Method for preparing pelletized ore and binder, and pelletized ore prepared by using the same
The binder is prepared by mixing the slag produced in the ferronickel preparation process and the slag produced in the carbon steel molten steel preparation process with flying dust, and by adding Na-based flux, the problems of high cost and insufficient strength of pellets are solved. It realizes the preparation of low-cost and high-strength pellets, reducing the usage of high-priced nickel ore and inventory management costs.
Patent Information
- Application Number
- CN202080053276.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-08-26
AI Technical Summary
The high-priced inorganic binders used to prepare pellets in the prior art lead to high costs, and the dust generated in the ferronickel preparation process is insufficient in strength when reused, resulting in an increase in dust generation and affecting process efficiency.
The slag produced in the ferronickel preparation process and the slag produced in the carbon steel molten steel preparation process are mixed with industrial by-product flying dust to prepare a binder containing silicon oxide, calcium oxide, aluminum oxide and iron oxide, and by controlling the proportion of ingredients And add Na-based flux to improve the strength and granulation of pellets.
It reduces the cost of pellet preparation, ensures the strength of pellets, reduces the use of high-priced nickel ore, saves the inventory management cost of small particle desulfurization slag, and improves process efficiency.
Smart Images

Figure CN114585755B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a pellet and a binder, and a pellet prepared by using the same. More specifically, the present invention relates to a method for preparing a pellet and a binder, which can reduce the cost of preparing the pellet, and a pellet prepared by using the same. Background Art
[0002] Molten steel used to make stainless steel is generally produced through a refining process in which solid ferronickel, ferrochrome and scrap iron are melted to produce molten iron containing nickel and chromium, and carbon is removed from the produced molten iron.
[0003] The process of preparing nickel iron includes: a process of drying nickel-containing ore (hereinafter referred to as nickel ore), a process of roasting and pre-reducing the dried nickel ore, a process of charging the roasted and pre-reduced nickel ore into an electric furnace for melting and reduction, a desulfurization process of removing sulfur (S) from the melt, and a process of preparing the desulfurized melt into a solid form.
[0004] On the other hand, gases are generated in the process of drying the nickel ore, the process of roasting and pre-reducing, and the process of melting and reducing, respectively, and the generated gases are discharged to the outside of each device.
[0005] The gas discharged to the outside (hereinafter referred to as exhaust gas) contains solid particulate dust. In addition, the dust contains a high content of nickel oxide (NiO).
[0006] Therefore, the dust is reused as a source material for preparing ferronickel. At this time, when the recovered dust is reused, the dust is prepared into pellets having a predetermined particle size or more, and the prepared pellets are added to the process of roasting and pre-reducing the nickel ore for reuse.
[0007] On the other hand, when the strength of the pellets is weak, the pellets may be re-powdered due to wear or crushing during transportation or roasting and pre-reduction processes. Therefore, a large amount of dust may be generated during roasting and pre-reduction processes.
[0008] Therefore, when the dust is molded into pellets, a binder for improving strength is added together for preparation. However, since an expensive inorganic binder is used as the binder, there is a problem that the cost for preparing the pellets is high.
[0009] Prior Art Literature
[0010] Patent Document 1: Korean Authorized Patent KR0942109 Summary of the invention
[0011] Technical issues
[0012] The present invention relates to a method for preparing pellets and a binder, which can reduce the cost of preparing pellets, and pellets prepared by using the method.
[0013] The invention relates to a method for preparing a pellet and a binder capable of recycling slag produced in a nickel-iron preparation process, and a pellet prepared by using the method.
[0014] Technical Solution
[0015] The method for preparing pellets according to an embodiment of the present invention includes: a process of recovering dust generated in the nickel-iron preparation process for later use; a process of preparing a binder using a first slag as slag generated in the nickel-iron preparation process and by-products generated in processes other than the nickel-iron preparation process; and a process of mixing and granulating the dust and the binder to prepare pellets.
[0016] The by-products include secondary slag, which is slag generated in the preparation of molten steel for preparing carbon steel, and fly ash.
[0017] The dust recovery process is used to recover dust generated in at least one of the following processes: in the nickel-iron preparation process, a drying process for drying nickel ore; a roasting and pre-reduction process for heating the nickel ore for roasting and pre-reduction; a melting and reduction process for heating the nickel ore to generate a melt and reducing the nickel ore.
[0018] The first slag contains 3.0 wt % to 5.0 wt % of nickel oxide (NiO).
[0019] The first slag is slag recovered and reserved from slag generated in a desulfurization process for removing sulfur (S) from the melt.
[0020] The second slag is slag obtained by recycling slag generated in a refining process in which the carbon (C) in molten steel is reduced to 1 wt % or less.
[0021] The method includes the following process: controlling the mixing amount of the first slag, the second slag and fly ash so that the total amount of the binder contains 30% to 50% by weight of silicon oxide (SiO2), 15% to 25% by weight of calcium oxide (CaO), 10% to 20% by weight of aluminum oxide (Al2O3), and 10% to 20% by weight of iron oxide (FeO).
[0022] When preparing the binder, a Na-based flux may be further mixed.
[0023] The Na-based flux may include Na2CO3.
[0024] The method includes at least one of the following processes: a process of crushing the first slag, the second slag and the fly ash separately before mixing them; and a process of crushing the first mixture mixed with the first slag, the second slag and the fly ash.
[0025] The process of preparing pellets includes the process of mixing the dust, a binder and water, wherein the mixture contains 65 to 85 weight % of the dust, 5 to 15 weight % of the binder and 10 to 20 weight % of the water, relative to the total weight % of the second mixture of the dust, the binder and the water.
[0026] The method for preparing a binder for preparing pelletized ore according to an embodiment of the present invention includes: a process of preparing a first slag as a slag produced in a nickel-iron preparation process; a process of preparing a second slag as a slag produced in a molten steel preparation process for preparing carbon steel; a process of preparing industrial by-product fly ash; and a process of mixing the first slag, the second slag and the fly ash to prepare a binder.
[0027] The first slag is a slag containing 3.0 wt % to 5.0 wt % of nickel oxide (NiO), and the second slag is a slag recovered and reserved from slag generated in a refining process in which the carbon (C) in molten steel is reduced to 1 wt % or less.
[0028] The first slag is slag prepared by recovering slag generated in a desulfurization process for removing sulfur (S) from the melt, and the first slag is slag prepared by recovering slag having a particle size of less than 1 mm from the slag generated in the desulfurization process.
[0029] The method includes the following process: controlling the mixing amount of the first slag, the second slag and fly ash so that the total amount of binder contains 30% to 50% by weight of silicon oxide (SiO2), 15% to 25% by weight of calcium oxide (CaO), 10% to 20% by weight of aluminum oxide (Al2O3), and 10% to 20% by weight of iron oxide (FeO); in the process of controlling the mixing amount of the first slag, the second slag and fly ash, relative to the total weight of the first mixture of the first slag, the second slag and fly ash, the mixture contains 10% to 30% by weight of the first slag, 10% to 30% by weight of the second slag, and 40% to 60% by weight of fly ash.
[0030] The process of preparing the binder also includes a process of mixing a Na-based flux, wherein the mixture contains 10 weight % to 30 weight % of the first slag, 10 weight % to 30 weight % of the second slag, 40 weight % to 60 weight % of the fly ash, and 3 weight % to 15 weight % of the Na-based flux, relative to the total weight % of the first mixture comprising the first slag, the second slag, the fly ash, and the Na-based flux.
[0031] The Na-based flux may include Na2CO3.
[0032] The pellets according to the embodiment of the present invention include dust generated in the ferronickel manufacturing process and a binder including first slag which is slag generated in the ferronickel manufacturing process.
[0033] The binder includes: second slag which is slag generated in the preparation of molten steel for preparing carbon steel; and fly ash which is an industrial by-product.
[0034] The first slag contains 3.0 wt % to 5.0 wt % of nickel oxide (NiO).
[0035] In the total amount of the binder, the binder comprises 30 wt % to 50 wt % silicon oxide (SiO2), 15 wt % to 25 wt % calcium oxide (CaO), 10 wt % to 20 wt % aluminum oxide (Al2O3), and 10 wt % to 20 wt % iron oxide (FeO).
[0036] The particle size of the pellets can be from 15mm to 20mm.
[0037] The pellet residue rate can be 94% to 99.5%, and the drop residue rate can be 92% to 95%.
[0038] The compressive strength of the pellets can be between 1.8 kgf and 2.1 kgf.
[0039] Effects of the Invention
[0040] In an embodiment of the present invention, the slag produced in the desulfurization process of the nickel iron preparation process, the slag produced in the molten steel preparation process for preparing carbon steel, and the industrial byproduct flay ash are reused to prepare the binder. Therefore, compared with the prior art, the binder can be prepared at low cost. In addition, when the raw material pellets for preparing nickel iron are prepared using the binder according to the embodiment, pellets with strength similar to or improved by the pellets prepared using the existing binder can be prepared.
[0041] Therefore, according to the embodiments of the present invention, the cost for preparing pellets can be reduced while ensuring the strength of the pellets.
[0042] In addition, since the small-particle desulfurization slag produced in the desulfurization process of the nickel-iron preparation process is reused to prepare the binder, the inventory management cost of the small-particle desulfurization slag that cannot be reused in the existing prior art can be saved.
[0043] In addition, the small-particle desulfurized slag contains nickel (Ni), which is reused as a raw material of a binder to prepare pellets, so the binder plays the role of a source material for preparing nickel iron or for providing nickel (Ni).
[0044] Therefore, the usage of the main raw material for preparing ferronickel and the high-priced nickel ore for providing the source material of nickel (Ni) can be reduced, thereby reducing the cost required for preparing ferronickel. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 1 is a flow chart sequentially showing a method for preparing pellets according to a first embodiment of the present invention.
[0046] Figure 2 are views sequentially showing a conventional ferronickel production method.
[0047] Figure 3 is a graph showing the nickel oxide (NiO) content based on the particle size of slag, wherein the slag is slag generated by a desulfurization process in a nickel-iron manufacturing process.
[0048] Figure 4 1 is a flow chart sequentially showing a method for preparing pellets according to a second embodiment of the present invention.
[0049] Figure 5 The table shows the residual rate (%), drop residual rate (%), compression strength (kgf), and shape of the pellets prepared by the methods according to the first and second comparative examples and the first and second embodiments. DETAILED DESCRIPTION
[0050] Hereinafter, the embodiments of the present invention will be described in further detail with reference to the accompanying drawings. However, the present invention can be implemented in various ways and is not limited to the embodiments disclosed below. The purpose of providing the present embodiments below is to fully disclose the present invention so that ordinary technicians can fully understand the scope of the invention. In order to describe the embodiments of the present invention, the accompanying drawings may be enlarged, and the same reference numerals in the accompanying drawings represent the same components.
[0051] The present invention relates to a method for preparing a pellet and a binder, which can reduce the cost of preparing a pellet and can reuse the slag generated in the nickel-iron preparation process. More specifically, the present invention relates to a method for preparing a pellet and a binder, which can ensure strength and reduce the preparation cost when preparing a pellet used as a raw material in the nickel-iron preparation.
[0052] Figure 1 1 is a flow chart sequentially showing a method for preparing pellets according to a first embodiment of the present invention. Figure 2 are views sequentially showing a conventional ferronickel production method. Figure 3 is a graph showing the nickel oxide (NiO) content based on the particle size of slag, wherein the slag is slag generated by a desulfurization process in a nickel-iron manufacturing process.
[0053] See also Figure 1 According to the first embodiment of the present invention, the method for preparing pellets S100 includes: a process S110 of preparing dust generated in the nickel-iron preparation process, a process S120 of preparing a binder, and a process S130 of mixing and granulating the dust and the binder to prepare pellets.
[0054] The adhesive is an adhesive prepared by the method according to the first embodiment.
[0055] The process of preparing a binder according to the first embodiment includes a process of preparing slag (first slag) produced in a nickel-iron preparation process, a process of preparing a by-product produced in a process other than the nickel-iron preparation process, a process of mixing the first slag and the binder, and a process of preparing a binder using the mixture of the first slag and the by-product.
[0056] The by-products mixed with the first slag may include slag (second slag) generated in a molten steel manufacturing process for manufacturing carbon steel and flay ash which is an industrial by-product.
[0057] In the following, reference is made to Figure 1 When describing the method for preparing the binder according to the first embodiment, it is described by taking as an example that the by-products mixed with the first slag are the second slag and flay ash generated in the molten steel preparation process for preparing carbon steel.
[0058] See also Figure 1 According to the first embodiment, the process S120 of preparing a binder includes a process S121 of preparing a first slag as slag produced in a nickel-iron preparation process, a process S122 of preparing a second slag as slag produced in a molten steel preparation process for preparing carbon steel, a process S123 of preparing industrial by-product flayat (flay ash), a process S124 of mixing the first and second slags and the flayat, and a process S125 of preparing a binder using the mixture of the first and second slags and the flayat.
[0059] In the present invention, when preparing pellets, as described above, the dust generated in the nickel-iron preparation process is reused.
[0060] Hereinafter, before describing in detail the method for preparing pellets according to the first embodiment, the method for preparing ferronickel will be described first.
[0061] See also Figure 2 The method for preparing ferronickel includes a process S10 of drying nickel ore, a process S20 of roasting and reducing the dried nickel ore, a process S30 of melting and reducing the roasted and reduced nickel ore to prepare a ferronickel melt (hereinafter referred to as the melt), and a desulfurization process S40 of removing sulfur (S) from the melt.
[0062] As a source material for preparing ferronickel or for providing nickel (Ni) and iron (Fe), nickel ore is an ore containing nickel oxide (NiO), calcium oxide (CaO), silicon oxide (SiO2), aluminum oxide (Al2O3), and iron oxide (FeO), and can be an ore containing 1.5% to 2% by weight of the nickel oxide (NiO). In addition, in addition to the above-mentioned components, the nickel ore can also contain manganese oxide (MnO), phosphorus pentoxide (P2O5), magnesium oxide (MgO), titanium oxide (TiO2), carbon (C), and sulfur (S). For this nickel ore, for example, it can be saprolite. More specifically, the nickel ore can have a component as shown in an example of Table 1 below.
[0063]
Table 1
[0064]
[0065] In the process S10 of drying the nickel ore, the water contained in the nickel ore is removed. At this time, the drying device for drying the nickel ore may be, for example, a rotary dryer having a rotatable drum and a material to be processed loaded therein.
[0066] In the method of drying using a rotary dryer, the nickel ore is placed inside a drum, and the inside of the drum is heated while rotating the drum, for example, to a temperature of 200° C. Thus, moisture is removed from the nickel ore placed inside the drum.
[0067] When heating the drum of the rotary dryer, for example, a method of sending hot air into the drum can be adopted. Of course, the method of heating the inside of the drum is not limited to the above example, and various methods can be adopted. In addition, the drying device for drying the nickel ore is not limited to the above rotary dryer, and various devices that can remove moisture from the nickel ore can be adopted.
[0068] In the roasting and reducing process S20, the nickel ore is heat-treated and roasted to increase its strength, and metal oxides such as nickel oxide (NiO) and iron oxide (FeO) contained in the nickel ore are reduced to nickel (Ni) and iron (Fe).
[0069] An apparatus for roasting and reducing nickel ore (hereinafter referred to as a roasting apparatus) may be, for example, a rotary kiln having a rotatable drum and a burner for generating flames inside the drum.
[0070] In the method of roasting and reducing nickel ore using a rotary kiln, nickel ore and a carbonaceous (C) reducing agent such as coal are loaded into the drum, and the drum is rotated while heating the inside. At this time, fuel gas is supplied to a burner, and flames are generated inside the drum by the burner to heat the inside of the drum to a temperature of 600° C. to 800° C.
[0071] In this way, when the inside of the drum is heated to a temperature of 600° C. to 800° C., the nickel ore is roasted, its strength is increased, and metal oxides such as nickel oxide (NiO) and iron oxide (FeO) contained in the nickel ore are reduced.
[0072] The above describes a method of generating flames by a burner when heating the inside of the drum of the rotary kiln, but it is not limited to this, and various heating methods that can heat the inside of the drum to a temperature of 600° C. to 800° C. can be used. In addition, the roasting device for roasting and reducing the nickel ore is not limited to the above-mentioned rotary kiln, and various devices that can roast and reduce the nickel ore can be used.
[0073] On the other hand, in this process S20, when the nickel ore is heated, it is easy to heat to the target temperature in the melting and reduction process S30 of the nickel ore as a subsequent operation. In addition, in the roasting and reduction process S20, the nickel ore is heated to a temperature of 600° C. to 800° C. as described above to reduce the metal oxide, which is lower than the temperature (1200° C. or more) in the melting and reduction process S30 as a subsequent operation. Therefore, in the roasting and reduction process S20, the amount of the reduced metal oxide is less than that in the melting and reduction process S30.
[0074] Therefore, the reduction occurring in the roasting and reducing process S20 can be described as a reduction performed in advance or in preparation of the reduction in the melting and reducing process S30. Therefore, the roasting and reducing process S20 performed before the melting and reducing process S30 is generally named as the roasting and pre-reducing process S20. More specifically, the roasting and reducing process S20 performed in the rotary kiln can be named as the roasting and pre-reducing process S20.
[0075] In the melting and reducing process S40, the nickel ore is melted so that metal oxides such as nickel oxide (NiO) and iron oxide (FeO) contained in the nickel ore are reduced. At this time, an electric furnace can be used when the nickel ore is melted and reduced. The electric furnace can be configured to include a main body having an internal space and an electrode rod for generating an arc as a heat source into the main body.
[0076] In the method of melting and reducing nickel ore in an electric furnace, first, nickel ore and a reducing agent containing carbon (C) are added to the interior of the main body of the electric furnace. The reducing agent may be, for example, coal. When the nickel ore and the reducing agent are loaded into the main body, an arc is generated into the interior of the main body through an electrode rod. At this time, the nickel ore and the reducing agent are melted by the arc heat, and the nickel ore is reduced, thereby preparing a melt, i.e., a nickel-iron melt.
[0077] On the other hand, the melt prepared in the electric furnace contains about 4000 ppm of sulfur (S), which is a factor that reduces the quality of products such as stainless steel. Therefore, when the melt is prepared in the electric furnace, desulfurization S40 for removing sulfur (S) from the melt is performed, and at this time, (S) needs to be controlled to 600 ppm or less.
[0078] Desulfurization for removing sulfur (S) from a melt can be carried out using, for example, a KR (Kanvara Reactor) device. The KR device may be a device including a rotatable impeller immersed in a melt contained in a ladle.
[0079] The desulfurization operation in the KR device can be performed as follows. When the melt prepared in the electric furnace is charged into a ladle, an impeller is immersed in the melt in the ladle. Then, the impeller immersed in the melt is rotated while a desulfurizing agent such as calcium oxide (CaO) is added to the melt.
[0080] When a desulfurizing agent is added to the melt, CaS is generated by a reaction between sulfur (S) in the melt and the desulfurizing agent, and the generated CaS enters the slag suspended on the surface of the melt. Thus, sulfur (S) is removed from the melt, and a nickel-iron melt having a sulfur (S) content of 600 ppm or less is prepared.
[0081] On the other hand, in the process for preparing ferronickel as described above, gas is generated in the drying process S10, the roasting and pre-reduction process S20, and the melting and reduction process S30, respectively, and the gas is discharged to the outside of the device. That is, gas is generated in the drying device for drying nickel ore, the roasting device for roasting and pre-reducing nickel ore, and the electric furnace for melting and reduction, respectively, and the generated gas is discharged to the outside of each device.
[0082] The gas discharged to the outside (hereinafter referred to as exhaust gas) contains solid particulate dust. In addition, the dust contains nickel oxide (NiO) with a content similar to that of nickel ore.
[0083] Therefore, the dust generated in the preparation of ferronickel is reused as a source material for preparing ferronickel or for providing nickel (Ni). That is, dust is recovered from the exhaust gas discharged from the drying device, roasting device and electric furnace, and the recovered dust is reused as a source material together with nickel ore.
[0084] To this end, dust is recovered by respectively arranging exhaust gas treatment devices for collecting dust in the exhaust gas on the drying device, the roasting device and the electric furnace.
[0085] For example, the exhaust gas treatment device may include a pipe through which gas passes, a driving unit for generating a suction force to draw the gas into the pipe, a filter arranged inside the pipe to allow the gas to flow through and trap dust, and a collecting unit for storing the trapped dust.
[0086] In addition, when the recovered dust is reused, the dust is added to the process S20 of roasting and pre-reducing the nickel ore for reuse. More specifically, the nickel ore and the recovered dust are added to the inside of a roasting device such as a rotary kiln for roasting and pre-reduction.
[0087] On the other hand, the particle size of the dust recovered from the exhaust gas is less than 0.1 mm. Due to the small particle size, if it is directly reused, the amount of dust generated may continue to increase as the number of processes for preparing nickel iron increases. More specifically, the amount of dust generated from the roasting device may continue to increase.
[0088] Therefore, the dust generated during the preparation of ferronickel is prepared into pellets having a particle size greater than a predetermined size, and the prepared pellets are added to a roasting device and reused as source materials.
[0089] However, even if the dust is prepared into pellets for reuse, if the strength of the pellets is weak, a large amount of dust may be regenerated due to wear and breakage. That is, if the strength of the pellets is weak, dust may be generated due to the impact or wear and breakage of the pellets during transportation for reuse. In addition, nickel ore and coal are loaded into the drum of the rotary kiln as a roasting device, and are roasted and reduced as the drum rotates. At this time, if the strength of the pellets is weak, the pellets will be worn and broken due to the rotation of the drum and the friction with the nickel ore and coal, so dust may be generated.
[0090] As described above, if the strength of the pellets is weak, the pellets will be re-powdered during the recycling process, so it is necessary to increase the strength of the pellets. For this reason, when preparing the pellets by granulating the dust, a binder is added together. However, in the prior art, due to the use of expensive inorganic binders as binders, there is a problem of increased production costs of the pellets.
[0091] Therefore, in the embodiment of the present invention, a binder which ensures the strength of pellets and is cheaper than existing binders is prepared, and pellets are prepared using the binder.
[0092] The binder according to the first embodiment is prepared using nickel-iron desulfurization slag (first slag) produced during the desulfurization (S40) process of the nickel-iron preparation process, slag (second slag) produced in the molten steel preparation process for preparing carbon steel, and fly ash.
[0093] In addition, the first slag, the second slag and the fly ash are used to prepare a binder containing silicon oxide (SiO2), calcium oxide (CaO), aluminum oxide (Al2O3) and iron oxide (FeO). At this time, relative to the total amount of the binder, the binder is prepared to contain 30% to 50% by weight of silicon oxide (SiO2), 15% to 25% by weight of calcium oxide (CaO), 10% to 20% by weight of aluminum oxide (Al2O3), and 10% to 20% by weight of iron oxide (FeO). In addition, in addition to silicon oxide (SiO2), calcium oxide (CaO), aluminum oxide (Al2O3) and iron oxide (FeO), the binder may also contain other inevitable components or impurities.
[0094] On the other hand, in the binder, if at least one of silicon oxide (SiO2), calcium oxide (CaO), aluminum oxide (Al2O3), and iron oxide (FeO) exceeds the content ranges given above, the strength of the pellets similar to that prepared using the existing binder cannot be ensured.
[0095] That is, in the binder, if the silicon oxide (SiO2) content is less than 30 wt% or greater than 50 wt%, or the calcium oxide (CaO) content is less than 15 wt% or greater than 25 wt%, or the aluminum oxide (Al2O3) content is less than 10 wt% or greater than 20 wt%, or the iron oxide (FeO) content is less than 10 wt% or greater than 20 wt%, the strength of the pellets prepared using the binder may not be similar to the strength of the pellets prepared using the existing binder.
[0096] For the preparation of a binder with 30 wt% to 50 wt% silicon oxide (SiO2), 15 wt% to 25 wt% calcium oxide (CaO), 10 wt% to 20 wt% aluminum oxide (Al2O3), and 10 wt% to 20 wt% iron oxide (FeO) as described above, this can be achieved by controlling the mixing amounts of the first slag, the second slag, and the fly ash.
[0097] In the following, reference will be made to Figure 1 A method for preparing an adhesive according to a first embodiment of the present invention is described.
[0098] See also Figure 1The process S120 for preparing a binder includes a process S121 for preparing a first slag as slag produced in the desulfurization process S40 of a nickel-iron preparation process, a process S122 for preparing a second slag as slag produced in a molten steel preparation process for preparing carbon steel, a process S123 for preparing fly ash, a process S124 for mixing the first and second slags and fly ash, and a process S125 for preparing a binder using the mixture of the first and second slags and fly ash.
[0099] In addition, the method may further include: before mixing the first and second slags and fly ash, respectively crushing the first and second slags and fly ash, or after mixing the first and second slags and fly ash, crushing the mixture.
[0100] The first slag is slag recovered and reserved from the slag generated in the desulfurization process S40 of the nickel-iron preparation process.
[0101] As described above, the desulfurization process S40 is a process of removing sulfur (S) from the melt prepared in the electric furnace. For desulfurization, a desulfurizing agent such as calcium oxide (CaO) is added to the melt. When the desulfurizing agent is added to the melt, CaS is generated by the reaction between sulfur (S) in the melt and the desulfurizing agent, and the generated CaS enters the slag suspended on the surface of the melt. Then, when the desulfurization is completed, the slag suspended on the surface of the melt is discharged to the outside.
[0102] The slag produced in the desulfurization process S40 contains nickel oxide (NiO), calcium oxide (CaO), silicon oxide (SiO2), aluminum oxide (Al2O3), and iron oxide (FeO). In addition, it may also contain manganese oxide (MnO), phosphorus pentoxide (P2O5), magnesium oxide (MgO), titanium oxide (TiO2), carbon (C), and sulfur (S).
[0103] As described above, the slag generated in the desulfurization process S40 contains nickel oxide (NiO), and due to the high content of nickel oxide (NiO), it is reused as a nickel source material for preparing nickel iron, and is reused by adding it to an electric furnace.
[0104] At this time, among the slag produced in the desulfurization process S40, only the slag with a particle size of 0.5 mm or more is added to the electric furnace for reuse, while the desulfurized slag with a particle size of less than 0.5 mm is stockpiled and will not be recycled. This is because when the small-particle desulfurized slag with a particle size of less than 0.5 mm is added to the electric furnace, the large amount of slag added is too light and will be directly sucked into the pipeline of the exhaust gas treatment device.
[0105] On the other hand, the content of nickel oxide (NiO) contained in the slag varies depending on the particle size of the slag. Figure 3As shown, in the slag with a particle size of more than 10 mm, the nickel oxide content is more than 10 wt %, in the slag with a particle size of more than 5 mm and less than 10 mm, the nickel oxide content is 6.6 wt %, in the slag with a particle size of more than 3 mm and less than 5 mm, the nickel oxide content is 2.9 wt %, in the slag with a particle size of more than 1 mm and less than 3 mm, the nickel oxide content is 3.3 wt %, in the slag with a particle size of more than 0.5 mm and less than 1 mm, the nickel oxide content is 1.9 wt %, and in the slag with a particle size less than 0.5 mm, the nickel oxide (NiO) content is 3.0 wt % to 5 wt %, more specifically about 4.0 wt %.
[0106] The nickel oxide content in slag with a particle size less than 0.5 mm is less than that in slag with a particle size of 10 mm or more and that in slag with a particle size of 5 mm or more and less than 10 mm. However, since its content is as high as 3.0 wt.% to 5 wt.%, it has sufficient recycling value.
[0107] However, currently, the desulfurized slag smaller than 0.5 mm among the slag generated in the desulfurization process S40 is not reused.
[0108] Therefore, in the embodiment, the slag with a particle size less than 0.5 mm in the slag produced in the desulfurization process S40 is reused as a raw material for preparing a binder. Therefore, the first slag can be described as the slag with a particle size of less than 0.5 mm in the slag produced in the desulfurization process S40 of the nickel-iron preparation process.
[0109] In addition, in the embodiment, as described above, the slag with a particle size of less than 0.5 mm in the slag produced in the desulfurization process S40, that is, the first slag, contains calcium oxide (CaO), silicon oxide (SiO2), and iron oxide (FeO) in addition to nickel oxide (NiO). Calcium oxide (CaO) may contain 25% to 30% by weight, silicon oxide (SiO2) may contain 15% to 20% by weight, and iron oxide (FeO) may contain 15% to 20% by weight. In addition, the first slag may contain aluminum oxide (Al2O3), manganese oxide (MnO), phosphorus pentoxide (P2O5), magnesium oxide (MgO), titanium oxide (TiO2), carbon (C), and sulfur (S). The specific example of the first slag is shown in Table 2.
[0110] The first slag, as a raw material for preparing a binder, contains a large amount of calcium oxide (CaO), silicon oxide (SiO2), and iron oxide (FeO) relative to other components. Therefore, the first slag can be described as a raw material for controlling the calcium oxide (CaO), silicon oxide (SiO2), and iron oxide (FeO) of the binder to target contents, respectively.
[0111] Furthermore, as described above, the first slag contains 3.0 wt % to 5 wt % of nickel oxide (NiO), and thus the first slag also functions as a source material for preparing ferronickel or for providing nickel (Ni).
[0112]
Table 2
[0113]
[0114] The second slag is slag produced in the process of preparing molten steel for carbon steel.
[0115] The preparation process of molten steel for carbon steel generally includes a pre-refining process for removing sulfur (S) from molten iron, a converter refining process for removing carbon (C) from the molten iron after the pre-refining, and a secondary refining process for further removing carbon (C) and oxygen (deoxidation) from the molten iron, i.e., molten steel, after the converter refining.
[0116] Pre-refining can be carried out using, for example, a KR (Kanvara Reactor) device, and a desulfurizing agent such as calcium oxide (CaO) can be used in this case.
[0117] The converter refining process is a process in which molten iron is charged into a converter and oxygen is blown into the molten iron through a lance to control the C (carbon) in the molten iron to be 4% by weight or less.
[0118] Secondary refining can be implemented in a vacuum degassing device RH (Rheinstahl Huttenwerke & Heraeus). The vacuum degassing device is arranged on the upper side of the ladle and includes a vacuum tank with an internal space, a spray gun arranged to penetrate the upper part of the vacuum tank, and a pair of dip tubes installed at the lower part of the vacuum tank along the width direction of the vacuum tank. A nozzle is inserted through one of the dip tubes in the pair of dip tubes, and an inert gas such as Ar gas is injected into the inside. In the pair of dip tubes, the dip tube with the nozzle inserted through or the inert gas supplied is called a riser, and the other is called a downcomer.
[0119] This vacuum tank degassing device reduces the pressure of the vacuum tank to less than several Torr, so that the molten steel in the ladle rises into the vacuum tank and then circulates from the riser to the downcomer. In this way, when the molten steel in the ladle circulates or refluxes through the riser and downcomer, oxygen is blown in through the lance to control the carbon (C) in the molten steel to less than 1 weight %.
[0120] After the secondary refining is completed in the vacuum tank degassing device, the slag suspended on the molten steel in the ladle is discharged.
[0121] The slag produced by secondary refining in the preparation process of molten steel for carbon steel contains calcium oxide (CaO), silicon oxide (SiO2), aluminum oxide (Al2O3), and iron oxide (FeO). Calcium oxide (CaO) can contain 35% to 40% by weight, silicon oxide (SiO2) can contain 10% to 15% by weight, aluminum oxide (Al2O3) can contain 20% to 25% by weight, and iron oxide (FeO) can contain 20% to 25% by weight. In addition, manganese oxide (MnO), phosphorus pentoxide (P2O5), magnesium oxide (MgO), titanium oxide (TiO2), carbon (C), and sulfur (S) can also be contained. Specific examples of the slag produced by secondary refining in the preparation process of molten steel for carbon steel are shown in Table 2.
[0122] In the first embodiment, the slag produced by secondary refining in the process of preparing molten steel for carbon steel is reused as a raw material for preparing a binder. Therefore, the second slag can be described as the slag produced by secondary refining in the process of preparing molten steel for carbon steel.
[0123] This second slag, as a raw material for preparing a binder, contains calcium oxide (CaO), silicon oxide (SiO2), aluminum oxide (Al2O3) and iron oxide (FeO) in large amounts relative to other components. Therefore, the second slag can be described as a raw material for controlling calcium oxide (CaO), silicon oxide (SiO2), aluminum oxide (Al2O3) and iron oxide (FeO) of the binder to target contents, respectively.
[0124] Fly ash is a raw material containing 60 to 80 wt % of silicon oxide (SiO 2 ) and 10 to 20 wt % of aluminum oxide (Al 2 O 3 ), and may be an industrial by-product generated when coal is burned in a thermal power plant or the like.
[0125] In addition to silicon oxide (SiO2) and aluminum oxide (Al2O3), fly ash contains calcium oxide (CaO) and iron oxide (FeO). In addition, fly ash may also contain manganese oxide (MnO), phosphorus pentoxide (P2O5), magnesium oxide (MgO), titanium oxide (TiO2), carbon (C), and sulfur (S). In addition, specific examples of fly ash are shown in Table 2.
[0126] This fly ash, as a raw material for preparing a binder, contains a large amount of silicon oxide (SiO2) and aluminum oxide (Al2O3) relative to other components. Therefore, fly ash can be described as a raw material for controlling the silicon oxide (SiO2) and aluminum oxide (Al2O3) of the binder to target contents, respectively.
[0127] After preparing the first and second slags and fly ash (S121, 122, 123) as described above, before mixing them, the first and second slags and fly ash are preferably crushed to a particle size of 100 μm or less. Of course, the present invention is not limited thereto, and the first and second slags and fly ash may be mixed and then the mixture may be crushed to a particle size of 100 μm or less.
[0128] This is to improve granulation properties when pellets are prepared by granulation after mixing a binder and dust.
[0129] After the first and second slags and fly ash (S121, 122, 123) are prepared as described above, they are mixed (S124). At this time, with respect to the total weight % of the mixture of the first slag, the second slag, and the fly ash (hereinafter referred to as the first mixture), the first slag is mixed at 10 to 30 weight %, the second slag is mixed at 10 to 30 weight %, and the fly ash is mixed at 40 to 60 weight %.
[0130] On the other hand, in the first mixture, when at least one of the first slag, the second slag and the fly ash exceeds the respective content ranges given above, it may be difficult to prepare a binder having 30 wt% to 50 wt% silicon oxide (SiO2), 15 wt% to 25 wt% calcium oxide (CaO), 10 wt% to 20 wt% aluminum oxide (Al2O3), and 10 wt% to 20 wt% iron oxide (FeO).
[0131] That is, in the first mixture, when the content of the first slag is less than 10 wt% or more than 30 wt%, or the content of the second slag is less than 10 wt% or more than 30 wt%, or the content of fly ash is less than 40 wt% or more than 60 wt%, it may be difficult to prepare a binder having 30 wt% to 50 wt% of silicon oxide (SiO2), 15 wt% to 25 wt% of calcium oxide (CaO), 10 wt% to 20 wt% of aluminum oxide (Al2O3), and 10 wt% to 20 wt% of iron oxide (FeO). In addition, when such a binder is used, it may not be possible to ensure the strength of pellets similar to that prepared using existing binders.
[0132] Therefore, in the embodiment, the first slag is mixed at 10 to 30 weight %, the second slag is mixed at 10 to 30 weight %, and the fly ash is mixed at 40 to 60 weight %.
[0133] After the first and second slags are mixed with the fly ash (S124), the mixture (ie, the first mixture) is mixed with water to prepare a binder (S125).
[0134] As described above, after the binder is prepared using the first and second slags and the fly ash, the prepared dust, the prepared binder and water are mixed to prepare pellets (S130).
[0135] The pelletizer for granulating dust into pellets may be, for example, a pelletizer having a disk for charging or accommodating the raw material to be granulated and a drive unit for rotating the disk.
[0136] In the method of preparing pellets using a pelletizer, dust, a binder and water are first added to the inside of a disc, and a driving unit is started to rotate the disc. At this time, the dust, the binder and the water are mixed and granulated by the rotating action of the disc, thereby preparing a granulated product of a predetermined size, i.e., a pellet.
[0137] When dust, a binder and water are mixed to prepare pellets, the dust accounts for 65 to 85 weight %, the binder accounts for 5 to 15 weight % and the water accounts for 10 to 20 weight % in the total amount of the mixture of dust, a binder and water (hereinafter referred to as the second mixture).
[0138] On the other hand, for example, when at least one of the second mixture mixed with dust, binder and water exceeds the respective content ranges given above, it may be difficult to prepare a binder having 30 to 50 wt% of silicon oxide (SiO2), 15 to 25 wt% of calcium oxide (CaO), 10 to 20 wt% of aluminum oxide (Al2O3), and 10 to 20 wt% of iron oxide (FeO). In addition, when such a binder is used, it may be impossible to ensure the strength of pellets similar to that of pellets prepared using existing binders.
[0139] In addition, the particle size of the pellets is preferably controlled to be 15 mm to 20 mm, which can be controlled by controlling at least one of the granulation time, the rotation speed of the disk, and the amount of the raw material (second mixture) loaded into the disk.
[0140] Figure 4 1 is a flow chart sequentially showing a method for preparing pellets according to a second embodiment of the present invention.
[0141] In the first embodiment described above, the binder is prepared by mixing the first slag, the second slag and fly ash.
[0142] However, the present invention is not limited thereto. When preparing the binder, Figure 4As shown, a Na-based flux may be further mixed. That is, the process of preparing a binder according to the second embodiment includes a process S121 of preparing a first slag as a slag produced in a desulfurization process of a nickel-iron preparation process, a process S122 of preparing a second slag as a slag produced in a molten steel preparation process for preparing carbon steel, a process S123 of preparing flayat (flay ash), a process S126 of preparing a Na-based flux, a process S124 of mixing the first slag, the second slag, the flayat and the Na-based flux, and a process S125 of preparing a binder using the mixture of the first slag, the second slag, the flayat and the Na-based flux.
[0143] The Na-based flux is added to improve the strength of the pellets, and the Na-based flux may be, for example, a material containing Na2CO3.
[0144] Furthermore, it is preferred that the content of the Na-based flux is 3 wt % to 15 wt % relative to the total amount of the mixture (first mixture) of the first slag, the second slag, the fly ash, and the Na-based flux. That is, the first slag is 10 wt % to 30 wt %, the second slag is 10 wt % to 30 wt %, the fly ash is 40 wt % to 60 wt %, and the Na-based flux is 3 wt % to 15 wt % in the total amount of the first mixture.
[0145] On the other hand, for example, when the content of the Na-based flux in the first mixture is less than 3 wt%, the strength improvement effect of the pellets may be minimal compared to the use of the binder according to the first embodiment in which the Na-based flux is not mixed. On the contrary, when the content of the Na-based flux is greater than 15 wt%, the strength increase rate of the pellets is small relative to the amount added. Therefore, from the perspective of the effect manifestation relative to the amount added, the content of the Na-based flux is preferably 15 wt% or less.
[0146] Figure 5 The table shows the residual rate (%), drop residual rate (%), compression strength (kgf), and shape of the pellets prepared by the methods according to the first and second comparative examples and the first and second embodiments.
[0147] The pellets according to the first and second comparative examples and the first and second embodiments are pellets prepared by recycling dust generated in the nickel-iron preparation process and granulating it. In addition, the first comparative example is a pellet without a binder, and the second comparative example is a pellet prepared using an existing inorganic binder.
[0148] In addition, the pellets according to the first embodiment are pellets prepared using the binder according to the first embodiment (i.e., the binder prepared by mixing the first slag, the second slag, and the fly ash). At this time, the first slag is 10 wt% to 30 wt%, the second slag is 10 wt% to 30 wt%, and the fly ash is 40 wt% to 60 wt% in the total amount of the first mixture of the first slag, the second slag, and the fly ash.
[0149] In addition, the pellets according to the second embodiment are pellets prepared using the binder according to the second embodiment (i.e., the binder prepared by mixing the first slag, the second slag, the fly ash, and the Na-based flux). At this time, the first slag is 10 wt% to 30 wt%, the second slag is 10 wt% to 30 wt%, the fly ash is 40 wt% to 60 wt%, and the Na-based flux is 3 wt% to 15 wt% in the total amount of the mixture of the first slag, the second slag, the fly ash, and the Na-based flux.
[0150] exist Figure 5 The residual rate refers to the weight ratio of pellets with a particle size of 10 mm or more after the roasting and reduction is completed when the pellets are loaded into the drum of the roasting device, i.e., the rotary kiln, and the drum is rotated at a speed of 5 rpm, and the inside of the drum is heated at a temperature of 600°C for 20 minutes to roast and reduce the pellets. In other words, the residual rate is the weight ratio of pellets with a particle size of 10 mm or more after the roasting and reduction is completed to the total weight of the pellets loaded into the drum of the rotary kiln.
[0151] The drop residual rate is the weight ratio of pellets with a particle size of 10 mm or more when the pellets are dropped five times continuously from a height of 2.5 m. In other words, the drop residual rate is the weight ratio of pellets with a particle size of 10 mm or more in the total amount of dropped pellets.
[0152] The compressive strength (kilogram force, kgf) refers to the resistance per unit weight, and is a value measuring the maximum load when pressure at a certain speed is applied to the upper part of the pellet placed on the roller press until the pellet is broken.
[0153] See also Figure 5 The residual rate, drop residual rate, and compression strength of the pellets according to the second comparative example, the first and second embodiments are much higher than those of the first comparative example. In addition, when comparing the amount of small-particle pellets with a particle size of less than 5 mm in the prepared pellets, the second comparative example, the first and second embodiments are much less than those of the first comparative example.
[0154] Furthermore, when comparing the second comparative example with the first and second embodiments, the residual rate of the pellets according to the first and second embodiments is higher than that of the second comparative example prepared using a high-priced inorganic binder.
[0155] In addition, compared with the second comparative example, the drop survival rate and the compressive strength of the pellets according to the first embodiment are smaller within the predetermined range, but the drop survival rate and the compressive strength are similar to those of the second comparative example, which is a degree that no problem occurs when preparing nickel iron. In addition, compared with the second comparative example using a high-priced inorganic binder, the drop survival rate and the compressive strength of the pellets according to the second embodiment are higher than the predetermined range.
[0156] It can be seen that the pellets prepared using the binder prepared by the method according to the embodiment of the present invention have similar or further improved strength to the pellets prepared using the existing binder.
[0157] In addition, compared with the binder according to the first embodiment, the binder according to the second embodiment can produce pellets with high residual rate, falling residual rate and compression strength.
[0158] As described above, in the embodiment of the present invention, the slag produced in the desulfurization process of the nickel-iron production process, the slag produced in the molten steel production process for producing carbon steel, and the industrial byproduct flay ash are reused to prepare the binder. Therefore, the binder can be prepared at a lower cost than the prior art.
[0159] In addition, when the raw material pellets for preparing ferronickel are prepared by using the binder according to the embodiment, pellets having strength similar to or improved from that of pellets prepared by using the existing binder can be prepared.
[0160] Therefore, according to the embodiments of the present invention, the cost for preparing pellets can be reduced while ensuring the strength.
[0161] In addition, since the small-particle desulfurization slag produced in the desulfurization process of the nickel-iron preparation process is reused to prepare the binder, the inventory management cost of the small-particle desulfurization slag that cannot be reused in the existing prior art can be saved.
[0162] In addition, the small-particle desulfurized slag contains nickel (Ni), which is reused as a raw material of a binder to prepare pellets, so the small-particle desulfurized slag plays the role of a source material for preparing nickel iron or for providing nickel (Ni).
[0163] Therefore, the usage of the main raw material for preparing ferronickel and the high-priced nickel ore for providing the source material of nickel (Ni) can be reduced, thereby reducing the cost required for preparing ferronickel.
[0164] Industrial Applicability
[0165] According to the method for preparing pellets according to the embodiment of the present invention, a binder with a lower cost than the prior art can be prepared. In addition, when the binder according to the embodiment is used to prepare raw material pellets for preparing ferronickel, a pellet with a strength similar to or improved to that of a pellet prepared using an existing binder can be prepared.
Claims
1. A method for preparing pelletized ore, comprising: The process of recovering dust generated in the nickel-iron preparation process for future use; A process for preparing a binder using slag produced in a ferronickel production process as a first slag and a by-product produced in a process other than the ferronickel production process; and The process of mixing the dust and the binder and granulating them to prepare pellets, The first slag is a slag recovered and reserved from a desulfurization process for removing sulfur (S) from a melt generated in the following process: a melting and reduction process in which nickel ore is heated to generate a melt and the nickel ore is reduced in the ferronickel preparation process, The first slag is slag produced in the desulfurization process and having a particle size of less than 0.5 mm, which is recovered and reserved. The first slag contains 3.0 wt % to 5.0 wt % of nickel oxide (NiO).
2. The method for preparing pelletized ore according to claim 1, wherein: The by-products include slag generated in the preparation of molten steel for preparing carbon steel as a second slag and fly ash.
3. The method for preparing pelletized ore according to claim 1, wherein: The dust recovery process is used to recover dust generated in at least one of the following processes: a drying process of drying nickel ore in the nickel-iron preparation process; a roasting and pre-reduction process of heating the nickel ore for roasting and pre-reduction; A melting and reduction process of heating the nickel ore to generate a melt and reducing the nickel ore.
4. The method for preparing pelletized ore according to claim 2, wherein: The second slag is slag obtained by recycling slag generated in a refining process in which the carbon (C) in molten steel is reduced to 1 wt % or less.
5. The method for preparing pelletized ore according to claim 2, comprising the following steps: The mixing amount of the first slag, the second slag and the fly ash is controlled so that the total amount of the binder contains 30 weight % to 50 weight % silicon oxide (SiO2), 15 weight % to 25 weight % calcium oxide (CaO), 10 weight % to 20 weight % aluminum oxide (Al2O3), and 10 weight % to 20 weight % iron oxide.
6. The method for preparing pelletized ore according to claim 3, wherein: When preparing the adhesive, a Na-based flux is further mixed.
7. The method for preparing pelletized ore according to claim 6, wherein: The Na-based flux includes Na2CO3.
8. The method for preparing pellets according to claim 2, comprising at least one of the following processes: A process of crushing the first slag, the second slag and the fly ash respectively before mixing them; and a process of crushing the first mixture mixed with the first slag, the second slag and the fly ash.
9. The method for preparing pellets according to any one of claims 1 to 8, wherein: The process of preparing pellets includes mixing the dust, a binder and water. Relative to the total weight % of the second mixture of the dust, the binder and the water, the mixture contains 65 to 85 weight % of the dust, 5 to 15 weight % of the binder and 10 to 20 weight % of the water.
10. A method for preparing a binder for preparing pelletized ore, comprising: A process of preparing slag produced in a nickel-iron preparation process as a first slag; A process for preparing slag produced in the preparation of molten steel for use in the preparation of carbon steel as a second slag; The process of preparing fly ash which is an industrial by-product; as well as The process of mixing the first slag, the second slag and the fly ash to prepare a binder, The first slag is a slag recovered and reserved from a desulfurization process for removing sulfur (S) from a melt generated in the following process: a melting and reduction process in which nickel ore is heated to generate a melt and the nickel ore is reduced in the ferronickel preparation process, The first slag is slag produced in the desulfurization process and having a particle size of less than 0.5 mm, which is recovered and reserved. The first slag contains 3.0 wt % to 5.0 wt % of nickel oxide (NiO).
11. The method for preparing the adhesive according to claim 10, comprising the following steps: The mixing amounts of the first slag, the second slag and the fly ash are controlled so that the total amount of the binder contains 30 wt % to 50 wt % of silicon oxide (SiO2), 15 wt % to 25 wt % of calcium oxide (CaO), 10 wt % to 20 wt % of aluminum oxide (Al2O3), and 10 wt % to 20 wt % of iron oxide. In the process of controlling the mixing amount of the first slag, the second slag and the fly ash, Relative to the total weight of the first mixture of the first slag, the second slag and the floating ash, the mixture contains 10 weight % to 30 weight % of the first slag, 10 weight % to 30 weight % of the second slag and 40 weight % to 60 weight % of the floating ash.
12. The method for preparing the binder according to claim 10, wherein: The process of preparing the binder also includes a process of mixing a Na-based flux. Relative to the total weight % of the first mixture of the first slag, the second slag, fly ash and Na-based flux, the mixture contains 10 weight % to 30 weight % of the first slag, 10 weight % to 30 weight % of the second slag, 40 weight % to 60 weight % of the fly ash, and 3 weight % to 15 weight % of the Na-based flux.
13. The method for preparing the binder according to claim 12, wherein: The Na-based flux includes Na2CO3.
14. A pelletized ore, comprising: Dust generated during the ferronickel production process; and A binder prepared by the method for preparing a binder according to any one of claims 10 to 13.
15. The pellets according to claim 14, having a particle size of 15 mm to 20 mm.
16. The pellets according to claim 14, wherein the residual rate is 94% to 99.5%, and the falling residual rate is 92% to 95%.
17. The pellets according to claim 14, having a compressive strength of 1.8 kgf to 2.1 kgf.
Citation Information
Patent Citations
Method for manufacturing melting materials of stainless steel
KR100942109B1
Method for using stainless steel dust to produce chrome, nickel and iron alloy
CN104498711A
Manufacture of binder
JP1987040326A
Manufacturing method of binder using electro arc furncace slag of stainless steel
KR1020090090115A
Recycling material for producing ferro-nickel and method for manufacturing same
KR1020140085911A