Conductive paste, preparation method and application thereof
By using polyurethane resin and other additives in conductive silver paste, combined with grinding and filtration processes, the problem of refined and large-scale production of conductive paste in screen printing is solved, and efficient printing performance and photoelectric conversion efficiency are achieved. .
Patent Information
- Application Number
- CN202210150139.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-02-18
AI Technical Summary
Existing conductive pastes are difficult to achieve refined and large-scale mass production in screen printing, especially when the line width is less than 20μm, the problem of serrated, broken wires, and uneven line widths of the whole plate are prone to occur, and the material utilization rate is low, and the process is Complex and costly.
Conductive silver paste containing polyurethane resin, thixotropic agent, dispersant and solvent is used to form urea bonds through the adsorption reaction of the urethane structure of polyurethane resin and the adsorption substrate, thereby improving the thixotropic properties and rheological properties of the paste. , combined with the three-roller grinding and filtration process, conductive silver paste with excellent printing and shaping was prepared.
It significantly improves the printing performance of silver paste, reduces the printing line width, optimizes the line shape, improves the photoelectric conversion efficiency, and solves the limitations of screen printing fineness and large-scale processing, realizing the industrialization and scale of solar cells. Production.
Smart Images

Figure CN114582544B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cell pastes, and in particular relates to a conductive paste with excellent printing performance, a preparation method and application thereof. Background Art
[0002] With the depletion of fossil energy, energy issues have become a limiting factor affecting human survival and development. Solar cells, as one of the ways to utilize solar energy, are expected to become an important way for humans to obtain energy needs in the long run. Conductive paste, as a material for metallization of the front of silicon solar cells, is mainly composed of conductive functional phase silver powder, bonding phase glass powder and organic carrier. The organic carrier is generally composed of solvents, thixotropic agents, dispersants and other functional additives. Its main function is to disperse and wet the powder particles in the conductive paste, so that the paste has good fluidity and printing processability. Functional additives are trace substances added according to process requirements and product modifications. They have a vital impact on the manufacturing process, performance (such as printing processability) of the conductive paste and the photoelectric conversion efficiency of solar cells. It is also one of the core technologies of each manufacturer.
[0003] For the paste, it is not just a simple mixture of the three, but a complex system. Different formulas of organic carriers have different viscosities, leveling and thixotropy, which affect the viscosity, leveling and thixotropy of the paste, and then affect the printing performance and plasticity of the paste, and finally affect the photoelectric conversion efficiency of solar cells. Therefore, obtaining a better organic carrier formula is one of the keys to making high-quality conductive paste. Therefore, although the content of organic carrier in solar conductive paste is very small, its role is irreplaceable, and the selection and ratio of its composition and various functional additives are particularly important.
[0004] In solar cells, the common methods for making electrodes are screen printing and photolithography. Photolithography can be refined to obtain high-quality electrode images, but this method has disadvantages such as low material utilization, complex process, and large usage. The screen printing process is simple, with high material utilization and low cost, and is very suitable for mass production. However, when faced with refined processing (such as line width less than 20μm), it is prone to serration, line breakage, and uneven line width across the entire plate. In addition, in large-scale production processes, the stretching of the screen mask during printing may cause deformation of the pattern and poor printing shaping. In order to break through the limitations of fine processing of screen printing, it is urgent to develop a conductive paste with excellent printing shaping. Summary of the invention
[0005] In order to solve the problems existing in the above-mentioned prior art, the present invention provides a conductive paste with excellent printing and shaping properties to meet the needs of refined and large-scale mass production.
[0006] In a first aspect, the present invention discloses a conductive silver paste, which adopts the following technical solution:
[0007] Conductive paste, raw material components include silver powder, glass powder and organic carrier, the organic carrier includes polyurethane resin, thixotropic agent, dispersant, solvent,
[0008] Among them, the mass percentage of each raw material is:
[0009] Silver powder 88-92%, glass powder 2-5%, polyurethane resin 0.1-1%, solvent 0.8-9.7%, thixotropic agent 0.1-0.6%, dispersant 0.1-0.6%.
[0010] Among them, the main function of the organic carrier is to disperse and wet the powder particles in the conductive paste, so that the paste has good fluidity and printing processability.
[0011] In certain embodiments, the polyurethane resin comprises a urethane structure.
[0012] In certain embodiments, the polyurethane resin is obtained by reacting an isocyanate compound with an active hydrogen compound.
[0013] In certain embodiments, the isocyanate compound is at least one of diphenylmethane diisocyanate (MDI) and toluene diisocyanate (TDI).
[0014] In certain embodiments, the active hydrogen compound is at least one of an alcohol, water, an amine, an alcoholamine, a phenol, a thiol, a carboxylic acid, and a urea.
[0015] In certain embodiments, the average molecular weight of the polyurethane resin is 20,000 to 80,000.
[0016] In certain embodiments, the polyurethane resin has a coating-4 cup viscosity of 40 to 80 seconds.
[0017] The test condition of the polyurethane resin coating-4 cup viscosity is carried out at a constant temperature of 25±1℃.
[0018] In certain embodiments, the thixotropic agent is at least one of modified hydrogenated castor oil and polyamide wax.
[0019] Among them, the thixotropic agent can make the slurry have better thixotropy, so that the slurry can maintain a good shape after printing.
[0020] In certain embodiments, the dispersant is at least one of a quaternary ammonium salt type cationic surfactant, a polyether modified copolymer, a higher fatty acid, BYK180, and Digo 655.
[0021] Among them, dispersants can improve the anti-sedimentation, stability and fluidity of the slurry.
[0022] In certain embodiments, the quaternary ammonium salt type cationic surfactant is at least one of dodecyltrimethylammonium chloride and hexadecyltrimethylammonium bromide.
[0023] In certain embodiments, the polyether-modified copolymer is at least one of polyether-modified polysiloxane and polyether-modified aminosilicone oil.
[0024] In certain embodiments, the higher fatty acid is at least one of palmitic acid (also known as palmitic acid), pearlitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, arachidic acid, behenic acid, and lignin acid.
[0025] In certain embodiments, the solvent is at least one of terpineol, butyl carbitol, diethyl phthalate, terpene glycol-12, butyl carbitol acetate, dimethyl adipate, dimethyl glutarate, ethylene glycol, phenyl ether, and tributyl citrate.
[0026] Among them, the solvent controls the volatilization rate of the slurry, allowing the carrier to volatilize in layers during the high-temperature sintering process, preventing uneven holes from appearing on the surface of the grid line and cracks that may be generated by concentrated volatilization.
[0027] In a second aspect, the present invention discloses a method for preparing a conductive silver paste:
[0028] The polyurethane resin, thixotropic agent, dispersant and solvent are fully mixed to obtain an organic carrier; the silver powder and glass powder are pre-mixed uniformly, and the organic carrier is added to the mixture of the silver powder and the glass powder according to the principle of equal and incremental amounts, and the mixture is fully mixed, and then the mixture is ground and filtered through a three-roll mill to obtain a conductive silver paste.
[0029] In a third aspect, the present invention discloses the application of the above conductive paste in solar cells.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) At present, polyurethane resin is basically used in low-temperature curing pastes, and there has never been a report on the use of polyurethane resin in high-temperature sintering pastes. The present invention creatively uses polyurethane resin as an important component of the sintering paste. On the one hand, the paste has excellent thixotropic properties and rheological properties, which has the effects of improving the printing performance of the paste, reducing the printing line width of the silver conductive layer, and optimizing the line shape. In addition, when the polyurethane resin containing carbamate groups (-NH-COO-) in the present invention is used, the -NCO groups contained in it react with the adsorbed water on the surface of the attached substrate to form urea bonds, and are firmly bonded to the attached substrate through hydrogen bonds.
[0032] (2) The organic carrier component provided by the present invention has a reasonable formula, which helps to improve the rheological properties of the slurry system. After being mixed and dispersed into the silver paste in a certain proportion, it can significantly improve the linear shaping ability of the gate line, thereby improving the silk screen printing quality of the silver paste on the silicon wafer and the aspect ratio of the electrode and the gate line after sintering. In addition, the line width after printing is narrow and the gate break ratio is low, which can effectively improve the photoelectric conversion efficiency.
[0033] (3) The conductive paste of the present invention has excellent printing performance, which can solve the limitations of screen printing refinement (line width less than 20 μm) and mass processing and production, and is conducive to the industrialization and large-scale production of solar cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a top view of the silver conductive layer after printing in Example 3;
[0035] Figure 2 It is a top view of the silver conductive layer after printing in Comparative Example 1;
[0036] Figure 3 This is a three-dimensional view of the silver conductive layer after printing in Example 3;
[0037] Figure 4 This is a three-dimensional view of the silver conductive layer after printing in Comparative Example 1. DETAILED DESCRIPTION
[0038] The specific implementation modes of the present invention are further described in detail below in conjunction with the embodiments.
[0039] The silver powder used in the following embodiments can be selected from various silver powders known to those skilled in the art, for example, XT-Ag-04 produced by Shanghai Xiangtian Nanomaterials Co., Ltd.; the glass powder can be selected from various glass powders known to those skilled in the art, for example, lead tellurium bismuth series glass powder of DuPont can be selected; the polyurethane resin can be selected from TS-8810 produced by Yantai Chemical Co., Ltd.
[0040] Example 1
[0041] According to the mass fraction, 0.1 parts of polyurethane resin, 0.3 parts of modified hydrogenated castor oil, 0.3 parts of alkyl ammonium salt type cationic surfactant and 7.3 parts of butyl carbitol are fully mixed to obtain an organic carrier; 90 parts of silver powder and 2 parts of glass powder are pre-mixed evenly, and then the organic carrier is added to the mixture of silver powder and glass powder according to the principle of equal amount increment. Stir evenly after each addition, add the next time, stir evenly at high speed after all are added, and finally grind the mixture with a three-roll mill to a particle size of less than 6μm, filter, and obtain a conductive silver paste.
[0042] Example 2
[0043] According to the mass fraction, 1.0 part of polyurethane resin, 0.3 part of polyamide wax, 0.3 part of BYK180 and 6.4 parts of alcohol ester-12 were fully mixed to obtain an organic vehicle; 90 parts of silver powder and 2 glass powder were pre-mixed evenly, and then the organic vehicle was added to the mixture of silver powder and glass powder according to the principle of equal increments. Stir evenly after each addition, add the next time, stir evenly at high speed after all additions are completed, and finally grind the mixture with a three-roll mill to a particle size of less than 6μm, filter, and obtain a conductive silver paste.
[0044] Example 3
[0045] According to the mass fraction, 0.4 parts of polyurethane resin, 0.3 parts of polyamide wax, 0.3 parts of Digo 655 and 7.0 parts of diethyl phthalate were fully mixed to obtain an organic carrier; 92 parts of silver powder and 2 parts of glass powder were pre-mixed evenly, and then the organic carrier was added to the mixture of silver powder and glass powder according to the principle of equal increments. Stir evenly after each addition, add the next time, stir evenly at high speed after all additions are completed, and finally grind the mixture with a three-roll mill to a particle size of less than 6μm, filter, and obtain a conductive silver paste.
[0046] Example 4
[0047] According to the mass fraction, 0.7 parts of polyurethane resin, 0.3 parts of thixotropic agent (modified hydrogenated castor oil: polyamide wax = 1:1), 0.3 parts of dispersant (BYK180: Digo 655 = 1:1) and 7.0 parts of solvent (pinene alcohol: butyl carbitol = 1:1) are fully mixed to obtain an organic vehicle; 90 parts of silver powder and 2 parts of glass powder are pre-mixed evenly, and then the organic vehicle is added to the mixture of silver powder and glass powder according to the principle of equal increments. Stir evenly after each addition, add the next time, stir evenly at high speed after all are added, and finally grind the mixture with a three-roll mill to a particle size of less than 6μm, filter, and obtain a conductive silver paste.
[0048] Example 5
[0049] According to the mass fraction, 0.8 parts of polyurethane resin, 0.6 parts of polyamide wax, 0.6 parts of BYK180 and 5 parts of ethylene glycol were fully mixed to obtain an organic vehicle; 88 parts of silver powder and 5 parts of glass powder were pre-mixed evenly, and then the organic vehicle was added to the mixture of silver powder and glass powder according to the principle of equal increments. Stir evenly after each addition, add the next time, stir evenly at high speed after all additions are completed, and finally grind the mixture with a three-roll mill to a particle size of less than 6μm, filter, and obtain a conductive silver paste.
[0050] Example 6
[0051] According to the mass fraction, 1 part of polyurethane resin, 0.1 part of polyamide wax, 0.1 part of Digo 655 and 3.8 parts of dimethyl glutarate are fully mixed to obtain an organic vehicle; 92 parts of silver powder and 3 parts of glass powder are pre-mixed evenly, and then the organic vehicle is added to the mixture of silver powder and glass powder according to the principle of equal increments. Stir evenly after each addition, add the next time, stir evenly at high speed after all additions are completed, and finally grind the mixture with a three-roll mill to a particle size of less than 6μm, filter, and obtain a conductive silver paste.
[0052] Comparative Example 1
[0053] According to the mass fraction, 0.4 parts of phenolic epoxy resin, 0.3 parts of polyamide wax, 0.3 parts of Digo 655 and 7.0 parts of diethyl phthalate are fully mixed to obtain an organic carrier; 92 parts of silver powder and 2 parts of glass powder are pre-mixed evenly, and then the organic carrier is added to the mixture of silver powder and glass powder according to the principle of equal increments. Stir evenly after each addition, add the next time, stir evenly at high speed after all additions are completed, and finally grind the mixture with a three-roll mill to a particle size of less than 6μm, filter, and obtain a conductive silver paste.
[0054] Comparative Example 2
[0055] According to the mass fraction, 0.05 parts of hydroxylated acrylic resin, 0.3 parts of modified hydrogenated castor oil, 0.3 parts of alkyl ammonium salt type cationic surfactant and 7.35 parts of butyl carbitol were fully mixed to obtain an organic carrier; 90 parts of silver powder and 2 parts of glass powder were pre-mixed evenly, and then the organic carrier was added to the mixture of silver powder and glass powder according to the principle of equal increments. Stir evenly after each addition, add the next time, stir evenly at high speed after all additions are completed, and finally grind the mixture with a three-roll mill to a particle size of less than 6 μm, filter, and obtain a conductive silver paste.
[0056] Comparative Example 3
[0057] According to the mass fraction, 1.05 parts of saturated polyester resin, 0.3 parts of polyamide wax, 0.3 parts of BYK180 and 6.35 parts of alcohol ester-12 are fully mixed to obtain an organic vehicle; 90 parts of silver powder and 2 glass powders are pre-mixed evenly, and then the organic vehicle is added to the mixture of silver powder and glass powder according to the principle of equal increments. Stir evenly after each addition, add the next time, stir evenly at high speed after all are added, and finally grind the mixture with a three-roll mill to a particle size of less than 6μm, filter, and obtain a conductive silver paste.
[0058] The proportions of raw material components in each embodiment and comparative example are shown in Table 1 below:
[0059] Table 1 Ratio of raw material components in Examples and Comparative Examples
[0060]
[0061] Performance Testing:
[0062] The prepared silver pastes of the embodiments and comparative examples were subjected to performance tests, and conventional screen printing was performed on a screen printer to produce solar cells. The performance test data of each embodiment and comparative example are shown in Table 2 below:
[0063] Table 2 Performance test data of embodiments and comparative examples
[0064]
[0065] Among them, the post-printing line width is the line width after printing when the designed screen is 18μm; the broken grid ratio is the number of broken grids on a photovoltaic cell.
[0066] At present, the printability and aspect ratio of the paste are mainly determined by the organic carrier. If you want to pursue a very good aspect ratio, you can add thixotropic agents, surfactants or other functional additives to increase the viscosity and thixotropic index, but this method also has certain problems. If the type of functional additives is not properly selected, it will have a great impact on the body of the paste, causing problems such as solvent expansion and centipede feet. When using thixotropic agents, surfactants and other additives to improve the thixotropic properties of the paste, although the shaping of the paste can be significantly improved, the working principle of these chemical substances is usually to increase the thixotropic index by forming a stronger spatial network structure, and the viscosity of silver paste is often unstable.
[0067] The present invention adopts a polyurethane resin containing a carbamate group as an important component of the mechanical carrier, so that the slurry has excellent thixotropic properties and rheological properties, and has the effects of improving the printing performance of the slurry, reducing the printing line width of the silver conductive layer, and optimizing the line shape.
[0068] It can be seen from the data in the above table that the only difference between Example 3 and Comparative Example 1 is the resin used. Compared with Example 3, the line width of Comparative Example 1 decreases by 10 μm and the photoelectric conversion efficiency increases by 0.05-0.1% (for every 2 μm decrease, the photoelectric conversion efficiency increases by 0.01-0.02%).
[0069] The formula of the present invention can improve the plasticity of the slurry, so that the slurry has more three-dimensional and fuller lines. The electrode grid lines prepared in this embodiment are of high quality, the upper surface of the lines is relatively flat, the edges are neat, and the line shape is better. Figure 1 , Figure 3 And the comparative example 1 Figure 2 , Figure 4 In addition, the slurry of the present invention can achieve good printing when printed on an 18 μm screen, and the line width after printing is narrow, the broken grid ratio is low, and the aspect ratio of the electrode grid line is significantly better than that of comparative example 1, and the photoelectric conversion efficiency can be effectively improved.
[0070] In summary, the organic carrier component provided by the present invention has a reasonable formula, which helps to improve the rheological properties of the slurry system, maintain the line width, prevent line diffusion and collapse, and make the upper edge of the line smooth and the line shape good, so that it has good application performance in high-precision crystalline silicon solar front silver paste and can realize refined printing and large-scale production.
[0071] The above description is only a preferred embodiment of the present invention. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the creative concept of the present invention, and these should also be regarded as within the scope of protection of the invention.
Claims
1. Conductive paste, characterized in that: The raw material components include silver powder, glass powder and organic carrier. The organic carrier includes polyurethane resin, thixotropic agent, dispersant and solvent. Among them, the mass percentage of each raw material is: Silver powder 88~92%, glass powder 2~5%, polyurethane resin 0.1~1%, solvent 0.8~9.7%, thixotropic agent 0.1~0.6%, dispersant 0.1~0.6%; The polyurethane resin contains a carbamate structure, the average molecular weight of the polyurethane resin is 20000-80000, and the coating-4 cup viscosity is 40-80s; The solvent is at least one of terpineol, butyl carbitol, diethyl phthalate, alcohol ester-12, butyl carbitol acetate, dimethyl adipate, dimethyl glutarate, ethylene glycol, phenyl ether and tributyl citrate; the thixotropic agent is at least one of modified hydrogenated castor oil and polyamide wax; the dispersant is at least one of quaternary ammonium salt cationic surfactant, BYK180 and Digo 655; The preparation method of the above conductive paste is: The polyurethane resin, thixotropic agent, dispersant and solvent are fully mixed to obtain an organic carrier; the silver powder and glass powder are pre-mixed uniformly, and the organic carrier is added to the mixture of the silver powder and the glass powder according to the principle of equal and incremental amounts, and the mixture is fully mixed, and then the mixture is ground and filtered through a three-roll mill to obtain a conductive silver paste.
2. The conductive paste according to claim 1, characterized in that: The polyurethane resin is obtained by reacting an isocyanate compound with an active hydrogen compound.
3. The conductive paste according to claim 2, characterized in that: The isocyanate compound is at least one of diphenylmethane diisocyanate and toluene diisocyanate, and the active hydrogen compound is at least one of alcohol, water, amine, alcoholamine, phenol, thiol, carboxylic acid, and urea.
4. Use of the conductive paste according to any one of claims 1 to 3 in a solar cell.