A colored anti-slip floor suitable for sponge cities and its construction process
By setting up multi-layer structures and reasonable material ratios in the floor of sponge cities, the problem of slow seepage speed of existing floors is solved, rapid drainage and high strength are achieved, service life is extended, and floor is maintained aesthetics and mechanical properties.
Patent Information
- Application Number
- CN202210185922.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-02-28
AI Technical Summary
The existing permeable floors have slow seepage speed when rainfall is high, resulting in water accumulation, and increasing the seepage speed will damage the strength and life of the floor.
Using a colored anti-slip floor consisting of a permeable layer, a leveling layer, a stabilizing layer and a filter layer, the floor is improved by setting the first and second gravel steel slag layer and a cement concrete layer, combining appropriate void ratio and particle size ratio. The strength and drainage speed are used to remove solid particles through the geotextile filter layer to ensure rapid penetration of rainwater.
It realizes rapid drainage, large seepage and high strength of the floor, extends the service life, and ensures the beauty and mechanical properties of the floor.
Smart Images

Figure CN114525708B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of floor technology, and in particular to a colored anti-slip floor suitable for a sponge city and a construction process thereof. Background Art
[0002] Due to poor urban drainage, the phenomenon of seeing the sea in the city has frequently occurred in recent years, which has increasingly aroused people's attention to urban drainage issues. In addition, more and more cities are experiencing water shortages. Sponge city is a new generation of urban stormwater management concept, which means that the city has good "elasticity" in adapting to environmental changes and responding to natural disasters caused by rainwater. It can also be called a "water-elastic city". The internationally accepted term is "low-impact development rainwater system construction". When it rains, it absorbs water, stores water, infiltrates water, and purifies water. When needed, the stored water is "released" and used.
[0003] At present, some permeable floors can be used in cities with less rainfall, but when the rainfall is heavy, the infiltration speed of rainwater is slow, which will cause a lot of water accumulation. If the porosity of the floor is increased to increase the infiltration speed of rainwater, the strength of the floor will be reduced and the life span will be shortened. In view of this, the present invention provides a colored anti-slip floor suitable for sponge cities and its construction process to solve the problems raised in the above background technology. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a colored anti-slip floor suitable for sponge cities and a construction process thereof, the floor has a fast drainage speed, a large infiltration volume, high strength and a long service life.
[0005] In order to achieve the above-mentioned object, the present invention provides a colored anti-skid floor suitable for sponge cities, which comprises, from top to bottom, a permeable layer, a leveling layer, a stabilizing layer, a filter layer and a soil base layer, wherein the permeable layer comprises a wear-resistant layer, a coloring layer and an anti-skid layer arranged in sequence, and the stabilizing layer comprises, from top to bottom, a first cement concrete layer, a first crushed stone steel slag layer, a second cement concrete layer and a second crushed stone steel slag layer arranged in sequence, wherein the porosity of the first cement concrete layer is less than that of the second crushed stone steel slag layer, and the first crushed stone steel slag layer and the second crushed stone steel slag layer are both composed of crushed stone and steel slag;
[0006] The particle size of the crushed stone in the first crushed stone and steel slag layer is 15-30 mm, the particle size of the steel slag is 5-25 mm, and the content of the crushed stone is 60%-70%. The laying thickness of the first crushed stone and steel slag layer is 4-8 cm;
[0007] The particle size of the crushed stones in the second crushed stone and steel slag layer is 40-55 mm, the particle size of the steel slag is 30-50 mm, and the content of the crushed stones is 70%-80%. The laying thickness of the second crushed stone and steel slag layer is 7-11 cm.
[0008] By adopting the above scheme, the first crushed stone and steel slag layer and the second crushed stone and steel slag layer are used as the cushion layer. By selecting the appropriate particle size and reasonable ratio of crushed stone and steel slag, the force on the floor is evenly distributed and the strength of the floor is improved. The first cement concrete layer and the second cement concrete layer are set to further improve the strength of the floor. While ensuring fast drainage speed and large infiltration volume of the floor, the service life of the floor is extended.
[0009] Furthermore, the void ratio of the first cement concrete layer is 15%-20%, and the laying thickness is 8-13 cm; the void ratio of the second cement concrete layer is 20%-25%, and the laying thickness is 6-9 cm.
[0010] By adopting the above solution, the porosity of the second cement concrete layer is smaller than that of the first cement concrete layer, which is beneficial to speeding up the drainage.
[0011] Furthermore, the first cement concrete layer is composed of the following components by mass concentration: water 95 kg / m 3 -100kg / m 3 , crushed stone 1530kg / m 3 -1560kg / m 3 , sand 25kg / m 3 -28kg / m 3 , cement 290kg / m 3 -295kg / m 3 , water reducing agent 2.5kg / m 3 -2.8kg / m 3 , the particle size of the crushed stone is 15-30mm.
[0012] With the above solution, water, gravel, sand, cement and water reducing agent are used together, so that the first cement concrete layer can provide strength for the floor and at the same time can seep water downward.
[0013] Furthermore, the second cement concrete layer is composed of the following components by mass concentration: water 95kg / m 3 -100kg / m 3 , crushed stone 1530kg / m 3 -1560kg / m 3 , sand 20kg / m 3 -23kg / m 3 , cement 290kg / m 3 -295kg / m 3 , water reducing agent 2.5kg / m 3 -2.8kg / m 3 , the particle size of the crushed stone is 40-55mm.
[0014] With the above solution, water, gravel, sand, cement and water reducing agent are used together, so that the second cement concrete layer can provide strength for the floor and at the same time be able to seep water downward.
[0015] Furthermore, the compaction coefficient of the soil base layer is 93%-94%.
[0016] Furthermore, the compaction coefficient of the first crushed stone slag layer is 94%-95%, and the compaction coefficient of the second crushed stone slag layer is 92%-93%.
[0017] Furthermore, the filter layer adopts a specification of 300-400g / m 2 Geotextile.
[0018] By adopting the above scheme, when rainwater penetrates downward, the geotextile can filter and remove solid particles in the rainwater passing through the permeable layer, the leveling layer, the first cement concrete layer, the first crushed stone slag layer, the second cement concrete layer and the second crushed stone slag layer.
[0019] Furthermore, the wear-resistant layer is composed of dipropylene glycol polyurethane, and the coloring layer is composed of iron oxide pigments.
[0020] By adopting the above scheme, the wear-resistant layer has good mechanical properties and can withstand long-term friction, and the colored layer has a decorative effect, making the road surface more beautiful.
[0021] Furthermore, the anti-slip layer comprises the following components in parts by weight: 20-30 parts of waterborne epoxy resin, 15-20 parts of waterborne acrylic resin, 3-5 parts of cellulose, 2-3 parts of polypropylene fiber, 0.5-2 parts of fumed silica, 0.1-0.5 parts of wetting agent, and 5-8 parts of deionized water.
[0022] The present invention also provides a construction process for a colored anti-slip floor suitable for a sponge city, comprising the following steps:
[0023] S1. Compact the soil base
[0024] S2. Laying the filter layer
[0025] S3. Lay the second crushed stone steel slag layer, the second cement concrete layer, the first crushed stone steel slag layer, the first cement concrete layer in sequence
[0026] S4. Laying the leveling layer
[0027] S5. Lay the anti-skid layer, coloring layer and wear-resistant layer in sequence
[0028] S6. Carry out floor maintenance.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The present invention uses water, crushed stone, sand, cement and a water reducing agent in combination, so that the first cement concrete layer and the second cement concrete layer can provide strength for the floor and at the same time can infiltrate water downwards. The first crushed stone steel slag layer and the second crushed stone steel slag layer are used as cushion layers. By selecting appropriate particle sizes and reasonable proportions of crushed stone and steel slag, the force on the floor is uniform, the strength of the floor is improved, and the service life of the floor is extended while ensuring that the drainage speed of the floor is fast and the infiltration amount is large. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the structure of the present invention.
[0032] In the figure: 1, permeable layer; 11, wear-resistant layer; 12, coloring layer; 13, anti-slip layer; 2, leveling layer; 3, stabilizing layer; 31, first cement concrete layer; 32, first crushed stone and steel slag layer; 33, second cement concrete layer; 34, second crushed stone and steel slag layer; 4, filter layer; 5, soil base layer. DETAILED DESCRIPTION
[0033] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.
[0034] Example 1
[0035] A colored anti-skid floor suitable for a sponge city, comprising, from top to bottom, a permeable layer 1, a leveling layer 2, a stabilizing layer 3, a filter layer 4 and a soil base layer 5, wherein the permeable layer 1 comprises a wear-resistant layer 11, a coloring layer 12 and an anti-skid layer 13 arranged in sequence, and the stabilizing layer 3 comprises, from top to bottom, a first cement concrete layer 31, a first crushed stone steel slag layer 32, a second cement concrete layer 33 and a second crushed stone steel slag layer 34 arranged in sequence, wherein the porosity of the first cement concrete layer 31 is less than that of the second crushed stone steel slag layer 34, and the first crushed stone steel slag layer 32 and the second crushed stone steel slag layer 34 are both composed of crushed stone and steel slag;
[0036] The particle size of the crushed stone of the first crushed stone steel slag layer 32 is 20 mm, the particle size of the steel slag is 15 mm, and the content of the crushed stone is 64%. The laying thickness of the first crushed stone steel slag layer 32 is 6 cm;
[0037] The particle size of the crushed stones of the second crushed stone-steel slag layer 34 is 45 mm, the particle size of the steel slag is 40 mm, the content of the crushed stones is 75%, and the laying thickness of the second crushed stone-steel slag layer 34 is 8 cm.
[0038] The first cement concrete layer 31 has a porosity of 15% and a laying thickness of 8 cm, and the second cement concrete layer 33 has a porosity of 20% and a laying thickness of 6 cm.
[0039] The first cement concrete layer 31 is composed of the following components in mass concentrations: water 95 kg / m3 , crushed stone 1530kg / m 3 , sand 25kg / m 3 , cement 290kg / m 3 , water reducing agent 2.5kg / m 3 , the particle size of the crushed stone is 15mm.
[0040] The second cement concrete layer 33 is composed of the following components in mass concentrations: water 95 kg / m 3 , crushed stone 1530kg / m 3 , sand 20kg / m 3 , cement 290kg / m 3 , water reducing agent 2.5kg / m 3 , the particle size of the crushed stone is 40mm.
[0041] The compaction coefficient of the soil base layer 5 is 93%.
[0042] The compaction coefficient of the first crushed stone slag layer 32 is 94%, and the compaction coefficient of the second crushed stone slag layer 34 is 92%.
[0043] The filter layer 4 adopts a specification of 300g / m 2 Geotextile.
[0044] The wear-resistant layer 11 is composed of dipropylene glycol polyurethane, and the coloring layer 12 is composed of iron oxide pigments.
[0045] The anti-slip layer 13 includes the following components in parts by weight: 28 parts of waterborne epoxy resin, 15 parts of waterborne acrylic resin, 3 parts of cellulose, 3 parts of polypropylene fiber, 0.5 parts of fumed silica, 0.4 parts of wetting agent, and 8 parts of deionized water.
[0046] The present invention also provides a construction process for a colored anti-slip floor suitable for a sponge city, comprising the following steps:
[0047] S1. Compacted soil base 5
[0048] S2. Laying filter layer 4
[0049] S3. Lay the second crushed stone slag layer 34, the second cement concrete layer 33, the first crushed stone slag layer 32, the first cement concrete layer 31 in sequence
[0050] S4. Laying the leveling layer 2
[0051] S5. Lay the anti-slip layer 13, the coloring layer 12, and the wear-resistant layer 11 in sequence
[0052] S6. Carry out floor maintenance
[0053] When maintaining, humidity must be maintained within a week. When the temperature is minus 5℃, only cover and do not water. When the temperature is above 5℃, water once a day (at noon). When the temperature is above 10℃, water twice a day, at 9 am and 2 pm respectively. When the temperature is above 20℃, water 2-3 times a day.
[0054] Example 2
[0055] A colored anti-skid floor suitable for a sponge city, comprising, from top to bottom, a permeable layer 1, a leveling layer 2, a stabilizing layer 3, a filter layer 4 and a soil base layer 5, wherein the permeable layer 1 comprises a wear-resistant layer 11, a coloring layer 12 and an anti-skid layer 13 arranged in sequence, and the stabilizing layer 3 comprises, from top to bottom, a first cement concrete layer 31, a first crushed stone steel slag layer 32, a second cement concrete layer 33 and a second crushed stone steel slag layer 34 arranged in sequence, wherein the porosity of the first cement concrete layer 31 is less than that of the second crushed stone steel slag layer 34, and the first crushed stone steel slag layer 32 and the second crushed stone steel slag layer 34 are both composed of crushed stone and steel slag;
[0056] The particle size of the crushed stone of the first crushed stone steel slag layer 32 is 30 mm, the particle size of the steel slag is 25 mm, and the content of the crushed stone is 70%. The laying thickness of the first crushed stone steel slag layer 32 is 8 cm;
[0057] The particle size of the crushed stones of the second crushed stone-steel slag layer 34 is 55 mm, the particle size of the steel slag is 50 mm, the content of the crushed stones is 80%, and the laying thickness of the second crushed stone-steel slag layer 34 is 11 cm.
[0058] The first cement concrete layer 31 has a porosity of 20% and a laying thickness of 13 cm, and the second cement concrete layer 33 has a porosity of 25% and a laying thickness of 9 cm.
[0059] The first cement concrete layer 31 is composed of the following components in mass concentrations: water 99 kg / m 3 , crushed stone 1550kg / m 3 , sand 28kg / m 3 , cement 290kg / m 3 , water reducing agent 2.8kg / m 3 , the particle size of the crushed stone is 25mm.
[0060] The second cement concrete layer 33 is composed of the following components in mass concentrations: water 99 kg / m 3 , crushed stone 1550kg / m 3 , sand 28kg / m 3 , cement 290kg / m 3 , water reducing agent 2.8kg / m 3 , the particle size of the crushed stone is 50mm.
[0061] The compaction coefficient of the soil base layer 5 is 94%.
[0062] The compaction coefficient of the first crushed stone slag layer 32 is 95%, and the compaction coefficient of the second crushed stone slag layer 34 is 93%.
[0063] The filter layer 4 adopts a specification of 400g / m 2 Geotextile.
[0064] The wear-resistant layer 11 is composed of dipropylene glycol polyurethane, and the coloring layer 12 is composed of iron oxide pigments.
[0065] The anti-slip layer 13 includes the following components in parts by weight: 30 parts of water-based epoxy resin, 20 parts of water-based acrylic resin, 5 parts of cellulose, 3 parts of polypropylene fiber, 2 parts of fumed silica, 0.5 parts of wetting agent, and 8 parts of deionized water.
[0066] In this embodiment, a construction process for a colored anti-slip floor suitable for sponge cities is specifically the same as in Embodiment 1.
[0067] Example 3
[0068] A colored anti-skid floor suitable for a sponge city, comprising, from top to bottom, a permeable layer 1, a leveling layer 2, a stabilizing layer 3, a filter layer 4 and a soil base layer 5, wherein the permeable layer 1 comprises a wear-resistant layer 11, a coloring layer 12 and an anti-skid layer 13 arranged in sequence, and the stabilizing layer 3 comprises, from top to bottom, a first cement concrete layer 31, a first crushed stone steel slag layer 32, a second cement concrete layer 33 and a second crushed stone steel slag layer 34 arranged in sequence, wherein the porosity of the first cement concrete layer 31 is less than that of the second crushed stone steel slag layer 34, and the first crushed stone steel slag layer 32 and the second crushed stone steel slag layer 34 are both composed of crushed stone and steel slag;
[0069] The particle size of the crushed stone of the first crushed stone steel slag layer 32 is 15 mm, the particle size of the steel slag is 5 mm, and the content of the crushed stone is 60%. The laying thickness of the first crushed stone steel slag layer 32 is 4 cm;
[0070] The particle size of the crushed stones of the second crushed stone-steel slag layer 34 is 40 mm, the particle size of the steel slag is 30 mm, the content of the crushed stones is 70%, and the laying thickness of the second crushed stone-steel slag layer 34 is 7 cm.
[0071] The first cement concrete layer 31 has a porosity of 18% and a laying thickness of 10 cm, and the second cement concrete layer 33 has a porosity of 22% and a laying thickness of 7 cm.
[0072] The first cement concrete layer 31 is composed of the following components in mass concentrations: water 97 kg / m 3 , crushed stone 1540kg / m 3 , sand 26kg / m 3 , cement 292kg / m 3 , water reducing agent 2.6kg / m 3, where the particle size of the crushed stone is 20 mm.
[0073] The second cement concrete layer 33 is composed of the following components in mass concentrations: water 97 kg / m 3 , crushed stone 1540kg / m 3 , sand 26kg / m 3 , cement 292kg / m 3 , water reducing agent 2.6kg / m 3 , the particle size of the crushed stone is 45mm.
[0074] The compaction coefficient of the soil base layer 5 is 93.5%.
[0075] The compaction coefficient of the first crushed stone slag layer 32 is 94.5%, and the compaction coefficient of the second crushed stone slag layer 34 is 92.5%.
[0076] The filter layer 4 adopts a specification of 350g / m 2 Geotextile.
[0077] The wear-resistant layer 11 is composed of dipropylene glycol polyurethane, and the coloring layer 12 is composed of iron oxide pigments.
[0078] The anti-slip layer 13 includes the following components in parts by weight: 24 parts of water-based epoxy resin, 18 parts of water-based acrylic resin, 4 parts of cellulose, 2 parts of polypropylene fiber, 1 part of fumed silica, 0.3 parts of wetting agent, and 6 parts of deionized water.
[0079] In this embodiment, a construction process for a colored anti-slip floor suitable for sponge cities is specifically the same as in Embodiment 1.
[0080] Example 4
[0081] A colored anti-skid floor suitable for a sponge city, comprising, from top to bottom, a permeable layer 1, a leveling layer 2, a stabilizing layer 3, a filter layer 4 and a soil base layer 5, wherein the permeable layer 1 comprises a wear-resistant layer 11, a coloring layer 12 and an anti-skid layer 13 arranged in sequence, and the stabilizing layer 3 comprises, from top to bottom, a first cement concrete layer 31, a first crushed stone steel slag layer 32, a second cement concrete layer 33 and a second crushed stone steel slag layer 34 arranged in sequence, wherein the porosity of the first cement concrete layer 31 is less than that of the second crushed stone steel slag layer 34, and the first crushed stone steel slag layer 32 and the second crushed stone steel slag layer 34 are both composed of crushed stone and steel slag;
[0082] The particle size of the crushed stone of the first crushed stone steel slag layer 32 is 25 mm, the particle size of the steel slag is 20 mm, and the content of the crushed stone is 68%. The laying thickness of the first crushed stone steel slag layer 32 is 7 cm;
[0083] The particle size of the crushed stones of the second crushed stone-steel slag layer 34 is 50 mm, the particle size of the steel slag is 45 mm, the content of the crushed stones is 78%, and the laying thickness of the second crushed stone-steel slag layer 34 is 10 cm.
[0084] The first cement concrete layer 31 has a porosity of 16% and a laying thickness of 12 cm, and the second cement concrete layer 33 has a porosity of 24% and a laying thickness of 8 cm.
[0085] The first cement concrete layer 31 is composed of the following components in mass concentrations: water 100 kg / m 3 , crushed stone 1560kg / m 3 , sand 28kg / m 3 , cement 295kg / m 3 , water reducing agent 2.8kg / m 3 , the particle size of the crushed stone is 30mm.
[0086] The second cement concrete layer 33 is composed of the following components in mass concentrations: water 100 kg / m 3 , crushed stone 1560kg / m 3 , sand 28kg / m 3 , cement 295kg / m 3 , water reducing agent 2.8kg / m 3 , the particle size of the crushed stone is 55mm.
[0087] The compaction coefficient of the soil base layer 5 is 94%.
[0088] The compaction coefficient of the first crushed stone slag layer 32 is 95%, and the compaction coefficient of the second crushed stone slag layer 34 is 93%.
[0089] The filter layer 4 adopts a specification of 380g / m 2 Geotextile.
[0090] The wear-resistant layer 11 is composed of dipropylene glycol polyurethane, and the coloring layer 12 is composed of iron oxide pigments.
[0091] The anti-slip layer 13 includes the following components in parts by weight: 20 parts of water-based epoxy resin, 15 parts of water-based acrylic resin, 3 parts of cellulose, 2 parts of polypropylene fiber, 0.5 parts of fumed silica, 0.1 parts of wetting agent, and 5 parts of deionized water.
[0092] In this embodiment, a construction process for a colored anti-slip floor suitable for sponge cities is specifically the same as in Embodiment 1.
[0093] Example 5
[0094] The colored anti-slip floor and its construction process are specifically the same as those in Example 1, except that the first crushed stone slag layer 32 is not provided.
[0095] Example 6
[0096] The colored anti-slip floor and its construction process are specifically the same as those in Example 2, except that the first crushed stone slag layer 32 is not provided.
[0097] Example 7
[0098] The colored anti-slip floor and its construction process are specifically the same as those in Example 3, except that the first crushed stone slag layer 32 is not provided.
[0099] Example 8
[0100] The colored anti-slip floor and its construction process are specifically the same as those in Example 4, except that the first crushed stone slag layer 32 is not provided.
[0101] Example 9
[0102] The colored anti-slip floor and its construction process are specifically the same as those in Example 1, except that the second cement concrete layer 33 is not provided.
[0103] Example 10
[0104] The colored anti-slip floor and its construction process are specifically the same as those in Example 2, except that the second cement concrete layer 33 is not provided.
[0105] Embodiment 11
[0106] The colored anti-slip floor and its construction process are specifically the same as those in Example 3, except that the second cement concrete layer 33 is not provided.
[0107] Example 12
[0108] The colored anti-slip floor and its construction process are specifically the same as those in Example 4, except that the second cement concrete layer 33 is not provided.
[0109] Comparative Example 1
[0110] The colored anti-slip floor and its construction process are specifically the same as those in Example 1, except that the first crushed stone slag layer 32 is composed of crushed stone only.
[0111] Comparative Example 2
[0112] The colored anti-slip floor and its construction process are specifically the same as those in Example 2, except that the first crushed stone slag layer 32 is composed of crushed stone only.
[0113] Comparative Example 3
[0114] The colored anti-slip floor and its construction process are specifically the same as those in Example 3, except that the first crushed stone slag layer 32 is composed of crushed stone only.
[0115] Comparative Example 4
[0116] The colored anti-slip floor and its construction process are specifically the same as those in Example 4, except that the first crushed stone slag layer 32 is composed of crushed stone only.
[0117] Comparative Example 5
[0118] The colored anti-slip floor and its construction process are specifically the same as those in Example 1, except that the second crushed stone slag layer 34 is composed of crushed stone only.
[0119] Comparative Example 6
[0120] The colored anti-slip floor and its construction process are specifically the same as those in Example 2, except that the second crushed stone slag layer 34 is composed of crushed stone only.
[0121] Comparative Example 7
[0122] The colored anti-slip floor and its construction process are specifically the same as those in Example 3, except that the second crushed stone slag layer 34 is composed of crushed stone only.
[0123] Comparative Example 8
[0124] The colored anti-slip floor and its construction process are specifically the same as those in Example 4, except that the second crushed stone slag layer 34 is composed of crushed stone only.
[0125] Comparative Example 9
[0126] The permeable pavement is constructed according to the construction method of the permeable integral pavement disclosed in Example 1 of Chinese Patent CN109958018A to produce a permeable pavement.
[0127] Test Example 1 Water Permeability and Strength Test
[0128] The water permeability and strength tests were performed on the floors of Example 1, Example 5, Example 9, Comparative Example 1, Comparative Example 5 and Comparative Example 9, and the results are shown in Table 1-2.
[0129] Table 1 Water permeability test of the floor of Example 1, Example 5, Example 9, Comparative Example 1, Comparative Example 5 and Comparative Example 9
[0130]
[0131]
[0132] It can be seen from the data in Table 1 that when the water spraying rates are 5L / min, 20L / min, 40L / min, and 60L / min respectively and the water is continuously sprayed for 10min, the floors of Example 1, Example 9, Comparative Example 1, and Comparative Example 5 can all be quickly infiltrated without water accumulation; the floor of Example 5 does not have a first crushed stone slag layer 32, and when the water spraying rate is 40L / min, a small amount of water accumulates on the floor of Example 5 after 3min, and more water accumulates after 5min; when the water spraying rate is 40L / min, a small amount of water accumulates on the floor of Example 5 after 1min, and more water accumulates after 3min; when the water spraying rate is 60L / min, a small amount of water accumulates on the floor of Comparative Example 9 after 5min, and more water accumulates after 8min; this indicates that the water seepage effects of the floors of Example 1, Example 9, Comparative Example 1, and Comparative Example 5 are better than those of Example 5 and Comparative Example 9.
[0133] Table 2 Strength performance test of the floor of Example 1, Example 5, Example 9, Comparative Example 1, Comparative Example 5 and Comparative Example 9
[0134]
[0135]
[0136] From the data in Table 2, we can see that the 5t roller can continuously roll for 1h, the 8t roller can continuously roll for 1h, and the 15t roller can continuously roll for 1h. When the rollers were continuously rolled for 1 hour and the 25t rollers were continuously rolled for 1 hour, the floor of Example 1 had no cracks; when the 5t rollers were continuously rolled for 1 hour and the 8t rollers were continuously rolled for 1 hour, the floors of Example 5, Example 9, Comparative Example 1 and Comparative Example 5 had no cracks, but when the 15t rollers were continuously rolled for 1 hour and the 25t rollers were continuously rolled for 1 hour, the floors of Example 5, Example 9, Comparative Example 1 and Comparative Example 5 had cracks; when the 5t rollers were continuously rolled for 1 hour, the 8t rollers were continuously rolled for 1 hour and the 15t rollers were continuously rolled for 1 hour, the floor of Comparative Example 9 had no cracks, but when the 25t rollers were continuously rolled for 1 hour, the floor of Comparative Example 9 had cracks; it shows that compared with Example 5, Example 9, Comparative Example 1, Comparative Example 5 and Comparative Example 9, the floor strength of Example 1 is the highest. In summary, the comprehensive performance of the floor of Example 1 is the best.
[0137] The above test was also carried out on Examples 2-4, Examples 6-8, Examples 10-12, Comparative Examples 2-4, Comparative Examples 6-8, and Comparative Examples 10-12, and their test results were similar to those of Example 1, Example 5, Example 9, Comparative Example 1, Comparative Example 5, and Comparative Example 9.
[0138] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.
[0139] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A colored non-slip floor suitable for sponge cities, characterized in that: The invention comprises, from top to bottom, a water-permeable layer (1), a leveling layer (2), a stabilizing layer (3), a filter layer (4) and a soil base layer (5); the water-permeable layer (1) comprises a wear-resistant layer (11), a coloring layer (12) and an anti-skid layer (13) which are arranged in sequence; the stabilizing layer (3) comprises, from top to bottom, a first cement concrete layer (31), a first crushed stone steel slag layer (32), a second cement concrete layer (33) and a second crushed stone steel slag layer (34); the porosity of the first cement concrete layer (31) is smaller than that of the second crushed stone steel slag layer (34); the first crushed stone steel slag layer (32) and the second crushed stone steel slag layer (34) are both composed of crushed stone and steel slag; The particle size of the crushed stones in the first crushed stone and steel slag layer (32) is 15-30 mm, the particle size of the steel slag is 5-25 mm, and the content of the crushed stones is 60%-70%. The laying thickness of the first crushed stone and steel slag layer (32) is 4-8 cm; The particle size of the crushed stones in the second crushed stone and steel slag layer (34) is 40-55 mm, the particle size of the steel slag is 30-50 mm, the content of the crushed stones is 70%-80%, and the laying thickness of the second crushed stone and steel slag layer (34) is 7-11 cm; The wear-resistant layer (11) is composed of dipropylene glycol polyurethane, and the coloring layer (12) is composed of iron oxide pigments; The anti-slip layer (13) comprises the following components in parts by weight: 20-30 parts of water-based epoxy resin, 15-20 parts of water-based acrylic resin, 3-5 parts of cellulose, 2-3 parts of polypropylene fiber, 0.5-2 parts of fumed silica, 0.1-0.5 parts of wetting agent, and 5-8 parts of deionized water.
2. The colored non-slip floor suitable for sponge cities according to claim 1 is characterized in that: The porosity of the first cement concrete layer (31) is 15%-20%, and the laying thickness is 8-13 cm; the porosity of the second cement concrete layer (33) is 20%-25%, and the laying thickness is 6-9 cm.
3. The colored non-slip floor suitable for sponge cities according to claim 2 is characterized in that: The first cement concrete layer (31) is composed of the following components in mass concentrations: water 95 kg / m 3 -100kg / m 3 , crushed stone 1530kg / m 3 -1560kg / m 3 , sand 25kg / m 3 -28kg / m 3 , cement 290kg / m 3 -295kg / m 3 , water reducing agent 2.5kg / m 3 -2.8kg / m 3 , the particle size of the crushed stone is 15-30mm.
4. The colored non-slip floor suitable for sponge cities according to claim 2 is characterized in that: The second cement concrete layer (33) is composed of the following components in mass concentrations: water 95 kg / m 3 -100kg / m 3 , crushed stone 1530kg / m 3 -1560kg / m 3 , sand 20kg / m 3 -23kg / m 3 , cement 290kg / m 3 -295kg / m 3 , water reducing agent 2.5kg / m 3 -2.8kg / m 3 , the particle size of the crushed stone is 40-55mm.
5. The colored non-slip floor suitable for sponge cities according to claim 1 is characterized in that: The compaction coefficient of the soil base layer (5) is 93%-94%.
6. The colored non-slip floor suitable for sponge cities according to claim 1 is characterized in that: The compaction coefficient of the first crushed stone slag layer (32) is 94%-95%, and the compaction coefficient of the second crushed stone slag layer (34) is 92%-93%.
7. The colored non-slip floor suitable for sponge cities according to claim 1 is characterized in that: The filter layer (4) has a specification of 300-400g / m 2 Geotextile.
8. A construction process for a colored anti-slip floor suitable for a sponge city according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1. Compacted soil base (5) S2. Laying the filter layer (4) S3. Lay the second crushed stone slag layer (34), the second cement concrete layer (33), the first crushed stone slag layer (32), and the first cement concrete layer (31) in sequence S4. Laying the leveling layer (2) S5. Lay the anti-skid layer (13), the coloring layer (12), and the wear-resistant layer (11) in sequence S6. Carry out floor maintenance.
Citation Information
Patent Citations
Permeable pavement structure for heavy rainfall urban road and construction method of permeable pavement structure
CN109958018A
A permeable concrete pavement structure with planting holes and its construction method
CN102296511A
Colored water permeable integral pavement and construction technology
CN105544338A
Flexible base layer of multilayer separation structure and construction method of flexible base layer
CN112982061A
Sponge urban rainwater circulation system's earth's surface permeable formation structure
CN206495107U