Method for preparing continuous casting protection slag using electrolytic aluminum waste slag, waste water and blast furnace slag
By using electrolytic aluminum waste slag, wastewater, blast furnace slag to prepare continuous casting protective slag, granulation at high temperature and using continuous casting steel heat, the hazardous substances in electrolytic aluminum overhaul and fluorine-containing wastewater are transformed into gun crystal stones, and the existing technology is solved The problems of environmental pollution and high costs have achieved efficient and environmentally friendly solid waste treatment.
Patent Information
- Application Number
- CN202210347379.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-01
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-04-01
AI Technical Summary
The prior art has environmental pollution and high cost problems when dealing with electrolytic aluminum overhaul slag and fluorine-containing wastewater. Landfill causes pollution, wet treatment is complex and costly, and fire treatment requires additional energy consumption.
Use electrolytic aluminum waste slag, wastewater, and blast furnace slag to prepare continuous casting protective slag, and use the heat of continuous casting steel to convert dangerous solid waste into products to form gun crystals to avoid additional Energy and reagent use.
It realizes solid waste treatment without additional energy and reagents, reduces production costs, reduces carbon emissions, and reduces environmental pollution.
Smart Images

Figure CN114589293B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of continuous casting protection slag, and in particular to a method for preparing continuous casting protection slag by utilizing electrolytic aluminum waste slag, waste water and blast furnace slag. Background Art
[0002] Aluminum is one of the most important metal materials, and its output is second only to steel. In 2020, the total output of electrolytic aluminum in the world was 67 million tons. At present, the Hall-Heroult method, which has a history of more than 100 years, is still used to produce aluminum. In the process of electrolytic aluminum production, due to the penetration and corrosion of molten high-temperature electrolyte, the lining structure of the electrolytic cell is deformed and cracked, and the aluminum liquid and electrolyte in the cell leak into the bottom of the electrolytic cell from the cracks, making the electrolytic cell unable to be used normally. Therefore, on average, the aluminum electrolytic cell needs to be overhauled every 5-8 years. The cathode lining material removed during the process is called electrolytic aluminum overhaul slag SPL (Spent Potlining). On average, 20 to 30 kilograms of overhaul slag is produced for every ton of aluminum produced. About 1.4 million tons of SPL will be produced in 2020. The main components of overhaul slag include fluoride 7.5%-22%, sodium 8.6%-22%, alumina 9.2%-26%, and cyanide 0.04%-0.6%. The 2016 National List of Hazardous Wastes defines electrolytic aluminum overhaul slag as hazardous waste, with a hazard code of HW48-321-023-48. In addition, the Environmental Protection Tax Law of the People's Republic of China, which came into effect on January 1, 2018, stipulates that hazardous wastes are subject to an environmental protection tax of 1,000 yuan per ton. In addition, in the production of electrolytic aluminum, in order to eliminate the volatilization of sodium fluoride, aluminum fluoride and other substances in cryolite at high temperatures, wet treatment is used to remove volatiles, and the treatment process will produce a large amount of fluorine-containing and sodium-containing wastewater.
[0003] There are three main ways to treat SPL. The first is landfill. The disadvantage is that the fluoride and cyanide in the SPL after landfill will be released into the surface water and groundwater with rainfall, and release harmful gases such as hydrogen fluoride, polluting the atmosphere, destroying the growth of plants and animals, and thus polluting the environment. Landfill, as an early SPL treatment method, has been almost eliminated. The second is wet treatment, which uses water to separate the water-soluble fluoride and cyanide in SPL from the fixed carbon, and then recovers the water-insoluble fixed carbon as fuel, and recovers the water-insoluble silicon aluminum oxide as cement-based raw materials. The large amount of fluorine-containing and cyanide-containing wastewater generated is adsorbed by activated alumina, activated carbon, nanomaterials and other materials, and then the fluoride and cyanide in the water are removed by membrane filtration. However, this water treatment method is relatively complicated, the cost of the desorbent is often high, and the defluorination and decyanation process in the water may bring in heavy metals, causing secondary pollution of the water. The third method is pyrometallurgy, which involves mixing SPL with coal, sludge and other materials evenly. Under high temperature, cyanide will burn and decompose, and unstable sodium fluoride in SPL will react with coal, calcium silicate and calcium oxide in sludge in a solid phase. Sodium fluoride, which is soluble in water and has a low melting point, will be converted into calcium fluoride or lanceolite, which is insoluble in water and has a high melting point. This will convert hazardous solid waste into ordinary solid waste and achieve the purpose of fluorine fixation. At the same time, the combustion of carbon materials such as graphite can also provide heat. Pyrometallurgy has high conversion efficiency and simple process, but because pyrometallurgy requires additional consumption of a large amount of energy and increases additional costs, the combustion temperature of graphite is also relatively high. Higher combustion temperatures may cause fluoride to volatilize at high temperatures. Summary of the invention
[0004] The purpose of the present invention is to overcome the problems existing in the prior art and provide a method for preparing continuous casting protection slag using electrolytic aluminum waste slag, waste water and blast furnace slag. The method uses the fluorine-containing waste water of the electrolytic aluminum plant as the water source of the protection slag slurry, and precipitates the water-soluble fluoride into the protection slag through high-temperature granulation, and uses the heat of continuous casting steel to convert hazardous solid waste into products.
[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing continuous casting mold slag using electrolytic aluminum waste slag, waste water, and blast furnace slag, comprising the following steps:
[0006] Step 1: The protective slag is made of 22%-45% calcium oxide, 17%-56% silicon oxide, and 0%-13% aluminum oxide as the basic slag. By adding materials containing 2%-16% fluorine and 2%-20% sodium as solvents, the melting point of the protective slag is controlled at about 900-1100 degrees. After adding 2%-20% carbon material, the melting rate of the protective slag is controlled by using the principle that carbon and slag do not wet each other.
[0007] Step 2: Although the maximum use temperature of the protective slag is 1550 degrees, the sodium fluoride produced by the slag layer will not escape from the surface of the protective slag due to the coverage of the protective slag sintering layer and the powder slag layer at high temperature. During the cooling process of the mold casting, the protective slag changes the heat transfer by forming gunite to control the cooling of the casting;
[0008] Step 3: The mold slag will experience a thermal process of first heating up and then cooling down, thereby forming a three-layer structure of slag layer, sintering layer and powder slag layer on the surface of the ingot. Since the mold slag powder slag has a lot of dust and in order to meet the requirements of automatic slag addition, the mold slag is first mixed with powder slag, water and binder to prepare a slurry, and then the formed slurry is made into a hollow particle slag product through high-temperature spray granulation;
[0009] Step 4: During the spray granulation process, water will evaporate quickly, and the sodium fluoride and cyanide dissolved in the water will precipitate onto the surface of the hollow particle protective slag. By converting blast furnace slag solid waste and SPL hazardous waste into raw materials for the production of protective slag, the heat of continuous casting of steel will be used to convert sodium fluoride and calcium silicate into gunite during the use of the protective slag, and solid waste treatment can be achieved without the need for additional energy and reagents.
[0010] Preferably, the common process of steel smelting is to make iron first and then steel, and iron smelting in a blast furnace will produce a large amount of blast furnace slag.
[0011] Preferably, 97% of the steel produced in converter steelmaking is produced by continuous casting.
[0012] Preferably, the continuous casting protection slag as a key functional material of the continuous casting billet has five major functions: lubricating the billet, controlling heat transfer, preventing secondary oxidation of molten steel, absorbing inclusions in the molten steel and insulating and heat-preserving.
[0013] Preferably, from the perspective of elemental composition, SPL can provide the fluorine, sodium, carbon, and aluminum elements required for the mold slag.
[0014] Preferably, blast furnace slag can provide the calcium, silicon and aluminum elements required for the protective slag.
[0015] Preferably, the contents of SPL and blast furnace slag are tested by XRF to adjust the ratio of SPL, wastewater and blast furnace slag to prepare continuous casting mold slag, and then the component content of the mold slag is verified by XRF.
[0016] Preferably, XRF is an X-ray fluorescence analyzer.
[0017] Preferably, SPL and blast furnace slag can be matched with each other due to their similarity in composition with the mold slag. By utilizing the characteristics of the mold slag production process, the fluorine-containing wastewater from the electrolytic aluminum plant can be used as the water source for the mold slag slurry.
[0018] Preferably, high-temperature granulation is used to cause the water-soluble fluoride to precipitate into the protective slag, and the heat of continuous casting of steel is used to convert the hazardous solid waste into products.
[0019] Compared with the prior art, the present invention provides a method for preparing continuous casting mold slag using electrolytic aluminum waste slag, waste water and blast furnace slag, which has the following beneficial effects:
[0020] 1. The present invention converts blast furnace slag solid waste and SPL hazardous waste into raw materials for the production of mold slag. During the use of the mold slag, the heat of steel continuous casting is used to convert sodium fluoride and calcium silicate into gunite, thereby achieving solid waste treatment without the need for additional energy and reagents.
[0021] 2. The present invention can greatly reduce the production cost of the protective slag plant, protect the environment, reduce carbon emissions, and save raw materials such as fluorite, sodium carbonate, graphite, tap water, etc. that the protective slag plant originally needs to purchase by treating SPL hazardous waste and fluorine-containing wastewater. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the three-layer structure and temperature gradient model of the mold slag proposed by the present invention;
[0023] Figure 2 It is a schematic diagram of the sodium fluoride circulation model proposed by the present invention;
[0024] Figure 3 It is a schematic diagram of the process of preparing the protective slag slurry proposed by the present invention;
[0025] Figure 4 It is a schematic diagram of the preparation process of the hollow particle protective slag proposed by the present invention. DETAILED DESCRIPTION
[0026] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0027] See also Figure 1-4 The present invention provides a technical solution: a method for preparing continuous casting mold slag using electrolytic aluminum waste slag, waste water, and blast furnace slag, comprising the following steps:
[0028] Step 1: The protective slag is made of 22%-45% calcium oxide, 17%-56% silicon oxide, and 0%-13% aluminum oxide as the basic slag. By adding materials containing 2%-16% fluorine and 2%-20% sodium as solvents, the melting point of the protective slag is controlled at about 900-1100 degrees. After adding 2%-20% carbon material, the melting rate of the protective slag is controlled by using the principle that carbon and slag do not wet each other.
[0029] Step 2: Although the highest use temperature of the protective slag is 1550 degrees, the sodium fluoride produced by the slag layer will not escape from the surface of the protective slag due to the coverage of the protective slag sintering layer and the powder slag layer at high temperature. Figure 2 As shown, during the cooling process of the mold casting, the protective slag changes the heat transfer by forming gunite to control the cooling of the casting;
[0030] Step 3: The protective slag will experience a thermal process of first heating up and then cooling down, thus forming a three-layer structure of molten slag layer, sintered layer and powder slag layer on the surface of the ingot. The use environment of the protective slag is as follows: Figure 1 As shown in the figure, due to the large dust content of the mold slag powder and in order to meet the requirements of automatic slag addition, the mold slag powder, water and binder are first mixed to prepare a slurry. The production process is as follows Figure 3 As shown, the formed slurry is then manufactured into a hollow particle slag product through high temperature spray granulation;
[0031] Step 4: During the spray granulation process, water will evaporate quickly, and the sodium fluoride and cyanide dissolved in the water will precipitate onto the surface of the hollow particle protective slag. The production process is as follows: Figure 4 As shown, by converting blast furnace slag solid waste and SPL hazardous waste into raw materials for the production of protective slag, the heat of continuous casting of steel is used to convert sodium fluoride and calcium silicate into gunite during the use of the protective slag, and solid waste treatment is achieved without the need for additional energy and reagents.
[0032] In the present invention, preferably, the common process of steel smelting is to first make iron and then make steel, and a large amount of blast furnace slag will be produced by blast furnace ironmaking.
[0033] In the present invention, preferably, 97% of the steel produced by converter steelmaking is produced by continuous casting.
[0034] In the present invention, preferably, the continuous casting protection slag as a key functional material of the continuous casting billet has five major functions of lubricating the billet, controlling heat transfer, preventing secondary oxidation of molten steel, absorbing inclusions in the molten steel and heat insulation.
[0035] In the present invention, preferably, from the perspective of elemental composition, SPL can provide the fluorine, sodium, carbon and aluminum elements required for the mold slag.
[0036] In the present invention, preferably, blast furnace slag can provide calcium, silicon and aluminum elements required for mold slag.
[0037] In the present invention, preferably, the contents of SPL and blast furnace slag are tested by XRF to adjust the SPL, the ratio of wastewater and blast furnace slag to configure the continuous casting mold slag, and then the component content of the mold slag is verified by XRF.
[0038] In the present invention, preferably, XRF is an X-ray fluorescence analyzer.
[0039] In the present invention, preferably, SPL and blast furnace slag can be matched with each other due to their similarity in composition with the mold slag, and the fluorine-containing wastewater of the electrolytic aluminum plant can be used as the water source for the mold slag slurry by utilizing the characteristics of the mold slag production process.
[0040] In the present invention, preferably, high-temperature granulation is performed to allow the water-soluble fluoride to precipitate into the protective slag, and the heat of continuous casting of steel is used to convert the hazardous solid waste into products.
[0041] Embodiment 1
[0042] A method for preparing continuous casting protection slag using electrolytic aluminum waste slag, waste water and blast furnace slag. The protection slag uses 22%-45% calcium oxide, 17%-56% silicon oxide and 0%-13% aluminum oxide as basic slag, and by adding materials containing 2%-16% fluorine and 2%-20% sodium as solvents, the melting point of the protection slag is controlled at about 900 degrees to 1100 degrees. After adding 2%-20% carbon material, the melting rate of the protection slag is controlled by using the principle that carbon and slag do not wet each other. Although the maximum use temperature of the protection slag reaches 1550 degrees, at high temperature, due to the coverage of the protection slag sintering layer and the powder slag layer, the sodium fluoride produced by the slag layer will not escape from the surface of the protection slag. The sodium fluoride circulation process is as follows: Figure 2 As shown in the figure, during the cooling process of the mold casting, the protective slag controls the cooling of the casting by forming gunite to change the heat transfer; the protective slag will experience a thermal process of first heating up and then cooling down, thus forming a three-layer structure of slag layer, sintering layer and powder slag layer on the surface of the casting. The use environment of the protective slag is as follows: Figure 1 As shown in the figure, due to the large dust content of the mold slag powder and in order to meet the requirements of automatic slag addition, the mold slag powder, water and binder are first mixed to prepare a slurry. The production process is as follows Figure 3 As shown, the slurry is then made into a hollow particle slag product through high temperature spray granulation; during the spray granulation process, water evaporates quickly, and the sodium fluoride and cyanide dissolved in the water precipitate onto the surface of the hollow particle protective slag. The production process is as follows Figure 4 As shown, by converting blast furnace slag solid waste and SPL hazardous waste into raw materials for the production of protective slag, the heat of continuous casting of steel is used to convert sodium fluoride and calcium silicate into gunite during the use of the protective slag, and solid waste treatment is achieved without the need for additional energy and reagents.
[0043] Embodiment 2
[0044] The common process of steel smelting is to make iron first and then steel. A large amount of blast furnace slag will be produced through blast furnace ironmaking. 97% of steel in converter steelmaking is produced by continuous casting. Continuous casting protection slag, as the key functional material of continuous casting billet, has five major functions: lubricating billet, controlling heat transfer, preventing secondary oxidation of molten steel, absorbing molten steel inclusions and heat insulation. From the perspective of element composition, SPL can provide the fluorine, sodium, carbon and aluminum elements required for protection slag, and blast furnace slag can provide the calcium, silicon and aluminum elements required for protection slag. The content of SPL and blast furnace slag is tested by XRF to adjust SPL, and the proportion of wastewater and blast furnace slag is configured to make continuous casting protection slag, and then the component content of protection slag is verified by XRF. XRF is an X-ray fluorescence analyzer. SPL and blast furnace slag can be matched with the similarity of the same protection slag composition. By utilizing the characteristics of the protection slag production process, the fluorine-containing wastewater of the electrolytic aluminum plant can be used as the water source of the protection slag slurry. Through high-temperature granulation, the fluoride dissolved in water is precipitated into the protection slag, and the heat of continuous casting steel is used to transform hazardous solid waste into products.
[0045] The working principle and use process of the present invention: when used, SPL can provide the fluorine, sodium, carbon, and aluminum elements required for the protective slag, while blast furnace slag can provide the calcium, silicon, and aluminum elements required for the protective slag. The content of SPL and blast furnace slag is tested by XRF (X-ray fluorescence analyzer) to adjust SPL, and the ratio of wastewater and blast furnace slag is configured to form continuous casting protective slag, and then the component content of the protective slag is verified by XRF. The raw material of the protective slag changes with the steel products and continuous casting conditions, and the composition of the SPL waste also fluctuates with the electrolytic aluminum process conditions. SPL and blast furnace slag can be matched with the similarity of the protective slag composition. By utilizing the characteristics of the protective slag production process, the fluorine-containing wastewater of the electrolytic aluminum plant can be used as the water source of the protective slag slurry. Through high-temperature granulation, the fluoride dissolved in water is precipitated into the protective slag, and the heat of continuous casting steel is used to convert hazardous solid waste into products.
[0046] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing continuous casting mold slag using electrolytic aluminum waste slag, waste water and blast furnace slag, It is characterized in that The following steps are involved: Step 1: The protective slag is made of 22%-45% calcium oxide, 17%-56% silicon oxide, and 0%-13% aluminum oxide as the basic slag. By adding materials containing 2%-16% fluorine and 2%-20% sodium as solvents, the melting point of the protective slag is controlled at about 900 degrees to 1100 degrees. After adding 2%-20% carbon material, the melting rate of the protective slag is controlled by using the principle that carbon and slag do not wet each other. Step 2: Although the maximum use temperature of the protective slag is 1550 degrees, the sodium fluoride produced by the slag layer will not escape from the surface of the protective slag due to the coverage of the protective slag sintering layer and the powder slag layer at high temperature. During the cooling process of the mold casting, the protective slag changes the heat transfer by forming gunite to control the cooling of the casting; Step 3: The mold slag will experience a thermal process of first heating up and then cooling down, thereby forming a three-layer structure of slag layer, sintering layer and powder slag layer on the surface of the ingot. Since the mold slag powder slag has a lot of dust and in order to meet the requirements of automatic slag addition, the mold slag is first mixed with powder slag, water and binder to prepare a slurry, and then the formed slurry is made into a hollow particle slag product through high-temperature spray granulation; Step 4: During the spray granulation process, water will evaporate quickly, and the sodium fluoride and cyanide dissolved in the water will precipitate onto the surface of the hollow particle protective slag. By converting the blast furnace slag solid waste and SPL hazardous waste into the production raw materials of the protective slag, the heat of steel continuous casting will be used to convert sodium fluoride and calcium silicate into gunite during the use of the protective slag, thus achieving solid waste treatment; From the perspective of element composition, SPL can provide the fluorine, sodium, carbon and aluminum elements required for mold slag. The content of SPL and blast furnace slag can be tested by XRF to adjust SPL, and the ratio of wastewater and blast furnace slag can be configured for continuous casting mold slag. The content of the mold slag can be verified by XRF. SPL and blast furnace slag can be matched with the similarity of the mold slag composition. By utilizing the characteristics of the mold slag production process, the fluorine-containing wastewater of the electrolytic aluminum plant can be used as the water source for the mold slag slurry. The normal process of steel smelting is to make iron first and then steel. Smelting iron in a blast furnace will produce a large amount of blast furnace slag, which can provide the calcium, silicon and aluminum elements needed for protective slag.
2. The method for preparing continuous casting mold slag using electrolytic aluminum waste slag, waste water and blast furnace slag according to claim 1, It is characterized in that 97% of steel is produced by continuous casting.
3. The method for preparing continuous casting mold slag using electrolytic aluminum waste slag, waste water and blast furnace slag according to claim 2, It is characterized in that As a key functional material for continuous casting billets, continuous casting protection slag has five major functions: lubricating the billet, controlling heat transfer, preventing secondary oxidation of molten steel, absorbing inclusions in molten steel and thermal insulation.
4. The method for preparing continuous casting mold slag using electrolytic aluminum waste slag, waste water and blast furnace slag according to claim 3, It is characterized in that XRF is an X-ray fluorescence analyzer.
5. The method for preparing continuous casting mold slag using electrolytic aluminum waste slag, waste water and blast furnace slag according to claim 4, It is characterized in that Through high-temperature granulation, the water-soluble fluorides are precipitated into the protective slag, and the heat of continuous casting of steel is used to transform hazardous solid waste into products.