A spindle lubricating coating

By forming a multi-layer structure of graphene, composite coating and parylene coating on the vascular stent mandrel, the problems of poor biocompatibility and lubrication effect are solved, and the service life and stability of the mandrel are improved.

CN114522001BActive Publication Date: 2024-11-22上海派拉纶新材料股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210159996.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-22
Publication Date
2024-11-22
Estimated Expiration
2042-02-22

AI Technical Summary

Technical Problem

The vascular stent mandrel is poor in biocompatibility, poor lubrication effect and wear resistance during use, resulting in a short service life.

Method used

The mandrel lubricating coating is used, consisting of an inner surface layer, a composite coating and a protective layer. The inner surface layer is a graphene layer. The composite coating contains epoxy acrylate, nanographite and molybdenum disulfide. The protective layer is a parylene coating. Chemical vapor deposition method and spraying technology are formed to enhance lubricating performance and biocompatibility.

Benefits of technology

It significantly improves the lubricating performance and biocompatibility of the mandrel surface, reduces friction resistance, extends the service life of the vascular stent, and ensures the stable operation of the mandrel in harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114522001B_ABST
    Figure CN114522001B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of paralon materials, and in particular to a spindle lubricating coating, comprising a spindle substrate and a lubricating coating body, wherein the lubricating coating body is arranged on the outside of the spindle substrate, and the lubricating coating body comprises an inner surface layer, a reinforcing layer, a composite coating and a protective layer, wherein the inner surface layer is bonded to the surface of the spindle substrate, and the reinforcing layer is arranged on the outside of the inner surface layer. The spindle lubricating coating proposed by the present invention has the advantages of increasing the lubrication performance and biocompatibility of the spindle surface and reducing friction resistance, and solves the problems that the current vascular stent spindle has poor biocompatibility during use, and the lubrication effect and wear resistance of the spindle are poor, and the spindle is prone to wear during operation, resulting in a short service life of the spindle, and greatly improves the lubrication performance of the spindle lubricating coating, so that the spindle can work safely and stably, and ensures that the lubricating coating can meet the use requirements of the vascular stent spindle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of paralon materials, in particular to a spindle lubricating coating. Background Art

[0002] A vascular stent refers to a stent placed in the diseased segment on the basis of luminal balloon dilatation to support the narrowed and occluded segment of the blood vessel, reduce the elastic retraction and reshaping of the blood vessel, and maintain smooth blood flow in the lumen. Some stents also have the function of preventing restenosis. They are mainly divided into coronary stents, cerebrovascular stents, renal artery stents, aortic stents, etc.

[0003] Paralon is a new type of conformal coating material, a paraxylene polymer. It is chemically inert, insoluble in acids, alkalis and organic solvents, and resistant to hydrolysis and erosion. The thin film coating formed by this technology can cover the edges and gaps of silk fabrics. Its surface is hydrophobic, has poor permeability to water vapor and corrosive gases, has good thermal stability, and has good isolation and protection functions in harsh environments such as acid mist, mold, humidity, and corrosion.

[0004] At present, the biocompatibility of the mandrel of a vascular stent is poor during use, and the lubrication effect and wear resistance of the mandrel are poor. The mandrel is prone to wear during operation, resulting in a short service life of the mandrel. Therefore, a mandrel lubricating coating is proposed to increase the lubrication performance and biocompatibility of the mandrel surface, reduce friction resistance, and thus extend the service life of the vascular stent. Summary of the invention

[0005] The purpose of the present invention is to provide a spindle lubricating coating, which has the advantages of increasing the lubrication performance and biocompatibility of the spindle surface and reducing friction resistance, thereby solving the problems that the current vascular stent spindle has poor biocompatibility during use, and the lubrication effect and wear resistance of the spindle are poor, and the spindle is prone to wear during operation, resulting in a short service life of the spindle.

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: a spindle lubrication coating, comprising a spindle substrate and a lubrication coating body, wherein the lubrication coating body is arranged on the outside of the spindle substrate, the lubrication coating body comprises an inner surface layer, a composite coating and a protective layer, the inner surface layer is bonded to the surface of the spindle substrate, the composite coating is arranged on the outside of the inner surface layer, and the protective layer is located on the outside of the composite coating.

[0007] Preferably, the mandrel substrate is made of nickel-titanium alloy or cobalt-chromium alloy, and the surface roughness Ra value of the mandrel substrate is 0.16-1.5 μm.

[0008] Preferably, the inner surface layer is a graphene layer, and the thickness of the inner surface layer is 0.2 to 5 μm.

[0009] Preferably, the composite coating has a thickness of 0.2 to 8 μm.

[0010] Preferably, the protective layer is made of parylene coating material, and the deposition thickness of the protective layer is 0.2-10 μm.

[0011] Preferably, the protective layer is coated on the outside of the composite coating by vacuum vapor deposition technology.

[0012] A method for preparing a spindle lubricating coating comprises the following steps:

[0013] Step 1: First, the mandrel product is placed inside the deposition chamber, and a carbon-containing organic gas is used as a raw material to deposit a graphene film on the outer surface of the mandrel by chemical vapor deposition;

[0014] Step 2: Weigh epoxy acrylate, nanographite, molybdenum disulfide, suspension dispersant, and curing agent respectively, put the raw materials into a mixing reactor, and use high-speed dispersion to mix the raw materials evenly to form a composite coating, and then spray it on the outer side of the mandrel product to obtain a composite coating;

[0015] Step 3: Select a parylene raw material and put it into the evaporation chamber. After the evaporation is completed, introduce the gaseous parylene raw material into the cracking chamber. After the gaseous parylene raw material is cracked into reactive monomers, the gaseous monomers are introduced into the deposition chamber to deposit and polymerize the gaseous monomers on the outside of the composite coating of the mandrel at room temperature to form a parylene coating, thereby obtaining a mandrel product with a lubricating coating.

[0016] Preferably, in step 1, the interior of the deposition chamber is in vacuum condition, and the temperature during deposition is controlled to be 1000-1100° C.

[0017] Preferably, in step 2, the spraying thickness of the composite coating is 0.2 to 8 μm. After spraying, the coating is cured at 50 to 60° C. for 2 to 4 hours, and then the temperature is lowered to room temperature for curing for 6 to 8 hours.

[0018] Preferably, in step three, the thickness of the parylene coating is 0.2-10 μm.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The spindle lubricating coating proposed in the present invention has the advantages of increasing the lubrication performance and biocompatibility of the spindle surface and reducing frictional resistance. It solves the problems that the current vascular stent spindle has poor biocompatibility during use, and the lubrication effect and wear resistance of the spindle are poor. The spindle is prone to wear during operation, which leads to a short service life of the spindle. The lubrication performance of the spindle lubricating coating is greatly improved, so that the spindle can work safely and stably, and it is ensured that the lubricating coating can meet the use requirements of the vascular stent spindle, thereby having a good use prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the structure of the present invention;

[0022] Figure 2 This is a cross-sectional view of the main structure of the lubricating coating of the present invention.

[0023] In the figure: 1, spindle substrate; 2, lubricating coating body; 201, inner surface layer; 202, composite coating; 203, protective layer. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Please refer to the attached Figure 1-2 A spindle lubrication coating comprises a spindle substrate 1 and a lubrication coating body 2, wherein the spindle substrate 1 is made of nickel-titanium alloy or cobalt-chromium alloy as raw material, and the surface roughness Ra value of the spindle substrate 1 is 0.16-1.5 μm, the lubrication coating body 2 is arranged on the outer side of the spindle substrate 1, the lubrication coating body 2 comprises an inner surface layer 201, a composite coating 202 and a protective layer 203, the inner surface layer 201 is bonded to the surface of the spindle substrate 1, the composite coating 202 is arranged on the outer side of the inner surface layer 201, the protective layer 203 is located on the outer side of the composite coating 202, the inner surface layer 201 is a graphene layer, the thickness of the inner surface layer 201 is 0.2-5 μm, the thickness of the composite coating 202 is 0.2-8 μm, the protective layer 203 is made of parylene coating material, and the deposition thickness of the protective layer 203 is 0.2-10 μm, and the protective layer 203 is coated on the outer side of the composite coating 202 by vacuum vapor deposition technology.

[0026] Embodiment 1:

[0027] A method for preparing a spindle lubricating coating comprises the following steps:

[0028] Step 1: First, place the mandrel product inside the deposition chamber, use carbon-containing organic gas as raw material, and deposit the graphene film on the outer surface of the mandrel by chemical vapor deposition. The deposition chamber is in vacuum condition, and the temperature during deposition is controlled at 1000°C, which can improve the coating uniformity of the graphene film and ensure the stability of the lubricating coating in actual use;

[0029] Step 2: Weigh epoxy acrylate, nanographite, molybdenum disulfide, suspension dispersant, and curing agent respectively, put the raw materials into a mixing reactor, and use high-speed dispersion to mix the raw materials evenly. After forming a composite coating, spray it on the outer side of the mandrel product to obtain a composite coating. The spraying thickness of the composite coating is 0.2 to 8 μm. After spraying, cure it at 50° C. for 2 hours, and then reduce it to room temperature for curing for 6 hours;

[0030] Furthermore, epoxy acrylate has good compatibility in the raw material system and can play a good synergistic role, thereby improving the corrosion resistance, hardness and thermal stability of the lubricating coating and broadening the use temperature range of the lubricating coating. Nanographite and molybdenum disulfide have a synergistic friction-reducing and lubricating effect and have a lasting stability of the lubricating effect. The suspending dispersant is conducive to the uniform dispersion of the mixture of nanographite and molybdenum disulfide, thereby ensuring the performance of the coating.

[0031] Step 3: Select a parylene raw material and put it into the evaporation chamber. After the evaporation is completed, introduce the gaseous parylene raw material into the cracking chamber. After the gaseous parylene raw material is cracked into reactive monomers, the gaseous monomers are introduced into the deposition chamber to deposit and polymerize the gaseous monomers on the outside of the composite coating of the mandrel at room temperature to form a parylene coating, thereby obtaining a mandrel product with a lubricating coating.

[0032] Furthermore, the parylene coating can improve the processing performance of the product, reduce the friction coefficient, and enhance the lubrication effect of the mandrel product surface.

[0033] Embodiment 2:

[0034] A method for preparing a spindle lubricating coating comprises the following steps:

[0035] Step 1: First, place the mandrel product inside the deposition chamber, use carbon-containing organic gas as raw material, and deposit the graphene film on the outer surface of the mandrel by chemical vapor deposition. The deposition chamber is in vacuum condition, and the temperature during deposition is controlled at 1050°C, which can improve the coating uniformity of the graphene film and ensure the stability of the lubricating coating in actual use;

[0036] Step 2: Weigh epoxy acrylate, nanographite, molybdenum disulfide, suspension dispersant, and curing agent respectively, put the raw materials into a mixing reactor, and use high-speed dispersion to mix the raw materials evenly. After forming a composite coating, spray it on the outer side of the mandrel product to obtain a composite coating. The spraying thickness of the composite coating is 0.2 to 8 μm. After spraying, cure at 55° C. for 3 hours, and then reduce to room temperature for curing for 7 hours;

[0037] Furthermore, epoxy acrylate has good compatibility in the raw material system and can play a good synergistic role, thereby improving the corrosion resistance, hardness and thermal stability of the lubricating coating and broadening the use temperature range of the lubricating coating. Nanographite and molybdenum disulfide have a synergistic friction-reducing and lubricating effect and have a lasting stability of the lubricating effect. The suspending dispersant is conducive to the uniform dispersion of the mixture of nanographite and molybdenum disulfide, thereby ensuring the performance of the coating.

[0038] Step 3: Select a parylene raw material and put it into the evaporation chamber. After the evaporation is completed, introduce the gaseous parylene raw material into the cracking chamber. After the gaseous parylene raw material is cracked into reactive monomers, the gaseous monomers are introduced into the deposition chamber to deposit and polymerize the gaseous monomers on the outside of the composite coating of the mandrel at room temperature to form a parylene coating, thereby obtaining a mandrel product with a lubricating coating.

[0039] Furthermore, the parylene coating can improve the processing performance of the product, reduce the friction coefficient, and enhance the lubrication effect of the mandrel product surface.

[0040] Embodiment three:

[0041] A method for preparing a spindle lubricating coating comprises the following steps:

[0042] Step 1: First, place the mandrel product inside the deposition chamber, use carbon-containing organic gas as raw material, and deposit the graphene film on the outer surface of the mandrel by chemical vapor deposition. The deposition chamber is in vacuum condition, and the temperature is controlled at 1100°C during deposition, which can improve the coating uniformity of the graphene film and ensure the stability of the lubricating coating in actual use;

[0043] Step 2: Weigh epoxy acrylate, nanographite, molybdenum disulfide, suspension dispersant, and curing agent respectively, put the raw materials into a mixing reactor, and use high-speed dispersion to mix the raw materials evenly. After forming a composite coating, spray it on the outer side of the mandrel product to obtain a composite coating. The spraying thickness of the composite coating is 0.2 to 8 μm. After spraying, cure at 60° C. for 4 hours, and then reduce to room temperature for curing for 8 hours;

[0044] Furthermore, epoxy acrylate has good compatibility in the raw material system and can play a good synergistic role, thereby improving the corrosion resistance, hardness and thermal stability of the lubricating coating and broadening the use temperature range of the lubricating coating. Nanographite and molybdenum disulfide have a synergistic friction-reducing and lubricating effect and have a lasting stability of the lubricating effect. The suspending dispersant is conducive to the uniform dispersion of the mixture of nanographite and molybdenum disulfide, thereby ensuring the performance of the coating.

[0045] Step 3: Select a parylene raw material and put it into the evaporation chamber. After the evaporation is completed, introduce the gaseous parylene raw material into the cracking chamber. After the gaseous parylene raw material is cracked into reactive monomers, the gaseous monomers are introduced into the deposition chamber to deposit and polymerize the gaseous monomers on the outside of the composite coating of the mandrel at room temperature to form a parylene coating, thereby obtaining a mandrel product with a lubricating coating.

[0046] Furthermore, the parylene coating can improve the processing performance of the product, reduce the friction coefficient, and enhance the lubrication effect of the mandrel product surface.

[0047] In summary, the spindle lubricating coating has the advantages of increasing the lubrication performance and biocompatibility of the spindle surface and reducing frictional resistance. It solves the problems that the current vascular stent spindle has poor biocompatibility during use, and the lubrication effect and wear resistance of the spindle are poor. The spindle is prone to wear during operation, which leads to a short service life of the spindle. The lubrication performance of the spindle lubricating coating is greatly improved, so that the spindle can work safely and stably, and it is ensured that the lubricating coating can meet the use requirements of the vascular stent spindle, thus having a good prospect for use.

[0048] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0049] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a spindle lubricating coating, characterized in that: The spindle lubricating coating comprises a spindle substrate (1) and a lubricating coating body (2), wherein the lubricating coating body (2) is arranged on the outside of the spindle substrate (1), the lubricating coating body (2) comprises an inner surface layer (201), a composite coating (202) and a protective layer (203), the inner surface layer (201) is bonded to the surface of the spindle substrate (1), the composite coating (202) is arranged on the outside of the inner surface layer (201), and the protective layer (203) is located on the outside of the composite coating (202); The method for preparing the spindle lubricating coating comprises the following steps: Step 1: First, the mandrel product is placed inside the deposition chamber, and a carbon-containing organic gas is used as a raw material to deposit a graphene film on the outer surface of the mandrel by chemical vapor deposition; Step 2: Weigh epoxy acrylate, nanographite, molybdenum disulfide, suspension dispersant, and curing agent respectively, put the raw materials into a mixing reactor, and use high-speed dispersion to mix the raw materials evenly to form a composite coating, and then spray it on the outer side of the mandrel product to obtain a composite coating; Step 3: Select a parylene raw material and put it into the evaporation chamber. After the evaporation is completed, introduce the gaseous parylene raw material into the cracking chamber. After the gaseous parylene raw material is cracked into reactive monomers, the gaseous monomers are introduced into the deposition chamber to deposit and polymerize the gaseous monomers on the outside of the composite coating of the mandrel at room temperature to form a parylene coating, thereby obtaining a mandrel product with a lubricating coating.

2. The method for preparing a spindle lubricating coating according to claim 1, characterized in that: In the step 1, the interior of the deposition chamber is in a vacuum condition, and the temperature during deposition is controlled to be 1000-1100° C.

3. The method for preparing a spindle lubricating coating according to claim 1, characterized in that: In the step 2, the spraying thickness of the composite coating is 0.2 to 8 μm. After spraying, the coating is cured at 50 to 60° C. for 2 to 4 hours, and then the temperature is lowered to room temperature for curing for 6 to 8 hours.

4. The method for preparing a spindle lubricating coating according to claim 1, characterized in that: In the step 3, the thickness of the parylene coating is 0.2-10 μm.

5. The method for preparing a spindle lubricating coating according to claim 1, characterized in that: The spindle substrate (1) uses nickel-titanium alloy or cobalt-chromium alloy as raw material, and the surface roughness Ra value of the spindle substrate (1) is 0.16 to 1.5 μm.

6. The method for preparing a spindle lubricating coating according to claim 1, characterized in that: The inner surface layer (201) is a graphene layer, and the thickness of the inner surface layer (201) is 0.2 to 5 μm.

7. The method for preparing a spindle lubricating coating according to claim 1, characterized in that: The composite coating (202) has a thickness of 0.2 to 8 μm.

8. The method for preparing a spindle lubricating coating according to claim 1, characterized in that: The protective layer (203) is made of parylene coating material, and the deposition thickness of the protective layer (203) is 0.2 to 10 μm.