A plating method for realizing high aspect ratio through-blind vias and PCB

By adjusting the magnitude of the forward pulse current according to the burst period and non-explosion period of the additive during the electroplating process, and combining electroplating agents with leveling agents, inhibitors and brighteners, the high cost and efficiency of blind hole electroplating in the prior art is solved. The problem of low achieves high-efficiency and low-cost high-aspect ratio electroplating effect.

CN114554727BActive Publication Date: 2024-12-06DONGGUAN SHENGYI ELECTRONICS
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210333275.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-31
Publication Date
2024-12-06
Estimated Expiration
2042-03-31

AI Technical Summary

Technical Problem

The existing blind hole electroplating technology cannot take into account both cost and efficiency, resulting in high processing costs and low electroplating time efficiency.

Method used

The forward pulse plating method is adopted to implement a large forward pulse current during the burst period of the additive and a small forward pulse current during the non-explosion period. The electroplating potion of leveling agent, inhibitor and brightener is combined to meet the through hole and blind hole. Electroplating requirements.

Benefits of technology

The electroplating with high aspect ratio through blind holes is achieved, with simple process, low cost and high efficiency, improving the electroplating time efficiency and ensuring the deep plating ability and reliability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114554727B_ABST
    Figure CN114554727B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of PCBs, and discloses a plating method and PCB for realizing high aspect ratio through and blind holes. The plating method comprises: providing a plate to be plated with through holes and / or blind holes, and copper depositing the plate to be plated; in a plating solution environment with additives added, using a forward pulse plating method to electroplate the plate to be plated after copper deposition; the additives include a leveling agent, an inhibitor and a brightener; during the plating process, the first forward pulse current implemented during the additive burst period of the entire plating cycle is controlled to be greater than the second forward pulse current implemented during the additive non-burst period. The plating method provided in an embodiment of the present invention adopts a plating method combining forward pulse plating with direct current plating solution, and according to the characteristics of the additives, different sizes of forward pulse currents are implemented during the burst period and the non-burst period, while meeting the plating needs of through holes and blind holes, and has the advantages of simple process, low cost and high efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of PCB (Printed Circuit Board), and in particular to an electroplating method for realizing high aspect ratio through and blind vias and a PCB. Background Art

[0002] With the rapid development and application promotion of 5G products, the trend of printed circuit boards (PCBs) towards high-speed and high-density design is becoming more and more obvious. For example, the mature 56G core network switches and routers in the communication field have a thickness of 4.5mm, a through-hole aspect ratio of 30:1, and a 1-4-layer aperture of 12-14mil and a depth-to-diameter ratio ≥1.0 deep micro-blind hole design. At present, this type of product is gradually breaking through the 112G rate. Its design layout is more intensive, and its related process manufacturing is more difficult. The stability maintenance bottleneck of the deep plating capacity of wet process copper plating is more prominent. At present, there are several methods for electroplating such products:

[0003] (1) Through holes and blind holes are plated separately

[0004] The main process of this method is: ...→ lamination → laser drilling (blind hole) → plasma → decontamination copper deposition → board surface electroplating 1 → ...→ copper thinning / sand belt grinding (optional process) → drilling (through hole) → plasma 1 → decontamination copper deposition 1 → board surface electroplating 2 1 → outer layer dry film → graphic electroplating → .... This method electroplates the blind holes and through holes separately, which can achieve good deep plating capabilities for through holes and blind holes, but due to its long process, the processing cost is very high.

[0005] (2) Flash plating for filling holes and long-term combination plating with low current

[0006] The main process of this method is: ...→ lamination → drilling (through hole) → laser drilling (blind hole) plasma → decontamination copper deposition → board surface electroplating one (VCP filling line through hole and blind hole flash plating) → decontamination copper deposition → board surface electroplating two (through hole thickening copper) → belt grinding (optional process) → ... → outer layer dry film → graphic electroplating → ..., this method has a relatively shorter process than the first method, but because the through hole is in the board surface electroplating process one, since the VCP line has weaker equipment capacity than the gantry line, the potion has poor hole filling ability for the through hole, so the flash plating layer has poor deep plating ability at this time. When thickening copper in the board surface electroplating process two, a small current and long time electroplating method (common current density is 4.5-6ASF, and the electroplating time is 400-700min) is required to achieve high aspect ratio through-hole electroplating. The electroplating time efficiency is extremely low and output is difficult.

[0007] (3) Forward and reverse pulse plating

[0008] The main process of this method is: ...→ lamination → drilling (through hole) → laser drilling (blind hole) plasma → decontamination copper deposition → board surface electroplating (positive and negative pulse electroplating) → ... → outer layer dry film → pattern electroplating → .... This method uses the reverse biting copper of pulse electroplating to achieve thin surface copper and improve the deep plating ability of through and blind holes. The process flow is relatively simple, but the simultaneous electroplating of through and blind holes of such products will produce columnar crystals due to the reverse current biting effect of the pulse. The crystal lattice gap is large and it is easy to crack when heated, as shown below Figure 1 and 2 As shown in the figure, when such products are soldered at high temperature on the client side, the copper layer may crack. Figure 3 As shown, it seriously affects the reliability of the product, so many customers currently do not accept products with columnar crystals.

[0009] (4) High copper solution and low copper solution combined electroplating

[0010] The main process of this method is: ...→ lamination → drilling (through hole) → laser drilling (blind hole) plasma → decontamination copper deposition → board surface electroplating (flash plating of through holes and blind holes with high copper solution) → decontamination copper deposition → board surface electroplating (thickening copper with low copper solution for through holes) → sanding (optional process) → ... → outer layer dry film → pattern electroplating → .... This method has the simplest process and uses the difference in copper ion concentration to achieve simultaneous electroplating of through and blind holes. However, when this method is implemented, low copper solution and high copper solution must be distributed in different electroplating tanks on the same electroplating line. When electroplating a board designed for through and blind holes, the high copper solution is first used in a high copper tank to meet the electroplating of the blind holes, and then the low current and long time method is used in a low copper solution to achieve the deep plating capability of the through holes, which is similar to some processes in method (2). The output is limited when the product is mass-produced.

[0011] The above-mentioned technologies for achieving through-hole and blind-hole electroplating each have their own advantages and disadvantages, and cannot take both cost and efficiency into consideration at the same time. Summary of the invention

[0012] The object of the present invention is to provide a method for electroplating through and blind vias with a high aspect ratio and a PCB, so as to overcome the defect of the existing through and blind via electroplating technology that both cost and efficiency cannot be taken into account at the same time.

[0013] To achieve this object, the present invention adopts the following technical solutions:

[0014] A method for electroplating a through-blind via with a high aspect ratio, comprising:

[0015] Providing a plate to be electroplated with through holes and / or blind holes, and depositing copper on the plate to be electroplated;

[0016] In an electroplating solution environment with additives added thereto, the copper-plated plate to be electroplated is electroplated by a forward pulse electroplating method; the additives include a leveling agent, an inhibitor and a brightener;

[0017] During the electroplating process, a first forward pulse current implemented during the additive burst period of the entire electroplating cycle is controlled to be greater than a second forward pulse current implemented during the additive non-burst period of the entire electroplating cycle.

[0018] Optionally, when switching between the first forward pulse current and the second forward pulse current, a power-off operation of a preset duration is performed.

[0019] Optionally, the waveform of the forward pulse includes a square wave and / or a sine wave.

[0020] Optionally, the current density corresponding to the first forward pulse current has a value range of 8ASF-15ASF, and the current density corresponding to the second forward pulse current has a value range of 5-10ASF.

[0021] Optionally, the current density corresponding to the first forward pulse current has a value range of 8ASF-10ASF, and the current density corresponding to the second forward pulse current has a value range of 5-8ASF.

[0022] Optionally, the start time of the additive burst period is: within 10 minutes to 15 minutes after the start of electroplating of the plate to be electroplated; the duration of the additive burst period is 10-30 minutes.

[0023] Optionally, in the electroplating solution environment, the concentration of copper sulfate is 60-90 g / L.

[0024] A PCB is manufactured according to any of the above electroplating methods for realizing high aspect ratio through and blind vias.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The electroplating method provided in the embodiment of the present invention adopts an electroplating method that combines forward pulse electroplating with direct current plating solution (i.e., a plating solution that includes three components of additives: a leveler, an inhibitor, and a brightener). According to the characteristics of the additives in the direct current plating solution, forward pulse currents of different sizes are implemented during the additive burst period and the additive non-burst period, thereby meeting the electroplating needs of through holes and blind holes, and has the advantages of simple process, low cost, and high efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 It is a view of the existing columnar crystal at the through hole opening;

[0029] Figure 2 This is the existing columnar crystal view of the blind hole mouth;

[0030] Figure 3 Weld copper fracture view for existing pulse columnar crystallization products;

[0031] Figure 4 It is a schematic diagram of conventional forward and reverse pulses;

[0032] Figure 5 A flow chart of a method for electroplating high aspect ratio through and blind vias provided by an embodiment of the present invention;

[0033] Figure 6 A schematic diagram of the distribution of electric lines of force during the non-explosion period of the additive in the electroplating process provided by an embodiment of the present invention;

[0034] Figure 7 A schematic diagram of the distribution of electric lines during the additive burst period in the electroplating process provided by an embodiment of the present invention;

[0035] Figure 8 (a) and (b) are the adsorption state of additives during the burst period and the copper plating effect of blind holes, respectively;

[0036] Fig. 9 (a) and (b) are the adsorption state of the additive in the non-explosion period and the copper plating effect of the blind hole, respectively;

[0037] Fig.10 A waveform diagram of a positive pulse wave provided by an embodiment of the present invention;

[0038] Fig.11 (a) and (b) are structural diagrams of through holes and blind holes after electroplating provided by embodiments of the present invention, respectively;

[0039] Fig.12 (a) and (b) are respectively slice diagrams of through holes and blind holes of an electroplated product with a plate thickness of 4.5 mm, a through hole aspect ratio of 30:1, a blind hole diameter of 14 mil and a depth-to-diameter ratio of 1.3 provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0040] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the embodiments described below are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Pulse plating refers to electroplating that uses pulse power instead of DC power. During the electroplating process, the electrodeposition process can be changed in a wide range by controlling parameters such as waveform, frequency, on-off ratio and average current density, so as to obtain a coating with certain characteristics in a certain plating solution.

[0042] Compared with ordinary DC electroplating, pulse electroplating has a very small pulse width (i.e., conduction time) and a very high peak current density. During operation, the metal ions near the cathode are sharply reduced, and the diffusion layer is cut off from the power supply before it has time to grow thick. During the pulse interval, the metal ions lacking on the cathode surface can be replenished in time by the main solution, and the pulse diffusion layer is basically eliminated, making the concentration of metal ions in the electrolyte tend to be consistent. Therefore, pulse electroplating has the advantages of smooth and dense coating, good adhesion, high current efficiency, and good environmental performance.

[0043] The pulse mode used in pulse plating can be divided into two types: unidirectional pulse and bidirectional pulse. The pulse mode commonly used to achieve synchronous electroplating of through and blind holes is bidirectional pulse, also known as forward and reverse pulse. Its pulse wave is as follows: Figure 4 shown.

[0044] In order to ensure the smoothness of the electroplating coating surface, it is often necessary to add additives to the plating solution. Commonly used additives include leveling agents, inhibitors and brighteners.

[0045] ① Leveling agent, mainly electrochemical adsorption, adsorbed in the high potential area of ​​the cathode, adsorbed electrons and Cu 2+ The competitive effect is formed, so that the Cu deposition rate in the high potential area is slowed down, making the surface copper and hole copper thickness close;

[0046] ②Inhibitor, also called wetting agent, is used to promote the better dissolution of leveling agent and brightener in the plating solution and improve the dispersibility of the plating solution. Its macromolecular multi-functional group structure characteristics can be combined with Cu 2+ and Cl - Complexation forms a long molecular chain film, which hinders Cu 2+ Electrons are obtained on the cathode surface to form Cu deposition.

[0047] ③ Brightener: Its main function is to refine copper grains, making the copper surface bright.

[0048] Normally, for DC electroplating, the additives used include three components: leveling agent, inhibitor and brightener; while for pulse electroplating, the additives used include only two components: inhibitor and brightener. This is because: when using forward and reverse pulse electroplating technology to achieve high aspect ratio through-blind hole electroplating, due to the reverse pulse anode stripping (anti-etching the electroplated copper layer) of the bidirectional pulse power supply, the leveling agent in the additive cannot be adsorbed on the cathode (the leveling agent will fall off along with the electroplated copper layer) to play a leveling role, so the electroplating solution system used can only be a pulse solution system (mainly inhibitors and brighteners, without leveling agent). On this basis, when the forward and reverse pulses are working, due to the lack of the inhibitory effect of the leveling agent, the copper layer will be thicker when electroplating with the forward pulse current. Therefore, it is necessary to use a very strong reverse current to erode the copper on the opposite side and the hole mouth, so that the copper thickness in the hole can be as close to the surface copper thickness as possible, and meet the deep plating capacity requirements required by customers.

[0049] To solve various existing technical problems, please refer to Figure 5 , an embodiment of the present invention provides an electroplating method for realizing high aspect ratio through and blind vias, comprising:

[0050] Step 101: Provide a plate to be plated with through holes and / or blind holes, and deposit copper on the plate to be plated.

[0051] In this step, a plate to be plated with through holes and / or blind holes can be prepared according to conventional processes. The number, diameter and depth of the through holes and / or blind holes are not limited.

[0052] Step 102, in an environment of electroplating solution with additives added thereto, a forward pulse electroplating method is used to electroplate the copper-plated board, wherein the additives include a leveler, an inhibitor and a brightener; at the same time, during the electroplating process, a first forward pulse current implemented during an additive burst period in the entire electroplating cycle is controlled to be greater than a second forward pulse current implemented during an additive non-burst period in the entire electroplating cycle.

[0053] The electroplating method provided in the embodiment of the present invention adopts an electroplating method that combines forward pulse electroplating with direct current plating solution (i.e., a plating solution that includes three components of additives: a leveler, an inhibitor, and a brightener), and according to the characteristics of the additives in the direct current plating solution, different sizes of forward pulse currents are implemented during the additive burst period and the additive non-burst period, thereby meeting the electroplating needs of through holes and blind holes.

[0054] It should be noted that the additive outbreak period refers to the time interval during which the leveling agent and brightener can exert a good adsorption effect during the electroplating process. The additive non-explosion period refers to the time interval during the entire electroplating process except the outbreak period, which can be further divided into the adjustment period (i.e., the cumulative process of additive adsorption, the start time of which is called the start of plating) and the stable period before and after the outbreak period.

[0055] Through repeated experiments, research and analysis, the starting time of the additive outbreak period is: within 10min-15min after the start of electroplating of the electroplated plate; the duration of the additive outbreak period is 10-30min.

[0056] The effect of additives on copper plating is mainly to affect the distribution of power lines. Figure 6 The schematic diagram of the distribution of electric lines during the non-explosion period of the additive during the electroplating process is shown. Figure 7 The figure shows the distribution of electric lines during the additive burst period in the electroplating process. Figure 6 and Figure 7 It can be seen that the plate surface area is a high current density area, the blind hole bottom area is a low current density area, and the current density of the blind hole bottom area during the burst period is higher than that during the non-burst period.

[0057] It should be noted that since the adsorption of the leveling agent component in the additive on the cathode surface is a strong potential chemical adsorption, it will adsorb electrons and be reduced, and 2+ The process of ion-attracting electrons and being reduced forms a competitive relationship, so the leveling agent is generally adsorbed in the high current density area.

[0058] Since the adsorption of the brightener in the additive on the cathode surface is a weak potential chemical adsorption, its main function is a grain refiner. Therefore, the brightener is generally adsorbed in the low current density area and has a certain effect of accelerating the deposition of copper ions. It must be completed with the assistance of a leveling agent.

[0059] Through repeated experimental analysis, it is known that the adsorption state of additives during the burst period is as follows Figure 8 As shown in (a), the leveling agent is mainly adsorbed on the plate surface area, and the brightener is mainly adsorbed on the hole bottom area. 2+ The process of ion absorption electron reduction forms a competitive relationship, which has a certain inhibitory effect on copper ion deposition, while the brightener has a certain effect of accelerating copper ion deposition. Therefore, this adsorption state will cause the copper plating speed of the low current density area at the bottom of the blind hole to be greater than the copper plating speed of the board surface. At this time, the copper plating effect of the blind hole is better, such as Figure 8 On this basis, the embodiment of the present invention implements a larger first positive pulse current during the burst period, which can simultaneously accelerate the copper plating speed of the hole bottom and the board surface, and increase the difference between the copper plating thickness at the hole bottom and the copper plating thickness on the board surface.

[0060] Through repeated experimental analysis, it is known that the adsorption state of the additive in the non-explosive period is as follows Fig. 9 As shown in (a), compared with the adsorption state in the burst period, the adsorption amount of the leveling agent in the board surface area decreases and the adsorption amount in the hole bottom area increases, the adsorption amount of the brightener in the board surface area increases and the adsorption amount in the hole bottom area decreases. Due to the inhibitory effect of the leveling agent on copper ion deposition and the accelerated effect of the brightener on copper ion deposition, the copper plating speed of the board surface is greater than the copper plating speed of the blind hole bottom, especially in the low current density area at the corner of the bottom of the blind hole, a wedge-shaped hole will appear, resulting in thin copper, such as Fig. 9 On this basis, if the electroplating continues according to the larger first forward pulse current implemented in the burst period, the surface copper will be too thick, so the forward pulse current is adjusted in the non-burst period, and a smaller second forward pulse current is implemented.

[0061] For through-holes, the main factors affecting the through-hole electroplating effect include the liquid exchange rate and additives (mainly leveling agents and brighteners). Under the same conditions, the influence of the liquid exchange rate in the outbreak period and the non-outbreak period is basically the same; however, the influence of additives in the outbreak period and the non-outbreak period is different. The following describes the electroplating process of through-holes in the outbreak period and the non-outbreak period respectively:

[0062] (1) During the outbreak period, since the leveling agent is mostly distributed at the hole mouth and the brightener is mostly distributed in the hole, a larger first positive pulse current is used in this stage, which will enhance the inhibitory effect of the leveling agent on copper ion deposition and the promoting effect of the brightener on copper ion deposition. Therefore, for the same through hole, the copper plating speed in the hole will be greater than the copper plating speed at the hole mouth, and ultimately the copper thickness in the hole will be greater than the copper thickness at the hole mouth.

[0063] Compared with the blind hole in the same environment, due to the structural difference, the brightener attached to the through hole in the outbreak period will be less than the brightener attached to the bottom of the blind hole. Therefore, after the outbreak period, the copper thickness in the through hole will be thinner than the copper thickness at the bottom of the blind hole. In other words, the difference in copper thickness between the through hole opening and the hole is smaller than the difference in copper thickness between the blind hole opening and the bottom.

[0064] In addition, compared with the conventional method of using a single current to electroplate through holes, the method of applying a larger first positive pulse current during the burst period adopted in the embodiment of the present invention can effectively promote the deposition of copper ions in the through holes, increase the electroplating speed in the holes, and achieve a higher deep plating capability.

[0065] (2) During the non-explosion period, the adsorption amount of the leveler in the hole mouth area decreases and the adsorption amount in the hole area increases, while the adsorption amount of the brightener in the hole mouth area increases and the adsorption amount in the hole area decreases. Therefore, during the electroplating process, the electroplating speed of the through hole mouth is higher than the electroplating speed in the hole. At this time, a smaller second forward pulse current is implemented to reduce the difference in electroplating speed between the hole mouth and the hole in the non-explosion period, thereby avoiding excessive thickness of the copper layer at the hole mouth.

[0066] It should be noted that although the second forward pulse current is smaller than the first forward pulse current, it is still larger than the current used in the conventional method of electroplating through holes with a single current (in the prior art, the current density corresponding to the current is usually less than 5ASF). Therefore, not only can a copper layer with a higher thickness consistency be deposited at the hole mouth and the hole after the non-explosion period, but also a higher electroplating speed is achieved.

[0067] In summary, for through holes, the electroplating method provided by the embodiment of the present invention can achieve a higher electroplating speed regardless of the burst period or the non-burst period, and has a strong deep plating ability, and the copper thickness finally formed at the hole mouth and in the hole has a high consistency.

[0068] In summary, the embodiment of the present invention implements different forward pulse currents at different stages, and switches the size of the forward pulse current according to the burst period of the additive, which can meet the needs of through-hole and blind-hole electroplating at the same time. Through-hole electroplating is mainly based on the exchange of chemical solution, and a smaller current is used in the non-burst period, which is conducive to through-hole electroplating; blind-hole electroplating is mainly based on the leveling agent and brightener of the additive. During the burst period, the adsorption of the leveling agent and brightener in the blind hole reaches a suitable ratio, and the electroplating rate suddenly increases. A larger current is used, which is conducive to electroplating and filling the bottom corner of the blind hole.

[0069] In addition, when switching between the first forward pulse current and the second forward pulse current, a power-off operation of a preset duration can be performed (the power-off time period is 2-6 mms). In this process, the Cu near the surface of the cathode (i.e., the plate to be plated) 2+ The consumption of ions can be quickly replenished through microscopic diffusion so that the cathode maintains continuous and uniform electroplating, so that both through holes and blind holes can obtain better deep plating capabilities.

[0070] In an optional embodiment, the waveform of the positive pulse wave can be a square wave (such as Fig.10 In practical applications, the first forward pulse current implemented during the entire burst period can remain unchanged or change according to a certain curve; similarly, the second forward pulse current implemented during the entire non-burst period can remain unchanged or change according to a certain curve. The specific design can be flexibly based on the characteristics of the plate to be plated and the actual electroplating requirements, as long as the prerequisite that the first forward pulse current is greater than the second forward pulse current is met.

[0071] For example, the current density corresponding to the first positive pulse current ranges from 8ASF to 15ASF (preferably 8ASF to 10ASF), which satisfies the blind hole corner filling; the current density corresponding to the second positive pulse current ranges from 5 to 10ASF (preferably 5 to 8ASF), which satisfies the through hole deep plating capability electroplating. In general, cathode current (i.e., positive pulse current) = current density (ASF) × board double-sided area (ft 2 )×number of plates. For example, the current density corresponding to the first forward pulse current is 10ASF and the current density corresponding to the second forward pulse current is 8ASF. Fig.10 The double-sided area of ​​the board is 6.0ft 2 In this waveform, the forward pulse current in the non-burst period (referring to stage ① and stage ③ in the figure) = 8ASF×6.0ft 2 ×1=48A, forward pulse current in the burst period (referring to stage ② in the figure)=10ASF×6.0ft 2 ×1=60A.

[0072] In addition, according to the characteristics of high copper, medium copper and low copper solution systems shown in the table below, when the embodiment of the present invention is applied to electroplating through holes and blind holes at the same time, medium copper solution (copper sulfate concentration is: 60g / L-90g / L) is preferred, which can take into account the electroplating requirements of through holes and blind holes, ensuring that both can obtain good electroplating effects.

[0073]

[0074] The embodiment of the present invention further provides a PCB, which is prepared by the above-mentioned electroplating method. Due to the above-mentioned through-hole and blind-hole synchronous electroplating technology, the technology adopts a combination of forward pulse electroplating and direct current electroplating solution, and has the characteristics of simple process flow, low cost and high efficiency. After the technology is implemented, slicing can be performed, and the through-hole depth capability and blind-hole depth capability can be respectively detected according to the following formulas:

[0075]

[0076]

[0077] Among them, A, B, C, D, E, F, C1, C2, S1, and S2 are Fig.11 Copper thickness measurements at corresponding locations in (a) and (b).

[0078] After repeated verification, the application of the embodiment of the present invention can achieve a deep plating capability of ≥80% for a through hole with a 4.5mm plate thickness and an aspect ratio of 30:1, and a process capability of a deep micro blind hole with a diameter of 14mil and an aspect ratio of 1.3. Fig.12 As shown in (a) and (b), the electroplating current density can be increased from an average of 5ASF to an average of 8ASF, the electroplating time is 200-300min, and the time efficiency is increased by an average of 43%. After the hot and cold shock (-55℃-125℃ 500 cycles) test, the quality meets the requirements and the equipment capacity is released.

[0079] As described above, the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for electroplating a through-blind via with a high aspect ratio, comprising: Providing a plate to be electroplated with through holes and blind holes, and depositing copper on the plate to be electroplated; In an electroplating solution environment with additives added thereto, the copper-plated plate to be electroplated is electroplated by a forward pulse electroplating method; the additives include a leveling agent, an inhibitor and a brightener; During the electroplating process, the first forward pulse current implemented during the additive burst period of the entire electroplating cycle is controlled to be greater than the second forward pulse current implemented during the additive non-burst period of the entire electroplating cycle, thereby meeting the electroplating requirements of the through hole and the blind hole at the same time; The additive burst period refers to the time interval during which the leveling agent and brightener can exert a good adsorption effect during the electroplating process, and the additive non-burst period refers to the time interval during the entire electroplating process except the additive burst period; The value of the current density corresponding to the second forward pulse current is greater than or equal to 5ASF.

2. The electroplating method for realizing high aspect ratio through and blind vias according to claim 1, characterized in that: When switching between the first forward pulse current and the second forward pulse current, a power-off operation of a preset duration is performed.

3. The electroplating method for realizing high aspect ratio through and blind vias according to claim 2, characterized in that: The waveform of the forward pulse includes a square wave and / or a sine wave.

4. The electroplating method for realizing high aspect ratio through and blind vias according to claim 2, characterized in that: The current density corresponding to the first forward pulse current has a value range of 8ASF-15ASF, and the current density corresponding to the second forward pulse current has a value range of 5-10ASF.

5. The electroplating method for realizing high aspect ratio through and blind vias according to claim 4, characterized in that: The current density corresponding to the first forward pulse current has a value range of 8ASF-10ASF, and the current density corresponding to the second forward pulse current has a value range of 5-8ASF.

6. The electroplating method for realizing high aspect ratio through and blind vias according to claim 1, characterized in that: The starting time of the additive burst period is: within 10 minutes to 15 minutes after the start of electroplating of the plate to be electroplated; the duration of the additive burst period is 10 to 30 minutes.

7. The electroplating method for realizing high aspect ratio through and blind vias according to claim 1, characterized in that: In the electroplating solution environment, the concentration of copper sulfate is 60-90 g / L.

8. A PCB, characterized in that: The PCB is manufactured according to the electroplating method for realizing high aspect ratio through and blind vias according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Filling through-holes

    CN105517371A

  • Blind hole-filling electroplating process, plated part obtained according to process, application of plated part, and electronic product

    CN111270277A

  • Through hole electroplating and filling method and preparation method of printed circuit board

    CN112030203A

  • Method for combined through-hole plating and via filling

    US20150289387A1

  • High-speed electroplating method

    US20200048786A1