Resin composition and resin sheet
By controlling the semi-calcined hydrotalcite content and moisture content, reducing the moisture content of the resin composition, the problem of deterioration in the improvement of moisture permeability of the existing resin composition is solved, and the excellent sealing performance of electronic devices and the effect of delaying moisture intrusion is achieved.
Patent Information
- Application Number
- CN202080068326.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-30
- Filing Date
- 2020-09-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Although increasing the content of semi-calcined hydrotalcite can improve sealing performance when the conventional resin composition improves moisture permeability, the phenomenon of deterioration over time still exists, and the problem of deterioration caused by moisture cannot be effectively solved by increasing semi-calcined hydrotalcite.
By controlling the semi-calcined hydrotalcite content and moisture content in the resin composition, it is ensured to be less than 2500 ppm, and a drying treatment is used to reduce the moisture content to form a resin composition and a resin sheet with excellent sealing properties.
It has achieved a significant improvement in the sealing performance of electronic devices, delayed the invasion of moisture, and effectively suppressed the deterioration caused by internal moisture.
Smart Images

Figure BDA0003570522360000221
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition that can be used for sealing electronic devices and a resin sheet using the same. Background Art
[0002] In order to protect electronic devices such as organic EL (electroluminescence) devices and solar cells from moisture, resin compositions are used to seal the electronic devices.
[0003] As a resin composition suitable for sealing electronic devices, a composition containing a hygroscopic filler is known. For example, Patent Document 1 discloses a sealing resin composition containing a hygroscopic metal hydroxide and a sealing sheet composed of a support and a resin composition layer formed of the sealing resin composition.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent document 1: International Publication No. 2017 / 057708. Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] In the field of electronic devices, there is a constant demand for the improvement of the sealing performance (specifically, the performance of suppressing the degradation of the sealed object part) of the resin composition used for sealing electronic devices. The resin composition containing a polyolefin resin and semi-calcined hydrotalcite has excellent moisture permeability resistance and transparency, and can be used for the sealing of electronic devices. However, the following problem has been found: if the content of the semi-calcined hydrotalcite in the resin composition is increased in order to improve the moisture permeability resistance, then even if the content of the semi-calcined hydrotalcite as a hygroscopic filler is increased, the degradation of the sealed object part over time still increases, and there is a limit to the improvement of the sealing performance. The present invention is an invention completed with an eye on such a situation, and its purpose is to provide a resin composition with excellent sealing performance and a resin sheet using the same.
[0009] Technical solutions adopted to solve technical problems
[0010] The inventors of the present invention have conducted careful research and found that the moisture captured by the semi-calcined hydrotalcite reaches the sealing target part over time, causing its deterioration. If the content of the semi-calcined hydrotalcite increases, the deterioration becomes significant. In addition, it was found that in order to improve the sealing performance, the moisture resistance is improved by increasing the content of the semi-calcined hydrotalcite, while reducing the amount of internal moisture in the resin composition brought into by the semi-calcined hydrotalcite, thereby achieving an improvement in the sealing performance (moisture resistance and suppression of deterioration of the sealing target part caused by internal moisture).
[0011] The present invention based on the above findings is as follows;
[0012] [1] A resin composition comprising a polyolefin resin and semi-calcined hydrotalcite, wherein the content of the semi-calcined hydrotalcite exceeds 45% by mass relative to 100% by mass of the non-volatile components of the resin composition, and the water content is 2500 ppm or less based on the mass of the entire resin composition;
[0013] [2] The resin composition according to [1] above, wherein the water content is 2000 ppm or less based on the mass of the entire resin composition;
[0014] [3] The resin composition according to [1] or [2], wherein the content of the semi-calcined hydrotalcite is more than 45% by mass and less than 80% by mass relative to 100% by mass of the non-volatile components of the resin composition;
[0015] [4] The resin composition according to any one of [1] to [3] above, wherein the resin composition is used for sealing an electronic device;
[0016] [5] The resin composition according to [4] above, wherein the electronic device is an organic EL device or a solar cell;
[0017] [6] A resin sheet comprising a support and a layer of the resin composition according to any one of [1] to [3] above provided on the support;
[0018] [7] The resin sheet according to [6] above, wherein the resin sheet is used for sealing electronic devices;
[0019] [8] The resin sheet according to [7] above, wherein the electronic device is an organic EL device or a solar cell.
[0020] Effects of the Invention
[0021] According to the present invention, a resin composition having excellent sealing performance for electronic components and a resin sheet using the same can be obtained. DETAILED DESCRIPTION
[0022] The present invention will be described below in order. The examples, preferred embodiments, etc. described below can be combined with each other unless they are contradictory.
[0023] <Resin composition>
[0024] The resin composition of the present invention comprises a polyolefin resin and semi-calcined hydrotalcite. The sealing layer formed of the resin composition comprising the semi-calcined hydrotalcite can suppress the deterioration of electronic devices caused by moisture intruding from the outside air because the semi-calcined hydrotalcite absorbs moisture in the outside air.
[0025] However, in a sealing layer formed of a resin composition containing semi-calcined hydrotalcite, moisture captured by the semi-calcined hydrotalcite (which can be considered to be interlayer water of the semi-calcined hydrotalcite and moisture adhering to the surface of the semi-calcined hydrotalcite) is taken into the sealing layer, and this moisture reaches the electronic device over time, becoming a major factor causing deterioration of the electronic device.
[0026] Therefore, it is known that it is difficult to improve the sealing performance of the resin composition by simply increasing the usage of the semi-calcined hydrotalcite. In addition, after the inventors and others explored, it was found that even if the semi-calcined hydrotalcite was dried in advance and mixed into the resin composition, the above problem could not be solved. It is speculated that the reason is that even after the semi-calcined hydrotalcite is dried, it immediately captures the moisture in the air and restores the original state. Therefore, it is necessary to dry the resin composition containing the semi-calcined hydrotalcite so that the moisture contained in the resin composition is reduced to below a certain value.
[0027] Even in the case of increasing the usage amount of semi-calcined hydrotalcite in order to improve moisture permeability resistance, the water content of the resin composition comprising semi-calcined hydrotalcite can be fully reduced, so as to fully suppress the degradation of electronic devices caused by the moisture in the resin composition brought in by semi-calcined hydrotalcite, and a resin composition with excellent sealing performance can be provided. One of the features of the present invention based on this discovery is that, according to the mass reference relative to the entire resin composition (the entire resin composition comprising volatile components and non-volatile components), the water content of the resin composition is less than 2500ppm. The lower the water content, the better (ideally 0ppm), preferably less than 2000ppm, more preferably less than 1500ppm, further more preferably less than 1000ppm, and particularly preferably less than 800ppm. The water content can be measured according to the description in the embodiment column described later.
[0028] The water content below 2500ppm can be achieved by appropriately setting the drying conditions of the resin composition. For example, when a resin composition layer is formed by applying a varnish of the resin composition to a support and heating, the heating temperature when forming the resin composition layer (i.e., the heating temperature of the coating formed by the varnish coating) is preferably set to 70 to 150°C, and the heating time is preferably set to 10 minutes to 2 hours to form a resin composition layer, and then the drying temperature (heating temperature) is preferably set to 100 to 180°C, and the drying time is preferably set to 10 minutes to 7 weeks, and the formed resin composition layer is dried additionally, so that the water content of the resin composition layer can reach below 2500ppm.
[0029] When the formation of resin combination layer and the subsequent additional drying heating temperature are low, it may take a long time to make the moisture content of resin combination reach less than 2500ppm, or it may be difficult to reach less than 2500ppm.Therefore, the formation of resin combination layer and the subsequent additional drying heating temperature are preferably a certain degree of high temperature.But, in the formation of resin combination layer, if the heating temperature is too high, problems such as entering bubbles in resin combination layer may be generated.Therefore, it is better that the formation temperature of resin combination layer is set to relatively low, and the subsequent additional drying temperature of resin combination layer is set to the formation temperature higher than resin combination layer.
[0030] <Polyolefin resin>
[0031] As the polyolefin resin that can be used in the present invention, there is no particular limitation as long as it is a resin having a skeleton derived from an olefin. For example, the polyolefin resin described in Patent Document 1 can include known resins. The olefin is preferably a monoolefin having one olefinic carbon-carbon double bond and / or a diene having two olefinic carbon-carbon double bonds. As a monoolefin, preferably α-olefins such as ethylene, propylene, 1-butene, isobutylene, 1-pentene, 1-hexene, 1-heptene, and 1-octene can be mentioned; as a diene, preferably 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethylbutadiene, etc. can be mentioned. The skeleton derived from olefin in the polyolefin resin can be one kind or two or more kinds. Only one kind of polyolefin resin can be used, or two or more kinds can be used in combination.
[0032] Polyolefin resin can be a homopolymer, or a copolymer such as a random copolymer or a block copolymer. As a copolymer, copolymers of more than two olefins and copolymers of monomers other than olefins such as olefins and non-conjugated dienes, styrene, etc. can be enumerated. As the example of preferred copolymers, ethylene-non-conjugated diene copolymers, ethylene-propylene copolymers, ethylene-propylene-non-conjugated diene copolymers, ethylene-butylene copolymers, propylene-butylene copolymers, propylene-butylene-non-conjugated diene copolymers, styrene-isobutylene copolymers, styrene-isobutylene-styrene copolymers, etc. can be enumerated.
[0033] Examples of the polyolefin-based resin include the isobutylene-modified resin described in International Publication No. 2011 / 62167 and the styrene-isobutylene-modified resin described in International Publication No. 2013 / 108731.
[0034] The polyolefin resin is preferably a polybutene resin or a polypropylene resin. Here, "polybutene resin" refers to a resin in which the main unit (the unit with the largest content) of all olefin monomer units constituting the polymer is derived from butene, and "polypropylene resin" refers to a resin in which the main unit (the unit with the largest content) of all olefin monomer units constituting the polymer is derived from propylene.
[0035] When the polybutene resin is a copolymer, examples of monomers other than butene include styrene, ethylene, propylene, isoprene, etc. When the polypropylene resin is a copolymer, examples of monomers other than propylene include ethylene, butene, isoprene, etc.
[0036] From the viewpoint of imparting excellent physical properties such as adhesion and adhesion moisture and heat resistance, the polyolefin resin preferably includes: a polyolefin resin having an anhydride group (i.e., a carbonyloxycarbonyl group (-CO-O-CO-)) and / or a polyolefin resin having an epoxy group. As the anhydride group, for example, a group derived from succinic anhydride, a group derived from maleic anhydride, a group derived from glutaric anhydride, etc. can be cited. The polyolefin resin may have one or more anhydride groups. The polyolefin resin having an anhydride group can be obtained by, for example, grafting modification of the polyolefin resin with an unsaturated compound having an anhydride group under free radical reaction conditions. In addition, the unsaturated compound having an anhydride group may also be subjected to free radical copolymerization with olefins, etc. Similarly, the polyolefin resin having an epoxy group can be obtained by grafting and modifying the polyolefin resin under free radical reaction conditions with an unsaturated compound having an epoxy group, such as (meth) glycidyl acrylate, 4-hydroxybutyl acrylate glycidyl ether, and allyl glycidyl ether. In addition, the unsaturated compound having an epoxy group can also be free radical copolymerized with an olefin, etc. One or more polyolefin resins can be used, and a polyolefin resin having an acid anhydride group and a polyolefin resin having an epoxy group can be used in combination.
[0037] As the polyolefin resin having an acid anhydride group, a polybutene resin having an acid anhydride group and a polypropylene resin having an acid anhydride group are preferred. Also, as the polyolefin resin having an epoxy group, a polybutene resin having an epoxy group and a polypropylene resin having an epoxy group are preferred.
[0038] The concentration of the acid anhydride group in the polyolefin resin having an acid anhydride group is preferably 0.05 to 10 mmol / g, more preferably 0.1 to 5 mmol / g. The concentration of the acid anhydride group is obtained by the value of the acid value defined as the number of mg of potassium hydroxide required to neutralize the acid present in 1 g of the resin according to JIS K 2501. In addition, the amount of the polyolefin resin having an acid anhydride group in the polyolefin resin is preferably 0 to 70% by mass, more preferably 10 to 50% by mass.
[0039] In addition, the concentration of epoxy groups in the polyolefin resin having epoxy groups is preferably 0.05 to 10 mmol / g, more preferably 0.1 to 5 mmol / g. The epoxy group concentration is determined based on the epoxy equivalent obtained based on JIS K 7236-1995. In addition, the amount of the polyolefin resin having epoxy groups in the polyolefin resin is preferably 0 to 70% by mass, more preferably 10 to 50% by mass.
[0040] From the viewpoint of imparting excellent physical properties such as sealing performance, the polyolefin resin is particularly preferably a polyolefin resin having an anhydride group and a polyolefin resin having an epoxy group. Such a polyolefin resin forms a cross-linked structure by heating to react the anhydride group with the epoxy group, and can form a sealing layer having excellent sealing performance. The cross-linked structure can also be formed after sealing, but in the case where the sealing object such as an electronic device has a weak tolerance to heat, it is ideal to use a sealing film for sealing, and the cross-linked structure is formed in advance when the sealing film is manufactured.
[0041] As long as a suitable cross-linking structure can be formed, the ratio of the polyolefin resin having anhydride group to the polyolefin resin having an epoxy group is not particularly limited. The molar ratio of the epoxy group to the anhydride group (epoxy group:anhydride group) is preferably 100:10 to 100:400, more preferably 100:25 to 100:350, and particularly preferably 100:40 to 100:300.
[0042] In the resin composition of the present invention, when a polyolefin resin having an epoxy group is used, a polyolefin resin having a functional group (excluding an acid anhydride group) reactive with the epoxy group can be used. Examples of the functional group include a hydroxyl group, a phenolic hydroxyl group, an amino group, and a carboxyl group.
[0043] In the resin composition of the present invention, when a polyolefin resin having an acid anhydride group is used, a polyolefin resin having a functional group (excluding an epoxy group) that can react with the acid anhydride group can be used. Examples of the functional group include a hydroxyl group, a primary or secondary amino group, a mercapto group, and an oxetane group.
[0044] The number average molecular weight of polyolefin resin is not particularly limited, but from the good coating property of the varnish of bringing resin combination and the good compatibility viewpoint with other components in the resin combination, preferably below 1000000, more preferably below 750000, further more preferably below 500000, more preferably below 400000, further more preferably below 300000, especially preferably below 200000, preferably below 150000. On the other hand, from the depression during the coating of the varnish of preventing resin combination, the sealing performance of the formed resin combination layer is brought into play, and from the viewpoint of improving mechanical strength, the number average molecular weight is preferably more than 1000, more preferably more than 2000. It should be noted that the number average molecular weight in the present invention is measured by gel permeation chromatography (GPC) method (polystyrene conversion). The number average molecular weight measured by the GPC method can be specifically measured using LC-9A / RID-6A manufactured by Shimadzu Corporation as a measuring apparatus, using Shodex K-800P / K-804L / K-804L manufactured by Showa Denko K.K. as a column, using toluene or the like as a mobile phase, and measuring at a column temperature of 40°C, and calculated using a calibration curve of standard polystyrene.
[0045] From the viewpoint of suppressing the decrease in fluidity caused by the thickening of the varnish, the polyolefin resin in the present invention is preferably amorphous. Here, amorphous means that the polyolefin resin does not have a clear melting point, for example, a resin in which no clear peak is observed when the melting point of the polyolefin resin is measured by DSC (differential scanning calorimetry) can be used.
[0046] Next, specific examples of polyolefin resins are described. Specific examples of polypropylene resins include: "T-YP341" manufactured by Seikyo PMC Co., Ltd. (methacrylic acid glycidyl modified propylene-butene random copolymer, the amount of butene units relative to the total of propylene units and butene units 100% by mass: 29% by mass, epoxy group concentration: 0.638 mmol / g, number average molecular weight: 155,000), "T-YP279" manufactured by Seikyo PMC Co., Ltd. (maleic anhydride modified propylene-butene random copolymer, the amount of butene units relative to the total of propylene units and butene units 100% by mass: 36% by mass, anhydride group concentration: 0.464 mmol / g, number average molecular weight: 35,000), "T-YP276" manufactured by Seikyo PMC Co., Ltd. (methacrylic acid glycidyl modified propylene-butene random copolymer, relative to the total of propylene units and butene units 100% by mass: 36% by mass, anhydride group concentration: 0.464 mmol / g, number average molecular weight: 35,000). "T-YP312" manufactured by Seikyo PMC Co., Ltd. (maleic anhydride-modified propylene-butene random copolymer, the amount of butene units relative to the total of propylene units and butene units of 100 mass%: 29 mass%, anhydride group concentration: 0.464 mmol / g, number average molecular weight: 60900), "T-YP313" manufactured by Seikyo PMC Co., Ltd. (glycidyl methacrylate-modified propylene-butene random copolymer, the amount of butene units relative to the total of propylene units and butene units of 100 mass%: 29 mass%, epoxy group concentration: 0.638 mmol / g, number average molecular weight: 155000), etc.
[0047] Specific examples of polybutene resins include: "HV-1900" (polybutene, number average molecular weight: 2900) manufactured by ENEOS Corporation (formerly known as "JXTG Energy Corporation"), "HV-300M" (maleic anhydride-modified liquid polybutene (modified product of "HV-300" (number average molecular weight: 1400)) manufactured by Toho Chemical Industry Co., Ltd., number average molecular weight: 2100, number of carboxyl groups constituting acid anhydride groups: 3.2 / 1 molecule, acid value: 43.4 mgKOH / g, acid anhydride group concentration: 0.77 mmol / g), "OPPANOL B100" (polyisobutylene, viscosity average molecular weight: 1110000) manufactured by BASF, and "N50SF" (polyisobutylene, viscosity average molecular weight: 400000) manufactured by BASF.
[0048] Specific examples of styrene-isobutylene copolymers include: "SIBSTART102" manufactured by Kaneka Corporation (styrene-isobutylene-styrene block copolymer, number average molecular weight: 100,000, styrene content: 30% by mass), "T-YP757B" manufactured by Seikyo PMC Corporation (maleic anhydride-modified styrene-isobutylene-styrene block copolymer, anhydride group concentration: 0.464 mmol / g, number average molecular weight: 100,000), "T-YP766" manufactured by Seikyo PMC Corporation (glycidyl methacrylate-modified styrene-isobutylene-styrene block copolymer, anhydride group concentration: 0.464 mmol / g, number average molecular weight: 100,000). Ethylene-isobutylene-styrene block copolymer, epoxy group concentration: 0.638 mmol / g, number average molecular weight: 100000), "T-YP8920" manufactured by Seikou PMC Co., Ltd. (maleic anhydride modified styrene-isobutylene-styrene copolymer, anhydride group concentration: 0.464 mmol / g, number average molecular weight: 35800), "T-YP8930" manufactured by Seikou PMC Co., Ltd. (glycidyl methacrylate modified styrene-isobutylene-styrene copolymer, epoxy group concentration: 0.638 mmol / g, number average molecular weight: 48700).
[0049] The content of the polyolefin resin in the resin combination of the present invention is not particularly limited. But, from the viewpoint of the sealing performance of the resin combination and the operability, relative to the non-volatile component 100 mass % of the resin combination, this content is preferably more than 5 mass %, more preferably more than 10 mass %, further more preferably more than 15 mass %, preferably below 50 mass %, more preferably below 40 mass %, further more preferably below 35 mass %.
[0050] <Semi-calcined hydrotalcite>
[0051] Hydrotalcite can be classified into uncalcined hydrotalcite, semi-calcined hydrotalcite, and calcined hydrotalcite. In the present invention, semi-calcined hydrotalcite is used from the viewpoint of transparency and moisture permeation resistance of the resin composition.
[0052] Uncalcined hydrotalcite is, for example, natural hydrotalcite (Mg6Al2(OH) 16 Metal hydroxides with a layered crystal structure, such as those represented by CO3·4H2O) are composed of layers [Mg 1-X Al X (OH)2] X+ and the mesosphere [(CO3) X / 2 ·mH2O] X- The uncalcined hydrotalcite in the present invention is a concept including hydrotalcite-like compounds such as synthetic hydrotalcite. Examples of the hydrotalcite-like compounds include compounds represented by the following formula (I) and the following formula (II).
[0053] [M 2+1-x M 3+ x (OH)2] x+ ·[(A n- ) x / n ·mH2O] x- (I)
[0054] (Where M 2+ Represents Mg 2+ 、Zn 2+ Divalent metal ions, M 3+ Indicates Al 3+ , Fe 3+ Etc. trivalent metal ions, A n- Indicates CO3 2- , Cl - 、NO3 - For an anion with equal n valence, 0<x<1, 0≤m<1, and n is a positive number.)
[0055] In formula (I), M 2+ Mg is preferred 2+ , M 3+ Preferably Al 3+ , A n- CO3 is preferred 2- .
[0056] M 2+ x Al2(OH) 2x+6-nz (A n- ) z ·mH2O (II)
[0057] (Where M 2+ Represents Mg 2+ 、Zn 2+ Equivalent metal ions, A n- Indicates CO3 2- , Cl - 、NO3 - For an n-valent anion, x is a positive number greater than 2, z is a positive number less than 2, m is a positive number, and n is a positive number.)
[0058] In formula (II), M 2+ Mg is preferred 2+ , A n- CO3 is preferred 2- .
[0059] Semi-calcined hydrotalcite refers to a metal hydroxide having a layered crystal structure in which the amount of interlayer water is reduced or eliminated, obtained by calcining uncalcined hydrotalcite. When describing using a composition formula, "interlayer water" refers to "H2O" described in the composition formula of the uncalcined natural hydrotalcite and hydrotalcite-like compound described above.
[0060] On the other hand, calcined hydrotalcite refers to a metal oxide having an amorphous structure obtained by calcining uncalcined hydrotalcite or semi-calcined hydrotalcite, in which not only interlayer water disappears but also hydroxyl groups disappear by condensation dehydration.
[0061] Uncalcined hydrotalcite, semi-calcined hydrotalcite and calcined hydrotalcite can be distinguished by saturated water absorption. The saturated water absorption of semi-calcined hydrotalcite is 1% by mass or more and less than 20% by mass. On the other hand, the saturated water absorption of uncalcined hydrotalcite is less than 1% by mass, and the saturated water absorption of calcined hydrotalcite is 20% by mass or more.
[0062] The "saturated water absorption rate" in the present invention means: 1.5 g of a test sample (e.g., semi-calcined hydrotalcite) is weighed on a balance, the initial mass is measured, and then the sample is allowed to stand for 200 hours in a small environmental tester (SH-222 manufactured by ESPEC) set at 60° C. and 90% RH (relative humidity) under atmospheric pressure. The mass increase rate of the mass after standing for 200 hours relative to the initial mass can be calculated by the following formula (i):
[0063] Saturated water absorption (mass %) = 100 × (mass after moisture absorption - initial mass) / initial mass (i).
[0064] The saturated water absorption of the semi-calcined hydrotalcite is preferably at least 3 mass% and less than 20 mass%, more preferably at least 5 mass% and less than 20 mass%.
[0065] In addition, the uncalcined hydrotalcite, the semi-calcined hydrotalcite and the calcined hydrotalcite can be distinguished by the thermogravimetric reduction rate measured by thermogravimetric analysis. The thermogravimetric reduction rate of the semi-calcined hydrotalcite at 280°C is less than 15% by mass, and the thermogravimetric reduction rate thereof at 380°C is 12% by mass or more. On the other hand, the thermogravimetric reduction rate of the uncalcined hydrotalcite at 280°C is 15% by mass or more, and the thermogravimetric reduction rate of the calcined hydrotalcite at 380°C is less than 12% by mass.
[0066] For thermogravimetric analysis, TG / DTAEXSTAR6300 manufactured by Hitachi High-Tech Science Co., Ltd. was used to weigh 5 mg of hydrotalcite into an aluminum sample pan, and the pan was opened without a lid, and the temperature was raised from 30°C to 550°C at a rate of 10°C / min in an atmosphere with a nitrogen flow rate of 200 mL / min. The thermogravimetric reduction rate can be calculated by the following formula (ii):
[0067] Thermal weight reduction rate (mass %) = 100 × (mass before heating - mass when reaching a predetermined temperature) / mass before heating (ii).
[0068] In addition, uncalcined hydrotalcite, semi-calcined hydrotalcite and calcined hydrotalcite can be distinguished based on the peaks and relative intensity ratios measured by powder X-ray diffraction. For semi-calcined hydrotalcite, by powder X-ray diffraction, a peak split into two is shown near 8 to 18° 2θ, or a peak having a shoulder peak is shown by the synthesis of two peaks, and the relative intensity ratio (low-angle side diffraction intensity / high-angle side diffraction intensity) of the diffraction intensity of the peak or shoulder peak appearing on the low-angle side (= low-angle side diffraction intensity) and the diffraction intensity of the peak or shoulder peak appearing on the high-angle side (= high-angle side diffraction intensity) is 0.001 to 1,000. On the other hand, uncalcined hydrotalcite has only one peak near 8 to 18°, or the relative intensity ratio of the diffraction intensity of the peak or shoulder peak appearing on the low-angle side to the peak or shoulder peak appearing on the high-angle side falls outside the aforementioned range. Calcined hydrotalcite has no characteristic peak in the range of 8° to 18°, but has a characteristic peak at 43°. Powder X-ray diffraction measurement was performed using a powder X-ray diffraction apparatus (Empyrean, manufactured by PANalytical) with CuKα The voltage was 45 V, the current was 40 mA, the sampling width was 0.0260°, the scanning speed was 0.0657° / s, and the diffraction angle range (2θ) was 5.0131 to 79.9711°. The peak search was performed using the peak search function of the software attached to the diffraction device under the conditions of "minimum significance of 0.50, minimum peak tip of 0.01°, maximum peak tip of 1.00°, peak baseline width of 2.00°, and method of minimum value of second-order differential".
[0069] The BET specific surface area of the semi-calcined hydrotalcite and the calcined hydrotalcite is preferably 1 to 250 m 2 / g, preferably 5 to 200 m 2 The BET specific surface area can be calculated by the BET multipoint method using a specific surface area measuring apparatus (Macsorb HM 1210, manufactured by Mounttech Co., Ltd.) by allowing nitrogen to adsorb on the surface of a sample.
[0070] The particle size of the semi-calcined hydrotalcite is preferably from 1 to 1000 nm, more preferably from 10 to 800 nm. The particle size is the median particle size of a particle size distribution obtained by laser diffraction scattering particle size distribution measurement (JIS Z 8825) on a volume basis.
[0071] Semi-calcined hydrotalcite can be a material that has been surface treated with a surface treatment agent. As the surface treatment agent used for surface treatment, for example, higher fatty acids, alkyl silanes, silane coupling agents, etc. can be used, wherein higher fatty acids and alkyl silanes are preferred. One or more surface treatment agents can be used.
[0072] Examples of the higher fatty acid include higher fatty acids having 18 or more carbon atoms, such as stearic acid, montanic acid, myristic acid, and palmitic acid, among which stearic acid is preferred. These can be used alone or in combination of two or more.
[0073] Examples of the alkylsilanes include methyltrimethoxysilane, ethyltrimethoxysilane, hexyltrimethoxysilane, octyltrimethoxysilane, decyltrimethoxysilane, octadecyltrimethoxysilane, dimethyldimethoxysilane, octyltriethoxysilane, and n-octadecyldimethyl(3-(trimethoxysilyl)propyl)ammonium chloride. One or more of these may be used.
[0074] Examples of the silane coupling agent include epoxy-based silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyl(dimethoxy)methylsilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; mercapto-based silane coupling agents such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, and 11-mercaptoundecyltrimethoxysilane; and 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyldimethoxymethylsilane, N-phenyl-3-aminopropyltrimethoxysilane, N-methylaminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2 Amino-based silane coupling agents such as (-aminoethyl)-3-aminopropyldimethoxymethylsilane; urea-based silane coupling agents such as 3-ureapropyltriethoxysilane; vinyl-based silane coupling agents such as vinyltrimethoxysilane, vinyltriethoxysilane and vinylmethyldiethoxysilane; styrene-based silane coupling agents such as p-styryltrimethoxysilane; acrylate-based silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltrimethoxysilane; isocyanate-based silane coupling agents such as 3-isocyanatepropyltrimethoxysilane; sulfide-based silane coupling agents such as bis(triethoxysilylpropyl)disulfide and bis(triethoxysilylpropyl)tetrasulfide; phenyltrimethoxysilane, methacryloxypropyltrimethoxysilane, imidazolesilane, triazinesilane, etc. These can be used alone or in combination.
[0075] The surface treatment of semi-calcined hydrotalcite, etc. can be carried out, for example, in the following manner: using a mixer to stir and disperse the untreated semi-calcined hydrotalcite, etc. at room temperature, spraying and adding a surface treatment agent, and stirring for 5 to 60 minutes. As a mixer, a known mixer can be used, such as a V-type mixer (blender), a ribbon blender (ribbon blender), a double cone mixer (バブルコーンブレンダー) and other mixers, Henschel mixers (Henschel mixer) and concrete mixers, mixers, ball mills, cutters (cutter mills), etc. can be cited. In addition, when the hydrotalcite is crushed with a ball mill, the aforementioned higher fatty acids, alkylsilanes or silane coupling agents can also be added and surface treated. The amount of the surface treatment agent used also varies according to the type of hydrotalcite or the type of the surface treatment agent, but it is preferably 1 to 10 parts by mass relative to 100 parts by mass of hydrotalcite that has not been surface treated. In the present invention, the surface-treated semi-calcined hydrotalcite is included in the concept of "semi-calcined hydrotalcite" in the present invention.
[0076] From the viewpoint of the sealing performance of the resin combination in the present invention, relative to the non-volatile component 100% by mass of resin combination, the content of the semi-calcined hydrotalcite in the resin combination of the present invention is to exceed 45% by mass. This content is preferably more than 50% by mass, more preferably more than 55% by mass, and further more preferably more than 60% by mass. In addition, as long as the effect of the present invention is brought into play, the upper limit of this content is not particularly limited, but from the viewpoints such as the transparency of resin combination, this content is preferably below 80% by mass, more preferably below 75% by mass, and further more preferably below 70% by mass.
[0077] As long as it is within the scope of not damaging the effect of the present invention, the resin composition of the present invention may include fillers other than semi-calcined hydrotalcite. As fillers other than semi-calcined hydrotalcite, for example, inorganic fillers such as silicon dioxide, aluminum oxide, barium sulfate, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, boron nitride, aluminum borate, barium titanate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium zirconate, calcium zirconate, silicate, and organic fillers such as rubber particles, silicone powder, nylon powder, and fluororesin powder can be cited. Relative to 100 parts by mass of the content of semi-calcined hydrotalcite, the content of fillers other than semi-calcined hydrotalcite is preferably less than 50 parts by mass, more preferably less than 30 parts by mass, further preferably less than 20 parts by mass, and further preferably less than 10 parts by mass.
[0078] <Adhesiveness-imparting agent>
[0079] The resin composition of the present invention may further contain an adhesion-imparting agent. The adhesion-imparting agent is also referred to as a tackifier and is a component that imparts adhesion to the composition. As the adhesion-imparting agent, there is no particular limitation, and preferably terpene resins, modified terpene resins (hydrogenated terpene resins, terpene-phenol copolymer resins, aromatic modified terpene resins, etc.), coumarone resins, indene resins, petroleum resins (aliphatic petroleum resins, hydrogenated alicyclic petroleum resins, aromatic petroleum resins, aliphatic aromatic copolymer petroleum resins, alicyclic petroleum resins, dicyclopentadiene petroleum resins and hydrides thereof, etc.) are used.
[0080] As commercially available products that can be used as adhesive imparting agents, for example, the following products can be cited. As terpene resins, YS RESIN PX, YS RESIN PXN (both manufactured by Yasuhara Chemical Co., Ltd.) and the like can be cited; as aromatic modified terpene resins, YS RESIN TO, TR series (both manufactured by Yasuhara Chemical Co., Ltd.) and the like can be cited; as hydrogenated terpene resins, CLEARON P, CLEARON M, CLEARON K series (all manufactured by Yasuhara Chemical Co., Ltd.) and the like can be cited; as terpene-phenol copolymer resins, YS POLYSTER 2000, POLYSTER U, POLYSTER T, POLYSTER S, Microace G (all manufactured by Yasuhara Chemical Co., Ltd.) and the like can be cited; as hydrogenated alicyclic petroleum resins, Escorez As aromatic petroleum resins, ENDEX 155 (manufactured by Eastman Chemical Company) and the like can be cited; as aliphatic aromatic copolymer petroleum resins, Quintone D100 (manufactured by Zeon Corporation of Japan) and the like can be cited; as alicyclic petroleum resins, Quintone 1325, Quintone 1345 (manufactured by Zeon Corporation of Japan) and the like can be cited; as saturated hydrocarbon resins, ARKON P100, ARKON P125, ARKON P140, TFS 13-030 (manufactured by Arakawa Chemical Co., Ltd.) and the like can be cited.
[0081] From the viewpoint of softening the sheet in the lamination step of the resin composition sheet and having desired heat resistance, the softening point of the tackifier is preferably from 50 to 200° C., more preferably from 90 to 180° C., further preferably from 100 to 150° C. The softening point is measured by the ring and ball method in accordance with JIS K2207.
[0082] Adhesion imparting agent can use 1 kind or use 2 or more kinds in combination.The content of adhesion imparting agent in resin combination is not particularly limited.But, from the viewpoint of maintaining the good sealing performance of resin combination, when using adhesion imparting agent, relative to the non-volatile component 100 mass % of resin combination, its content is preferably below 50 mass %, more preferably below 40 mass %, further more preferably below 30 mass %.On the other hand, from the viewpoint with sufficient adhesion, when using adhesion imparting agent, relative to the non-volatile component 100 mass % of resin combination, its content is preferably more than 5 mass %, more preferably more than 10 mass %.
[0083] From the viewpoint of the adhesion, sealing performance, transparency, etc. of the resin composition, petroleum resin is preferred. Examples of the petroleum resin include aliphatic petroleum resins, aromatic petroleum resins, aliphatic-aromatic copolymer petroleum resins, alicyclic petroleum resins, and the like. From the viewpoint of the adhesion, sealing performance, compatibility, etc. of the resin composition, aromatic petroleum resins, aliphatic-aromatic copolymer petroleum resins, and alicyclic petroleum resins are preferred. In addition, from the viewpoint of achieving good transparency, alicyclic petroleum resins are particularly preferred. Alicyclic petroleum resins obtained by hydrogenating aromatic petroleum resins may also be used. In this case, the hydrogenation rate of the alicyclic petroleum resin is preferably 30 to 99%, more preferably 40 to 97%, and further preferably 50 to 90%. If the hydrogenation rate is too low, there is a tendency for the transparency to decrease due to coloring; if the hydrogenation rate is too high, there is a tendency for the production cost to increase. The hydrogenation rate can be determined by the ratio of hydrogen atoms in the aromatic ring before and after hydrogenation. 1 The ratio of the peak intensity of H-NMR is obtained. As the alicyclic petroleum resin, a cyclohexane ring-containing hydrogenated petroleum resin or a dicyclopentadiene hydrogenated petroleum resin is particularly preferred. The petroleum resin can be used alone or in combination of two or more. The number average molecular weight Mn of the petroleum resin is preferably 100 to 2000, more preferably 700 to 1500, and further preferably 500 to 1000.
[0084] <Curing agent and / or curing accelerator>
[0085] The resin composition of the present invention may include a curing agent and / or a curing accelerator (preferably a curing accelerator). Both the curing agent and the curing accelerator may be used in one kind only, or in combination of two or more kinds. As the curing agent, for example, imidazole compounds, tertiary amine / quaternary ammonium compounds, dimethyl urea compounds, organic phosphine compounds, primary amine / secondary amine compounds, etc. may be cited. As the curing accelerator, for example, imidazole compounds, tertiary amine / quaternary ammonium compounds, dimethyl urea compounds, organic phosphine compounds, etc. may be cited.
[0086] As for the imidazole compound used as the curing agent and / or curing accelerator in the present invention, for example, 1H-imidazole, 2-methylimidazole, 2-phenyl-4-methylimidazole, 2-ethyl-4-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-undecylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-undecylimidazole, 2,4-diamino-6-(2'-undecylimidazolyl-(1'))-ethyl-s-triazine, 2-phenyl-4,5-bis((2'-undecylimidazolyl)-triazine) and 2,4-diamino-6-(2'-undecylimidazolyl-(1'))-ethyl-s-triazine are mentioned. hydroxymethyl) imidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 2-phenylimidazole, 2-dodecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,4-diamino-6-(2'-methylimidazolyl-(1')-ethyl-s-triazine, 2,4-diamino-6-(2'-methylimidazolyl-(1'))-ethyl-s-triazine isocyanuric acid adduct, etc. Specific examples of imidazole compounds include Curezol 2MZ, 2P4MZ, 2E4MZ, 2E4MZ-CN, C11Z, C11Z-CN, C11Z-CNS, C11Z-A, 2PHZ, 1B2MZ, 1B2PZ, 2PZ, C17Z, 1.2DMZ, 2P4MHZ-PW, 2MZ-A, 2MA-OK (all manufactured by Shikoku Chemical Industry Co., Ltd.), etc.
[0087] The tertiary amine / quaternary ammonium compound used as the curing agent and / or curing accelerator in the present invention is not particularly limited, and examples thereof include quaternary ammonium salts such as tetramethylammonium bromide and tetrabutylammonium bromide; diazabicyclic compounds such as DBU (1,8-diazabicyclo[5.4.0]undecene-7), DBN (1,5-diazabicyclo[4.3.0]nonene-5), DBU-phenolate, DBU-octanoate, DBU-p-toluenesulfonate, DBU-formate, and DBU-phenol novolac resin salts; tertiary amines such as benzyldimethylamine, 2-(dimethylaminomethyl)phenol, and 2,4,6-tris(dimethylaminomethyl)phenol (TAP) and salts thereof, and dimethyl urea compounds such as aromatic dimethyl urea and aliphatic dimethyl urea.
[0088] The primary / secondary amine compounds used as the curing agent in the present invention include, for example, aliphatic amines such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, trimethylhexamethylenediamine, 2-methylpentamethylenediamine, 1,3-bisaminomethylcyclohexane, dipropylenediamine, diethylaminopropylamine, bis(4-aminocyclohexyl)methane, norbornene diamine, and 1,2-diaminocyclohexane; alicyclic amines such as N-aminoethylpiperazine and 1,4-bis(3-aminopropyl)piperazine; and aromatic amines such as diaminodiphenylmethane, m-phenylenediamine, meta-phenylenediamine, meta-phenylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone, and diethyltoluenediamine. Specific examples of the primary / secondary amine compounds include KAYAHARDA-A (manufactured by Nippon Kayaku Co., Ltd.: 4,4′-diamino-3,3′-dimethyldiphenylmethane) and the like.
[0089] Specific examples of the dimethyl urea compound as the curing agent and / or curing accelerator in the present invention include: DCMU (3-(3,4-dichlorophenyl)-1,1-dimethylurea), aromatic dimethyl urea such as U-CAT3512T (manufactured by San-Apro Co., Ltd.), aliphatic dimethyl urea such as U-CAT3503N (manufactured by San-Apro Co., Ltd.), etc. Among them, aromatic dimethyl urea is preferably used from the viewpoint of curability.
[0090] As for the organic phosphine compound used as the curing agent and / or curing accelerator in the present invention, for example, triphenylphosphine, tetraphenylphosphonium tetra-p-tolyl borate, tetraphenylphosphonium tetraphenyl borate, tri-tert-butylphosphonium tetraphenyl borate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, triphenylphosphine triphenylborane, etc. Specific examples of the organic phosphine compound include TPP, TPP-MK, TPP-K, TTBuP-K, TPP-SCN, TPP-S (manufactured by Hokuko Chemical Industry Co., Ltd.), etc.
[0091] The total of the content of the curing agent and curing accelerator in the resin composition is not particularly limited. From the viewpoint of preventing the transparency of the sealing layer (resin composition layer) from decreasing, relative to 100% by mass of the non-volatile component of the resin composition, it is preferably less than 5% by mass, and more preferably less than 1% by mass. On the other hand, from the viewpoint of suppressing the viscosity of the sealing layer, relative to 100% by mass of the non-volatile component of the resin composition, the total of the content is preferably more than 0.0005% by mass, and more preferably more than 0.001% by mass.
[0092] The content of the curing accelerator in the resin composition is not particularly limited. From the viewpoint of preventing the transparency of the sealing layer (resin composition layer) from decreasing, relative to 100% by mass of the non-volatile component of the resin composition, it is preferably below 5% by mass, and more preferably below 1% by mass. On the other hand, from the viewpoint of suppressing the viscosity of the sealing layer, relative to 100% by mass of the non-volatile component of the resin composition, the content is preferably above 0.0005% by mass, and more preferably above 0.001% by mass.
[0093] <Plasticizer>
[0094] The resin composition of the present invention may further contain a plasticizer. By using a plasticizer, the softness and formability of the resin composition can be improved. As a plasticizer, there is no particular limitation, but a material that is liquid at room temperature is preferred. As specific examples of plasticizers, there can be cited: mineral oils such as paraffin processing oils, cycloparaffin processing oils, liquid paraffin, polyethylene wax, polypropylene wax, vaseline, etc., castor oil, cottonseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, olive oil and other vegetable oils, liquid polybutene, hydrogenated liquid polybutene, liquid polybutadiene, hydrogenated liquid polybutadiene and other liquid polyalphaolefins, etc. As a plasticizer used in the present invention, liquid polyalphaolefins are preferred, and liquid polybutadiene is particularly preferred. In addition, as a liquid polyalphaolefin, from the viewpoint of adhesion, a liquid polyalphaolefin with a low molecular weight is preferred, preferably those in the range of 500 to 5000, and more preferably 1000 to 3000 in terms of weight average molecular weight. These plasticizers can be used alone or in combination. Here, "liquid" refers to the state of the plasticizer at room temperature (25°C). When using a plasticizer, from the viewpoint of not causing adverse effects on electronic devices, relative to 100% by mass of the non-volatile component of the resin combination, its content is preferably less than 50% by mass.
[0095] <Other ingredients>
[0096] The resin composition of the present invention may contain any components other than the above components to the extent that the effects of the present invention are not impaired. Such components include, for example, resins other than the above-mentioned polyolefin resins (e.g., epoxy resins, polyurethane resins, acrylic resins, polyamide resins, etc.), thickeners such as Orben and Benton, silicone-based, fluorine-based, and polymer-based defoamers or leveling agents, and adhesion-imparting agents such as triazole compounds, thiazole compounds, triazine compounds, and porphyrin compounds.
[0097] <Method for producing resin composition>
[0098] The method for producing the resin composition of the present invention is not particularly limited as long as the water content thereof can be sufficiently reduced. For example, a resin composition having a reduced water content can be produced by mixing the components with a solvent as required and drying the resulting compound.
[0099] It is relatively simple to dry the mixture by heating. Heating can be performed under normal pressure or under reduced pressure. The heating temperature and heating time may vary depending on the ingredients used. The heating temperature and heating time for sufficiently reducing the moisture content can be appropriately set by those skilled in the art according to the ingredients used.
[0100] <Resin sheet and method for producing the same>
[0101] The present invention also provides a resin sheet comprising a support and a layer of the resin composition of the present invention provided on the support (hereinafter also simply referred to as a "resin composition layer").
[0102] The resin composition layer of the resin sheet can be formed by a method known to those skilled in the art. For example, it can be formed by preparing a varnish obtained by dissolving the above-mentioned components in an organic solvent, applying the varnish on a support and drying. The non-volatile component of the varnish is preferably 20 to 80% by mass, more preferably 30 to 70% by mass.
[0103] Examples of the organic solvent include ketones such as acetone, methyl ethyl ketone (MEK), and cyclohexanone; acetates such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate; cellosolves such as cellosolve, and carbitols such as butyl carbitol; aromatic hydrocarbons such as toluene and xylene; dimethylformamide, dimethylacetamide, and N-methylpyrrolidone. The organic solvent may be used alone or in combination of two or more.
[0104] For drying of the varnish, it is relatively simple to carry out by heating. Heating can be carried out under normal pressure or under reduced pressure. The heating temperature and heating time may vary according to the components and organic solvents used. Regarding the heating temperature and heating time for fully reducing the moisture content, those skilled in the art may appropriately set them according to the components and organic solvents used. In addition, the preferred conditions for making the moisture content of the resin composition layer below 2500ppm are as described above.
[0105] When a resin sheet is prepared using a resin composition comprising a polyolefin resin having an acid anhydride group and a polyolefin resin having an epoxy group, the acid anhydride group and the epoxy group are reacted to form a cross-linked structure in advance, thereby improving the moisture permeation resistance of the layer of the resin composition, and obtaining a resin sheet with higher sealing performance (barrier performance to moisture and oxygen in the air, etc.).
[0106] The thickness of the resin composition layer in the resin sheet is preferably from 1 to 1000 μm, more preferably from 2 to 800 μm.
[0107] Examples of the support for the resin sheet include polyolefins such as polyethylene, polypropylene, and polyvinyl chloride, cycloolefin polymers, polyesters such as polyethylene terephthalate (hereinafter sometimes referred to as "PET") and polyethylene naphthalate, polycarbonate, and plastic films of polyimide. The surface of the support that is bonded to the resin composition layer may be subjected to a release treatment. Examples of the release treatment include release treatment using a release agent such as a silicone resin release agent, an alkyd resin release agent, and a fluororesin release agent.
[0108] The thickness of the support is not particularly limited, but is preferably from 10 to 150 μm, more preferably from 20 to 100 μm, from the viewpoint of the handleability of the resin sheet.
[0109] As a support for the resin sheet, a support having a barrier layer (for example, a plastic film having a barrier layer) is preferred. Examples of the barrier layer include inorganic films such as silicon dioxide vapor-deposited films, silicon nitride films, and silicon oxide films. The barrier layer may be composed of a plurality of inorganic films (for example, silicon dioxide vapor-deposited films). In addition, the barrier layer may be composed of an organic substance and an inorganic substance, or may be a composite multilayer of an organic layer and an inorganic film.
[0110] As the support having a barrier layer, for example, a support having a water vapor transmission rate (WVTR) of 0.0005 (g / m 2 / 24hr) or less high barrier plastic film. As a high barrier plastic film, for example, a material made of an inorganic film such as silicon oxide (silicon dioxide), aluminum oxide, magnesium oxide, silicon nitride, silicon oxynitride, SiCN, amorphous silicon, etc., stacked in a single layer or multiple layers by chemical vapor deposition (for example, chemical vapor deposition based on heat, plasma, ultraviolet light, vacuum heat, vacuum plasma or vacuum ultraviolet light) or physical vapor deposition (for example, vacuum evaporation, sputtering, ion plating, laser deposition, molecular beam epitaxy) on the surface of the plastic film (refer to, for example, Japanese Patent Publication No. 2016-185705, Japanese Patent Publication No. 5719106, Japanese Patent Publication No. 5712509, Japanese Patent Publication No. 5292358, etc.). In order to prevent cracks in the inorganic film, it is better to alternately stack an inorganic film and a transparent planarization layer (for example, a transparent plastic layer).
[0111] In addition, as a support having a barrier layer, for example, a support having a WVTR of 0.01 (g / m 2 / 24hr) or more and 1(g / m 2 / 24hr) or less. Examples of the medium barrier plastic film include materials produced by, for example, the following methods: a method of vapor-depositing an inorganic film containing inorganic materials such as silicon oxide (silicon dioxide), aluminum oxide, magnesium oxide, silicon nitride, silicon oxynitride, SiCN, and amorphous silicon on the surface of a substrate as a barrier layer, or a method of applying a coating liquid composed of a metal oxide and an organic resin having barrier properties to a substrate and drying the coating liquid, etc. (see, for example, Japanese Patent Publication No. 2013-108103 and Japanese Patent Publication No. 4028353).
[0112] The water vapor transmission rate can be measured as follows. First, a test piece of 60 mm φ is punched out from a plastic film having a barrier layer. According to JIS Z 0208:1976, the water vapor transmission rate is measured at a transmission area of 2.826×10 -3 m 2 7.5 g of calcium chloride was weighed into an aluminum moisture permeable cup (60 mm φ), and a test piece was installed in the moisture permeable cup. Calcium chloride was placed, and the initial mass of the moisture permeable cup with the test piece installed was measured with a precision balance. Next, the above-mentioned moisture permeable cup was left to stand for 24 hours in a constant temperature test room at a temperature of 40°C and a humidity of 90% RH, and calcium chloride was placed in it. The mass of the moisture permeable cup with the test piece installed after moisture permeation was measured with a precision balance. The mass increase (= mass after moisture permeation - initial mass) was taken as the amount of water vapor permeation, and the water vapor permeability (g / m 2 / 24hr).
[0113] As a support having a barrier layer, a commercially available product can be used. Commercially available products of medium barrier plastic films include, for example, "KURARISTER CI" manufactured by Kuraray Co., Ltd., "TECHBARRIER HX", "TECHBARRIER LX" and "TECHBARRIER L" manufactured by Mitsubishi Plastics Co., Ltd., "IB-PET-PXB" manufactured by Dai Nippon Printing Co., Ltd., and "GL, GX Series" manufactured by Toppan Printing Co., Ltd.; commercially available products of high barrier plastic films include, for example, "X-BARRIER" manufactured by Mitsubishi Plastics Co., Ltd.
[0114] It is preferred that the resin composition layer disposed on the support is protected in advance with a protective film. The lamination of the protective film on the resin composition layer can be carried out using known equipment. As equipment for laminating the protective film, for example, a roll laminator, a pressurizing machine, a vacuum pressurizing laminator, etc. can be cited.
[0115] As the protective film, the above-mentioned plastic film etc. can be mentioned. The surface of the protective film bonded with the resin composition layer is preferably subjected to a demoulding treatment. As the demoulding treatment, for example, a demoulding treatment using a demoulding agent such as a silicone resin demoulding agent, an alkyd resin demoulding agent, or a fluororesin demoulding agent can be mentioned.
[0116] The thickness of the protective film is not particularly limited, but is preferably from 10 to 150 μm, more preferably from 20 to 100 μm, from the viewpoint of the handleability of the resin sheet.
[0117] In order to suppress the resin composition layer from absorbing moisture after drying, the protective film preferably uses a protective film having a barrier layer. As the protective film having a barrier layer, the above-mentioned plastic film having a barrier layer can be cited. From the viewpoint of cost, the plastic film having a barrier layer used for the protective film preferably uses the above-mentioned medium barrier plastic film.
[0118] <Application>
[0119] The resin composition and resin sheet of the present invention can be used for sealing electronic devices. The electronic device is preferably an electronic device with weak water tolerance such as an organic EL device or a solar cell. That is, the resin composition and resin sheet of the present invention can be suitably used for sealing electronic devices with weak water tolerance such as an organic EL device or a solar cell.
[0120] Example
[0121] Hereinafter, the present invention will be described in more detail with reference to the following examples, but the present invention is not limited to the following examples and can be implemented by appropriately adding changes within the scope of the gist of the context, and all of these are included in the technical scope of the present invention. It should be noted that, unless otherwise specified, the "parts" and "%" in the amount of the component and the amount of the copolymerization unit refer to "parts by mass" and "% by mass", respectively.
[0122] <Ingredients>
[0123] The components used in the Examples and Comparative Examples are as follows;
[0124] (Polyolefin resin)
[0125] "HV-1900" (manufactured by JXTG Energy Corporation): polybutene, number average molecular weight 2900
[0126] “HV-300M” (manufactured by Toho Chemical Industry Co., Ltd.): maleic anhydride-modified liquid polybutene, anhydride group concentration 0.77 mmol / g, number average molecular weight 2100
[0127] "T-YP341" (produced by Seiko PMC Co., Ltd.): glycidyl methacrylate-modified propylene-butene random copolymer, propylene unit / butene unit 71% / 29%, epoxy group concentration 0.638 mmol / g, number average molecular weight 155,000
[0128] (Semi-calcined hydrotalcite)
[0129] “DHT-4C” (manufactured by Kyowa Chemical Industry Co., Ltd.): semi-calcined hydrotalcite, average particle size 400 nm, BET specific surface area 15 m 2 / g
[0130] (Adhesiveness Imparting Agent)
[0131] "ARKON P125" (produced by Arakawa Chemical Co., Ltd.): saturated hydrocarbon resin containing cyclohexane rings, softening point 125°C
[0132] (Curing accelerator)
[0133] 2,4,6-Tris(dimethylaminomethyl)phenol (hereinafter abbreviated as "TAP") (manufactured by Kayaku Akzo Co., Ltd.): a curing accelerator.
[0134] <Example 1>
[0135] According to the following steps, a varnish of the proportion shown in the following table is made, and the obtained varnish is used to make a resin sheet. It should be noted that the usage (part) of each component recorded in the following table represents the amount of the non-volatile components of each component in the varnish. In addition, the following table represents the content of 100% by mass of the non-volatile components of the semi-calcined hydrotalcite used as the semi-calcined hydrotalcite relative to the resin composition.
[0136] Specifically, maleic anhydride-modified liquid polybutene (HV-300M, manufactured by Toho Chemical Industry Co., Ltd.), polybutene (HV-1900, manufactured by JXTG Energy Co., Ltd.), and semi-calcined hydrotalcite (DHT-4C, manufactured by Kyowa Chemical Industry Co., Ltd.) were dispersed in a Swasol solution (non-volatile matter 60%) of a cyclohexane ring-containing saturated hydrocarbon resin (adhesive imparting agent, ARKON P125, manufactured by Arakawa Chemical Co., Ltd.) using a triple roll mill to obtain a mixture. To the obtained mixture, a Swasol solution (non-volatile content 20%) of a glycidyl methacrylate-modified propylene-butene random copolymer (T-YP341, manufactured by Seiko PMC Co., Ltd.), a curing accelerator (TAP, manufactured by Kayaku Akzo Corporation) and toluene were added, and the obtained mixture was uniformly dispersed using a high-speed rotary mixer to obtain a varnish of a resin composition. The obtained varnish was uniformly applied to a release-treated surface of a polyethylene terephthalate (PET) film "SP4020" (PET: 50 μm, manufactured by TOYO CLOTH Co., Ltd.) treated with a silicone-based release agent using a die coater, and heated at 130°C for 30 minutes and then at 160°C for 30 minutes to obtain a resin sheet having a resin composition layer with a thickness of 25 μm.
[0137] <Example 2>
[0138] A resin composition varnish and a resin sheet having a 25 μm thick resin composition layer were prepared in the same manner as in Example 1 except that the amount of semi-calcined hydrotalcite (DHT-4C, manufactured by Kyowa Chemical Industry Co., Ltd.) used was changed from 300 parts to 250 parts.
[0139] <Example 3>
[0140] A resin composition varnish and a resin sheet having a 25 μm thick resin composition layer were prepared in the same manner as in Example 1 except that the amount of semi-calcined hydrotalcite (DHT-4C, manufactured by Kyowa Chemical Industry Co., Ltd.) used was changed from 300 parts to 200 parts.
[0141] <Example 4>
[0142] A resin composition varnish and a resin sheet having a 25 μm thick resin composition layer were prepared in the same manner as in Example 1 except that the amount of semi-calcined hydrotalcite (DHT-4C, manufactured by Kyowa Chemical Industry Co., Ltd.) used was changed from 300 parts to 100 parts.
[0143] <Comparative Example 1>
[0144] According to the following steps, the varnish of the proportion shown in the following table is made, and the obtained varnish is used to make a resin sheet. It should be noted that the usage (part) of each component recorded in the following table represents the amount of the non-volatile component of each component in the varnish. In addition, the content of 100% by mass of the non-volatile component of the semi-calcined hydrotalcite relative to the resin composition is represented in the following table.
[0145] Specifically, maleic anhydride-modified liquid polybutene (HV-300M, manufactured by Toho Chemical Industry Co., Ltd.), polybutene (HV-1900, manufactured by JXTG Energy Co., Ltd.), and semi-calcined hydrotalcite (DHT-4C, manufactured by Kyowa Chemical Industry Co., Ltd.) were dispersed in a Swasol solution (non-volatile content 60%) of a saturated hydrocarbon resin containing a cyclohexane ring (adhesive agent, ARKON P125, manufactured by Arakawa Chemical Co., Ltd.) using a three-roll mill to obtain a mixture. A Swasol solution (non-volatile content 20%) of a glycidyl methacrylate-modified propylene-butene random copolymer (T-YP341, manufactured by Seiko PMC Co., Ltd.), a curing accelerator (TAP, manufactured by Kayaku Akzo Corporation), and toluene were added to the obtained mixture, and the obtained mixture was uniformly dispersed using a high-speed rotary mixer to obtain a varnish of a resin composition. The obtained varnish was evenly applied on the release-treated surface of a PET film "SP4020" (PET: 50 μm, manufactured by TOYO CLOTH Co., Ltd.) treated with a silicone-based release agent using a die coater, and heated at 130°C for 30 minutes and then at 160°C for 15 minutes to obtain a resin sheet having a resin composition layer with a thickness of 25 μm.
[0146] <Comparative Example 2>
[0147] A varnish of the resin composition was prepared in the same manner as in Example 1, and the varnish was evenly applied using a die coater onto the release-treated surface of a PET film "SP4020" (PET: 50 μm, manufactured by TOYO CLOTH Co., Ltd.) treated with a silicone-based release agent, and heated at 130° C. for 30 minutes to obtain a resin sheet having a resin composition layer with a thickness of 25 μm.
[0148] <Comparative Example 3>
[0149] A varnish of the resin composition was prepared by the same method as in Example 4, and the varnish was evenly applied on the release-treated surface of a PET film "SP4020" (PET: 50 μm, manufactured by TOYO CLOTH Co., Ltd.) treated with a silicone release agent using a die coater, and heated at 130°C for 60 minutes to obtain a resin sheet having a resin composition layer with a thickness of 25 μm.
[0150] <Comparative Example 4>
[0151] A resin sheet having a resin composition layer with a thickness of 25 μm was prepared in the same manner as in Comparative Example 3 except that the varnish was prepared in the formulation of Comparative Example 4 shown in Table 1 below.
[0152] The resin composition layer of each resin sheet obtained in the examples and comparative examples was evaluated for transparency by total light transmittance, for moisture permeation resistance (sealing performance) by average molecular penetration distance, and for suppression of degradation of the sealed portion due to internal moisture (sealing performance) by reflectance ratio.
[0153] <Water content of resin composition layer>
[0154] The resin sheets prepared in the examples and comparative examples were cut into a length of 70 mm and a width of 40 mm, the support (i.e., a PET film "SP4020" treated with a silicone release agent) was peeled off, and the resin composition layer was folded and placed in a fully dried screw vial (screw vial container) (VABH17, manufactured by Mitsubishi Chemical Analytical Tech Co., Ltd.), and placed in an electric furnace (VA-236S type, manufactured by Mitsubishi Chemical Analytical Tech Co., Ltd.) directly connected to a Karl Fischer measuring instrument (CA-310 type, manufactured by Mitsubishi Chemical Analytical Tech Co., Ltd.). In a N2 gas flow, the temperature of the electric furnace was raised to 250°C, and the water escaping from the measured sample was captured in a Karl Fischer measuring solution, and the mass of the water was measured by a conventional method. Based on the mass of the measured water, the water content (ppm) of the resin composition layer was calculated relative to the mass of the entire resin composition. The results are shown in the following table.
[0155] <Total light transmittance>
[0156] The resin sheets prepared in the examples and comparative examples were cut into a length of 50 mm and a width of 20 mm, and the cut resin sheets were laminated on a glass plate (a microscope slide having a length of 76 mm, a width of 26 mm, and a thickness of 1.2 mm, a white slide glass S1112 edge grinding No. 2 manufactured by Matsunami Glass Industries, Ltd.) using a batch vacuum laminator (manufactured by Nichigo-Morton Co., Ltd., V-160) in such a manner that the resin composition layer was in contact with the glass plate. The lamination conditions were a temperature of 80° C., a decompression time of 30 seconds, and then a pressure of 0.3 MPa for 30 seconds. Then, the PET film of the resin sheet was peeled off, and the transmittance spectrum of the exposed resin composition layer was measured using a fiber optic spectrophotometer (MCPD-7700, Model 311C, manufactured by Otsuka Electronics Co., Ltd., external light source unit: halogen lamp MC-2564 (24V, 150W specification)) equipped with a φ60mm integrating sphere (Model SRS-99-010, reflectivity 99%), and the total light transmittance (%) at a wavelength of 450nm was calculated and evaluated according to the following criteria. The results are shown in the table below. It should be noted that the distance between the integrating sphere and the sample (laminated body) was set to 0mm, and glass was used as a reference;
[0157] Good (○): Total light transmittance is 90% or more
[0158] Defective (×): The total light transmittance is less than 90%.
[0159] <Average water penetration distance>
[0160] An alkali-free glass with a side length of 50 mm × 50 mm was cleaned with boiling isopropyl alcohol for 5 minutes and dried at 150°C for more than 30 minutes. Next, the alkali-free glass was cleaned with UV ozone. A calcium film (purity 99.8%) (thickness 200 nm) was deposited on the cleaned alkali-free glass using a mask with a distance of 2 mm from the end.
[0161] An aluminum foil / PET composite film "AL1N30 with PET" (aluminum foil: 30 μm, PET: 25 μm, manufactured by Tokai Toyo Aluminum Sales Co., Ltd.) was used as a support. Other operations were performed in the same manner as in the embodiments and comparative examples to obtain a resin sheet having a laminated structure of PET / aluminum foil / resin composition layers having the same resin composition layers as in the embodiments and comparative examples.
[0162] In a glove box, the alkali-free glass on which the calcium film was deposited and the resin sheet were laminated using a heat laminator (Lamipacker DAiSY A4 (LPD2325) manufactured by Fuji Prole Co., Ltd.) so that the calcium film was in contact with the resin composition layer to obtain a sample for evaluation.
[0163] When calcium contacts water and forms calcium oxide, it becomes transparent. Therefore, the penetration of water into the evaluation sample can be evaluated by measuring the distance (mm) from the end of the evaluation sample to the calcium film.
[0164] The distance from the edge of the evaluation sample obtained as described above to the calcium film was measured at 8 locations using a measuring microscope (MF-U) manufactured by Mitutoyo Corporation, and the average value thereof was defined as X2.
[0165] Next, the evaluation sample was placed in a constant temperature and humidity chamber set at 85°C and 85%RH. The distance from the end of the evaluation sample to the calcium film was measured at 8 locations after 40 hours in the constant temperature and humidity chamber, and the average value was defined as X1 (mm).
[0166] The average water penetration distance X (= X1-X2) into the calcium film after being placed in a constant temperature and humidity chamber was calculated based on the obtained X1 and X2, and the moisture permeability resistance of the resin composition layer under high temperature and high humidity was evaluated according to the following criteria. The higher the moisture permeability resistance, the more the water penetration rate can be slowed down, and the smaller the value of the average water penetration distance X. The results are shown in the following table. It should be noted that when X is less than 0.1 mm, it is recorded as "<0.1" in the following table. In addition, for Comparative Examples 3 and 4 (where X1 could not be measured due to the degradation of the calcium film caused by moisture), the results were evaluated as poor (×);
[0167] Good (○): X less than 1mm
[0168] Bad (×): X is 1 mm or more, or X1 cannot be measured due to degradation of the calcium film caused by moisture.
[0169] <Reflectivity ratio>
[0170] An alkali-free glass with a side length of 50 mm × 50 mm was cleaned with boiling isopropyl alcohol for 5 minutes and dried at 150°C for more than 30 minutes. Next, the alkali-free glass was cleaned with UV ozone. A calcium film (purity 99.8%) (thickness 200 nm) was deposited on the cleaned alkali-free glass using a mask with a distance of 2 mm from the end.
[0171] An aluminum foil / PET composite film "AL1N30 with PET" (aluminum foil: 30 μm, PET: 25 μm, manufactured by Tokai Toyo Aluminum Sales Co., Ltd.) was used as a support. Except for this, the same operation as in the embodiments and comparative examples was performed to obtain a resin sheet having a laminated structure of PET / aluminum foil / resin composition layer having the same resin composition layer as in the embodiments and comparative examples.
[0172] In a glove box, the alkali-free glass on which the calcium film was deposited and the resin sheet were laminated using a heat laminator (Lamipacker DAiSY A4 (LPD2325) manufactured by Fuji Prole Co., Ltd.) so that the calcium film was in contact with the resin composition layer to obtain a sample for evaluation.
[0173] The reflectance spectrum of the evaluation sample obtained above was measured using a fiber optic spectrophotometer (MCPD-7700, Model 311C, manufactured by Otsuka Electronics Co., Ltd., external light source unit: halogen lamp MC-2564 (24V, 150W specification)) equipped with a φ60mm integrating sphere (Model SRS-99-010, reflectance 99%), and the reflectance (%) at a wavelength of 850nm was calculated, and this value was set to Y2.
[0174] Next, the evaluation sample was heated for 39 hours using a hot plate at a temperature of 80° C. in a glove box, and then the reflectance spectrum of the heated evaluation sample was measured, and the value was defined as Y1.
[0175] The reflectance ratio Y (=Y1 / Y2) was calculated from the obtained Y1 and Y2, and the inhibition of calcium film degradation caused by moisture contained in the semi-calcined hydrotalcite of the resin composition layer was evaluated according to the following criteria. The results are shown in the following table. At this time, for Comparative Examples 1 to 4 (where the reflectance spectrum Y1 could not be measured due to calcium film degradation caused by moisture), the results were evaluated as poor (×);
[0176] Good (○): Reflectance ratio Y is 0.90 or more
[0177] Pass (△): Reflectivity ratio Y is less than 0.90
[0178] Bad (×): The reflectance spectrum Y1 could not be measured due to degradation of the calcium film caused by moisture.
[0179] [Table 1]
[0180]
[0181] Possibility of industrial application
[0182] The resin composition of the present invention and a resin sheet using the same can be used for sealing electronic devices (for example, organic EL devices, sensor devices, solar cells, etc.).
[0183] This application is based on Japanese Patent Application No. 2019-180606 filed in Japan, the entire contents of which are incorporated herein by reference.
Claims
1. A resin composition, wherein Contains a polyolefin resin, semi-calcined hydrotalcite and an adhesiveness-imparting agent, The content of the polyolefin resin is 5% by mass or more and 50% by mass or less relative to 100% by mass of the nonvolatile components of the resin composition, The content of the semi-calcined hydrotalcite is more than 45% by mass and less than 80% by mass relative to 100% by mass of the non-volatile components of the resin composition, The content of the adhesion-imparting agent is 5% by mass or more and 50% by mass or less relative to 100% by mass of the nonvolatile components of the resin composition, Furthermore, the resin composition containing the semi-calcined hydrotalcite is dried by heating, and the water content of the resin composition is 2500 ppm or less based on the mass of the entire resin composition.
2. The resin composition according to claim 1, wherein The water content is 2000 ppm or less based on the mass of the entire resin composition.
3. The resin composition according to claim 2, wherein The water content is 1500 ppm or less based on the mass of the entire resin composition.
4. The resin composition according to claim 1 or 2, wherein The content of the semi-calcined hydrotalcite is 50% by mass or more and 75% by mass or less relative to 100% by mass of the nonvolatile components of the resin composition. The resin composition according to claim 1 or 2, which is used for sealing electronic devices.
6. The resin composition according to claim 5, wherein The electronic device is an organic EL device or a solar cell. 7 . A resin sheet comprising: a support, and a layer of the resin composition according to claim 1 or 2 provided on the support. The resin sheet according to claim 7 , which is used for sealing electronic devices.
9. The resin sheet according to claim 8, wherein The electronic device is an organic EL device or a solar cell.
Citation Information
Patent Citations
Method for producing gas barrier film
JP2013108103A
Gas barrier film
JP2016185705A
Resin composition
WO2011062167A1
Resin composition for sealing
WO2013108731A1
Resin composition for sealing
WO2017057708A1