containing a valve metal and causing a gas-solid chemical adsorption reaction on the surface of the anode aluminum foil.
[0014] Furthermore, the protective film of the anode lead bar is a protective film formed after the anode lead bar is subjected to a high pressure treatment.
[0015] Furthermore, the corrosion inhibitor is sodium oleate.
[0016] Furthermore, the thickness of the release paper is 0.1 μm-0.8 μm.
[0017] Furthermore, the thickness of the release paper is 0.4 μm-0.6 μm.
[0018] The technical solution disclosed in this disclosure has the following beneficial effects:
[0019] The present invention adopts a composite oxide film doped with valve metal as the medium of the electrolytic capacitor. The relative dielectric constant of the composite oxide film component is greater than that of A1203 (A1203 is 8, HfO2 and ZrO2 are both about 20), so the electrolytic capacitor will have a larger specific capacitance.
[0020] The composite oxide film doped with valve metal is dense and uniform, which can improve the specific capacitance level of low-voltage electrolytic capacitors. At the same time, since the electrolytic capacitor will generate leakage current due to electrolyte corrosion when it is not working, it needs to be repaired by applying a DC voltage. Due to the good insulation performance of the composite film, the leakage current caused by defects in the composite medium caused by corrosion of chloride ions in the electrolyte will be greatly reduced.
[0021] Sodium oleate is added to the electrolyte as a corrosion inhibitor, which is a chemical substance or complex that effectively alleviates or prevents material corrosion. Its addition can alleviate the degree of corrosion and slow down the corrosion rate, thereby delaying the corrosion process, improving product performance and extending product service life. The specific capacity of the capacitor under DC corrosion is increased by about 20%, the weight loss of aluminum foil is significantly reduced, and the distribution of corrosion holes is more uniform.
[0022] The invention performs high-voltage chemical formation treatment on the anode lead bar, forms a protective film with sufficient voltage resistance on the surface of the lead bar, and improves the corrosion resistance of the lead bar. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a schematic diagram of the principle of chloride ions penetrating the oxide film in electrolytic corrosion in this specification;
[0024] Figure 2 A cross-sectional view of the core package structure in the embodiment of this specification;
[0025] Figure 3 This is a schematic diagram of the structure of the packaging container and the packaging cover plate in the embodiment of this specification;
[0026] Figure 4 This is a microstructure diagram of the composite oxide film in the examples of this specification.
[0027] Reference numerals:
[0028] 100, core package; 110, cathode aluminum foil; 120, anode aluminum foil; 121, composite oxide film; 122, anode lead; 130, isolation paper; 140, electrolyte; 200, packaging container; 300, packaging cover plate. DETAILED DESCRIPTION
[0029] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] like Figure 2 and Figure 3 As shown, the embodiment of this specification provides a composite dielectric aluminum electrolytic capacitor, including
[0031] A composite dielectric aluminum electrolytic capacitor includes a core package 100, a packaging container 200 covering the core package 100, and a packaging cover plate 300 sealing the packaging container 200;
[0032] The core package 100 is formed by winding a cathode aluminum foil 110 and an anode aluminum foil 120 with a separator 130 sandwiched therebetween. The separator 130 is impregnated with a liquid electrolyte 140 containing a mixed corrosion inhibitor. The separator 130 has a thickness of 0.014 μm to 0.9 μm.
[0033] The anode aluminum foil 120 is connected to an anode lead bar 122, and a voltage-resistant protective film is formed on the surface of the anode lead bar 122;
[0034] The surface of the anode aluminum foil 120 is provided with tiny tunnels formed by an etching process, and the surface of the anode aluminum foil 120 is provided with a composite oxide film 121 uniformly composed of aluminum oxide doped with valve metal oxides, wherein the valve metal includes one or more of Hf, Zr, and Ti.
[0035] Among them, continue to refer to Figure 2 , Figure 2 It is a cross-sectional view of a part of the structure of the core package 100. The anode aluminum foil 120, the cathode aluminum foil 110 and the separator paper 130 are overlapped and wound, and then soaked in the liquid electrolyte 140, and installed in the packaging container 200 through the separator. The tiny tunnels formed on the surface of the anode aluminum foil 120 are thousands of tiny tunnels formed by the high-purity aluminum corrosion process to increase the contact area with the electrolyte 140. Correspondingly, the composite oxide film 121 is formed on the inner wall of the tiny tunnel and other surfaces of the aluminum foil. Its cross section presents Figure 1The positive electrode of the capacitor is the anode aluminum foil 120, the medium is the composite oxide film 121 doped with valve metal, the real negative electrode of the capacitor is the conductive liquid electrolyte 140, and the cathode aluminum foil 110 is the lead-out electrode of the real negative electrolyte 140. The isolation paper 130 serves to isolate the anode foil and the cathode foil, and is also a carrier for storing the electrolyte 140. In addition, it can also repair the composite oxide film 121.
[0036] like Figure 4 As shown, Figure 4 This is the microstructure of the composite oxide in this embodiment. After valve metals are doped into aluminum oxide, the composite oxide forms a stable and dense structure, and the dielectric constants of valve metal oxides such as Ti, Zr, Hf, etc. are higher than those of aluminum oxide. Ferroelectric materials such as barium titanate and strontium titanate have dielectric constants ranging from several hundred to several thousand. Valve metal oxides or ferroelectric materials are compounded in aluminum anodized film to form a composite oxide film 121, which can greatly increase the specific volume of aluminum electrode foil, thereby significantly reducing the volume of aluminum electrolytic capacitors. At the same time, the composite oxide film 121 successfully modifies the aluminum oxide film, inhibiting the corrosion of the oxide film by chloride ions in the electrolyte 140; at the same time, the dense composite dielectric layer better blocks the penetration and ion exchange between the electrolyte 140 and the aluminum foil, thereby improving the life and safety of the aluminum electrolytic capacitor.
[0037] In one embodiment, the composite oxide film 121 is a layer or multiple layers of thin films formed by alternate pulse contact of a vapor phase precursor containing a valve metal with the anode aluminum foil 120 and a gas-solid phase chemical adsorption reaction on the surface of the anode aluminum foil 120 .
[0038] Among them, the composite oxide film 121 formed in the anode aluminum foil 120 by gas-solid phase chemical adsorption reaction has outstanding advantages such as large-area uniformity, good film thickness control, low-temperature growth, and high film quality. The high dielectric constant composite oxide film 121 obtained by using Hf, Zr, Ti and other element doping technology can significantly increase the specific capacitance of the electrolytic capacitor, reduce leakage current, and extend the time period that the capacitor needs to be energized.
[0039] In one experiment, the breakdown field strength of the composite oxide film 121 was about 7-8 MV / cm, which means that its working electric field strength value will be much higher than that of thin film capacitors and ceramic capacitors.
[0040] In one embodiment, the protective film of the anode lead bar 122 is formed by subjecting the anode lead bar 122 to a high pressure treatment.
[0041] Among them, the anode lead bar 122 of the traditional aluminum electrolytic capacitor is often corroded by chloride ions, and the products include additional hydrogen, etc., which can easily increase the internal pressure, causing bottom explosion, early failure, and low yield. By performing high-pressure chemical treatment on the anode lead bar 122, a protective film that can withstand sufficient voltage is formed on the surface of the lead bar, thereby improving the corrosion resistance of the lead bar.
[0042] In one embodiment, the corrosion inhibitor is sodium oleate.
[0043] Among them, sodium oleate is added to the electrolyte 140 as a corrosion inhibitor, and its hydrophilic group is adsorbed by the active points on the metal surface, and the hydrophobic group is arranged on the metal surface to form a hydrophobic film to inhibit corrosion, so as to delay the progress of corrosion, improve the performance of the product and extend the service life of the product. Sodium oleate is an environmentally friendly corrosion inhibitor, which can reduce environmental pollution. The anode aluminum foil 120 immersed in the corrosion inhibitor for a short time, because the corrosion inhibitor has not yet formed a complete protective film on its surface, and the aluminum oxide passivation film is mainly used to inhibit electrochemical corrosion at this time, so the aluminum surface model is mainly composed of the aluminum substrate, the passivation film and the liquid film formed between the surface and the solution. The electrochemical corrosion process mainly occurs on the aluminum substrate, and the equivalent circuit is a capacitor and a resistor in parallel. In the early stage of immersion, the aluminum oxide passivation film is not destroyed by Cl ions and has good compactness, so it has a certain hindering effect on the diffusion of Cl ions, thereby protecting the aluminum substrate from corrosion. The equivalent circuit adds a limited diffusion element in the passivation film. After long-term immersion, a protective film of corrosion inhibitor has been formed on the surface of the aluminum negative electrode. At this time, the cathode and anode potential polarizations increase, the corrosion current decreases significantly, the metal corrosion rate decreases greatly, the weight loss of the aluminum foil decreases significantly, and the corrosion hole distribution becomes more uniform.
[0044] In one embodiment, the thickness of the release paper 130 is 0.1 μm-0.8 μm.
[0045] In addition, the thickness of the release paper 130 is 0.4 μm-0.6 μm.
[0046] The thickness of the isolation paper 130 used in the present invention is usually 0.014μm-0.9μm, and the thickness of the electrolyte of other capacitors is basically tens or even hundreds of times the thickness of the isolation paper 130, and the dielectric constant of the dielectric is low. Therefore, the capacitance per unit volume of the aluminum electrolytic capacitor of the present invention is much higher than that of other capacitors. Since the surface area of the anode aluminum foil 120 after corrosion processing is hundreds of times its geometric area, and the thickness of the composite oxide film 121 layer is also less than a micron, the capacitor has a huge plate area and a very close plate distance, and can obtain a very large capacitance, which can reach a huge capacity of 3 F, and the rated voltage can cover 3-500 V.
[0047] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them; although the present invention is described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In addition, those skilled in the art can understand that although some embodiments described herein include certain features included in other embodiments instead of other features, the combination of features of different embodiments means that they are within the scope of the present invention and form different embodiments. For example, in the above claims, any one of the embodiments claimed for protection can be used in any combination. The information disclosed in this background technology section is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as admitting or suggesting in any form that the information constitutes prior art known to those skilled in the art.
Claims
1. A composite dielectric aluminum electrolytic capacitor, characterized in that: It includes a core package, a packaging container covering the core package, and a packaging cover plate sealing the packaging container; The core package is formed by winding a separator paper sandwiched between a cathode aluminum foil and an anode aluminum foil, wherein the separator paper is impregnated with a liquid electrolyte mixed with a corrosion inhibitor, and the thickness of the separator paper is 0.014 μm-0.9 μm; The anode aluminum foil is connected to an anode lead bar, and a voltage-resistant protective film is formed on the surface of the anode lead bar; The surface of the anode aluminum foil is provided with tiny tunnels formed by a corrosion process, and the surface of the anode aluminum foil is formed with a composite oxide film uniformly composed of an oxide of a valve metal doped with aluminum oxide, wherein the valve metal includes one or more of Hf, Zr, and Ti, and the composite oxide film is formed by a gas-phase precursor containing the valve metal alternately pulse-contacting the anode aluminum foil and undergoing a gas-solid chemical adsorption reaction on the surface of the anode aluminum foil to form one or more thin films.
2. The composite dielectric aluminum electrolytic capacitor according to claim 1, characterized in that: The protective film of the anode lead bar is a protective film formed after the anode lead bar is subjected to a high pressure treatment.
3. The composite dielectric aluminum electrolytic capacitor according to claim 1, characterized in that: The corrosion inhibitor is sodium oleate.
4. The composite dielectric aluminum electrolytic capacitor according to claim 1, characterized in that: The thickness of the release paper is 0.1 μm-0.8 μm.
5. The composite dielectric aluminum electrolytic capacitor according to claim 4, characterized in that: The thickness of the release paper is 0.4 μm-0.6 μm.