A multifunctional textile softening composition and preparation method thereof
A multifunctional textile softening composition using inorganic particles and carbon materials addresses the limitations of existing agents by enhancing antibacterial, UV protection, and self-cleaning properties through optimized particle structures and preparation methods, ensuring safety and efficacy.
Patent Information
- Application Number
- CN202110480041.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-04-30
AI Technical Summary
Existing textile softening agents lack multifunctionality, particularly in antibacterial, UV protection, and self-cleaning properties, often containing toxic components and prone to yellowing and silicon spots, while current multifunctional agents do not adequately address these needs.
A multifunctional textile softening composition comprising inorganic particles (modified basic zinc carbonate, nano silicon dioxide, nano silver, or modified titanium dioxide), carbon materials (graphene, graphene oxide, graphite, carbon nanotubes, carbon nanofibers, fullerene), and alkane oils, with specific ratios and preparation methods to enhance dispersibility and antibacterial, UV protection, and self-cleaning effects.
The composition achieves improved safety, antibacterial efficacy, UV resistance, and self-cleaning properties by utilizing non-toxic materials and optimized particle structures, enhancing dispersibility and surface energy to increase photogenerated carriers and electron holes for effective UV protection and antibacterial action.
Smart Images

Figure BDA0003048841180000091 
Figure BDA0003048841180000101
Abstract
Description
Technical Field
[0001] The invention relates to the field of textile softening finishing, and in particular to a multifunctional textile softening composition and a preparation method thereof. Background Art
[0002] With the advancement of science and technology, people's production and living standards are gradually improving. The public's demand for textiles is not only about keeping warm and bright colors, but also about antibacterial, UV protection, self-cleaning and other functions of textiles. In particular, the antibacterial function of textiles has received more and more attention today when the concept of healthy life is prevalent.
[0003] Therefore, more and more manufacturers pay more and more attention to improving the antibacterial properties of textiles during the preparation of textiles. Softening finishing is an important subsequent finishing process in the preparation of textiles. In the usual textile processing process, the surface of the textile will become rough after the previous treatments. In order to make the textiles have good flexibility, lubricity and feel, a softening finishing process of the textiles is required. However, the finishing agents used in the usual process have relatively single active components, mostly single oil emulsions, which make the functions relatively single. They rarely take into account the antibacterial, UV protection, self-cleaning and other functions in addition to softening, and are prone to yellowing, silicon spots and other phenomena. Other multifunctional finishing agents also have some toxic components.
[0004] Therefore, it is a very meaningful task to develop an antibacterial composition that is highly efficient, low-toxic, and has excellent UV protection and cleaning resistance. Summary of the invention
[0005] In order to solve the above technical problems, the first aspect of the present invention provides a multifunctional textile softening composition, the raw materials of which include inorganic particles, carbon materials, dispersants, and alkane oils; the content of the inorganic particles is 4 to 6 wt%; the content of the carbon materials is 2 to 3 wt%; the content of the dispersant is 0.1 to 0.5 wt%; and the alkane oil is the remainder.
[0006] Preferably, the inorganic particles are at least one of modified basic zinc carbonate, nano silicon dioxide, nano silver, nano titanium dioxide, and modified titanium dioxide.
[0007] Preferably, the inorganic particles are modified basic zinc carbonate; the fineness of the modified basic zinc carbonate is 50 to 100 nm.
[0008] Preferably, the modified basic zinc carbonate is at least one of basic zinc carbonate modified by coating with barium sulfate, basic zinc carbonate modified by coating with zinc hydroxide, and basic zinc carbonate modified by composite coating with barium sulfate and zinc hydroxide.
[0009] Preferably, the carbon material is at least one of graphene, graphene oxide, graphite, carbon nanotubes, carbon nanofibers, and fullerene.
[0010] Preferably, the weight ratio of the modified basic zinc carbonate to the carbon material is (1-6):(2-3).
[0011] Preferably, the dispersant is at least one of alkylbenzene sulfonate, dodecyldimethylbenzyl ammonium chloride, dioctadecyldimethylammonium chloride, and ester-based quaternary ammonium salt.
[0012] Preferably, the alkane oil is at least one of white oil, dimethyl silicone oil and hydroxy silicone oil.
[0013] The second aspect of the present invention provides a method for preparing a multifunctional textile softening composition, comprising the following steps:
[0014] S1: mixing and stirring inorganic particles, carbon material and dispersant to obtain a mixture;
[0015] S2: adding alkane oil into a mixing container, heating and stirring evenly, and then cooling the reaction to obtain the antibacterial composition.
[0016] Preferably, in step S2, the stirring temperature is 200-220° C., and the stirring time is 1-2 hours.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The softening composition prepared by the present invention uses alkane oil and modified inorganic nanomaterials which are non-toxic to the human body as raw materials, which improves the safety of the softening composition and conforms to the concept of healthy life.
[0019] 2. The softening composition prepared by the present invention is added with barium sulfate, zinc hydroxide or barium sulfate and zinc hydroxide composite-coated modified basic zinc carbonate, which improves the dispersibility of the modified basic zinc carbonate in the composition, improves the retention rate of basic zinc carbonate on the surface of textiles, and improves the antibacterial effect of textiles.
[0020] 3. The soft composition prepared by the present invention adds modified titanium dioxide, graphene and other materials, and through the joint action of multiple raw materials, the surface energy of the modified particles is improved, the generation speed and number of photogenerated carriers and electron holes are effectively increased, the anti-ultraviolet and anti-fouling properties of the textile are improved, and the antibacterial effect of the textile can be further improved. DETAILED DESCRIPTION
[0021] In order to solve the above technical problems, the first aspect of the present invention provides a multifunctional textile softening composition, the raw materials of which include inorganic particles, carbon materials, dispersants, and alkane oils; the content of the inorganic particles is 4 to 6 wt%; the content of the carbon materials is 2 to 3 wt%; the content of the dispersant is 0.1 to 0.5 wt%; and the alkane oil is the remainder.
[0022] Preferably, the inorganic particles are at least one of modified basic zinc carbonate, nano silicon dioxide, nano silver, nano titanium dioxide, and modified titanium dioxide.
[0023] Preferably, the inorganic particles are modified basic zinc carbonate; the fineness of the modified basic zinc carbonate is 50 to 100 nm.
[0024] Preferably, the modified basic zinc carbonate is at least one of basic zinc carbonate modified by coating with barium sulfate, basic zinc carbonate modified by coating with zinc hydroxide, and basic zinc carbonate modified by composite coating with barium sulfate and zinc hydroxide.
[0025] Preferably, the weight ratio of the modified basic zinc carbonate to the carbon material is (1-6):(2-3).
[0026] Preferably, the modified basic zinc carbonate is barium sulfate-coated modified basic zinc carbonate.
[0027] Preferably, the method for preparing the barium sulfate-coated modified basic zinc carbonate comprises the following steps:
[0028] (1) Weighing basic zinc carbonate solid, adding deionized water to prepare a suspension;
[0029] (2) adding a saturated aqueous solution of barium chloride to the suspension system, placing the suspension system in an electric magnetic stirrer for stirring, and then adding dropwise an aqueous solution of sodium sulfate;
[0030] (3) After the dropwise addition is completed, the mixture is kept warm and stirred for a period of time to allow the generated barium sulfate to precipitate on the surface of the basic zinc carbonate to obtain a modified basic zinc carbonate suspension;
[0031] (4) After the reaction is completed, the suspension is filtered and washed, and then the filtrate is dried at 105° C. to a constant mass, and ground to obtain a powdered modified basic zinc carbonate.
[0032] Preferably, in the preparation method of the modified basic zinc carbonate, the insulation temperature is 70 to 90° C. and the insulation time is 2 to 4 hours.
[0033] In the present application, the overall antibacterial effect of the antibacterial composition is effectively improved by coating and modifying basic zinc carbonate. The applicant speculates that the possible reason is that the basic zinc carbonate is coated and protected by the formation of coating layers such as barium sulfate and zinc hydroxide, and a simple core-shell structure is formed. Further, when the insulation temperature during the preparation of modified basic zinc carbonate is 70-90°C; the insulation time is 2-4 hours, the deposition of barium sulfate on the surface of basic zinc carbonate is close to 30wt%, the particle size of barium sulfate particles is significantly increased, and an uneven "peak-valley" structure is formed on the surface of zinc carbonate, the surface pores are increased, and the specific surface area is significantly increased, which effectively helps the dispersion effect of zinc carbonate in the oil phase; and the formation of the "peak-valley" structure effectively increases the microscopic friction coefficient of the surface of the modified particles, effectively improves its physical entanglement effect with graphene, and improves its retention rate between graphene layers.
[0034] Preferably, the inorganic particles may also contain modified titanium dioxide.
[0035] Preferably, the modified titanium dioxide is amorphous silicon dioxide-coated modified titanium dioxide.
[0036] Preferably, the preparation method of the modified titanium dioxide comprises the following steps:
[0037] (1) Mix titanium dioxide and ammonia water, and then add a certain amount of ethanol and stir to mix evenly;
[0038] (2) preparing a dropwise solution of ethyl orthosilicate and a certain amount of ethanol, and dropping the solution into the mixed solution in step (1) while stirring;
[0039] (3) After the dropwise addition is completed, the temperature is kept constant for 20 to 30 minutes. After the reaction is completed, the product is centrifuged and dried to obtain silica-coated modified titanium dioxide particles.
[0040] Preferably, the reaction time of adding dropwise while stirring is 2 to 5 hours.
[0041] Preferably, the particle size of the modified titanium dioxide is 25 to 30 nm.
[0042] Preferably, the average thickness of the silicon dioxide coating layer of the modified titanium dioxide is 1.5 to 3.5 nm.
[0043] In the present invention, the anti-ultraviolet and anti-pollution effects of the antibacterial composition are improved by adding an amorphous silicon dioxide-coated modified titanium dioxide effective body. The applicant speculates that the possible reason is that the modified titanium dioxide particles are wrapped with silica, and the silica shell is formed on the surface of the titanium dioxide particles, forming a simple core-shell structure; and at the same time, the formation of the silica shell on the amorphous rough surface increases the specific surface area of the titanium dioxide particles, effectively improving the surface energy of the modified particles; it is further found that when the thickness of the silica shell is 1.5 to 3.5 nm, the presence of the silica shell can not only improve the oil phase dispersion effect of titanium dioxide, but also the thinner shell thickness will not significantly reduce the light wave energy during sunlight irradiation, thereby hindering the excitation and aggregation of photogenerated carriers on the titanium dioxide surface; when the thickness of the silica shell is greater than 3.5 nm, the density of photogenerated carriers and electron holes on the titanium dioxide surface drops sharply, and the energy band distance between the conduction band and the valence band of the modified titanium dioxide becomes larger, the ultraviolet light wavelength absorption effect is reduced, and effective photocatalytic degradation cannot be carried out.
[0044] Preferably, the carbon material is at least one of graphene, graphene oxide, graphite, carbon nanotubes, carbon nanofibers, and fullerene.
[0045] Preferably, the carbon material is graphene.
[0046] Preferably, the graphene is graphene that has been ball-milled and ultrasonically pretreated.
[0047] Preferably, the fineness of the graphene that has been ball-milled and ultrasonically pretreated is 100 to 300 nm.
[0048] Preferably, the method of graphene ball milling and ultrasonic pretreatment comprises the following steps:
[0049] (1) Place the purchased graphene of larger size and fineness into an automatic ball mill and mill for 5 to 10 minutes;
[0050] (2) taking out the ball-milled graphene, using a high-power probe ultrasound of 800 to 1000 W for 2 to 3 hours, and then drying;
[0051] (3) Repeat the first two steps 3 to 5 times until the average fineness of the graphene is less than 300 nm, thereby obtaining pretreated graphene.
[0052] Preferably, the weight ratio of the modified titanium dioxide to the carbon material is (3-4):(2-3).
[0053] In the present invention, the antibacterial, anti-ultraviolet and anti-pollution effects of the antibacterial composition are further effectively improved by ball milling and ultrasonic pretreatment of large-sized graphene and limiting its weight ratio with modified titanium dioxide. The applicant speculates that: the graphene after ball milling and ultrasonic pretreatment of large-sized graphene has fewer stacked layers and more edge active groups, which effectively improves the interlayer adsorption and hydrogen bonding between graphene and the surface of barium sulfate and modified titanium dioxide, and improves the in-situ loading effect of graphene; at the same time, the in-situ loading of graphene and titanium dioxide at low fineness forms a specific heterojunction structure, which effectively improves the generation speed and number of photogenerated carriers and electron holes, and because of the special PN junction structure in the heterojunction, the occurrence of electronic reset phenomenon is greatly avoided, and the carriers and electron holes are respectively gathered on the conduction band and valence band of the composite structure surface, and the forbidden band distance between the conduction band and the valence band of the composite structure is reduced, which significantly improves the ultraviolet light absorption effect and anti-pollution effect of the antibacterial composition.
[0054] Pretreated graphene will produce many edge groups, which are easy to modify the hydroxyl groups on the surface of titanium dioxide to produce hydrogen bonds, thereby retaining the modified titanium dioxide between graphene layers. The optical valence band and conduction band of graphene materials are higher than those of titanium dioxide. The loading of titanium dioxide on graphene is very easy to form a composite heterojunction structure, which is easy to aggregate the photocatalytically excited carriers and electron holes, reducing the occurrence of recombination. And these carriers and electron holes have a strong ability to oxidize and degrade organic matter when they appear on the surface of the composite structure, and have excellent ultraviolet light absorption ability; both absorb ultraviolet light and convert it into self-cleaning ability of oxidized organic matter. When the combination is used, it has both anti-ultraviolet and anti-pollution effects.
[0055] Preferably, the dispersant is at least one of alkylbenzene sulfonate, dodecyldimethylbenzyl ammonium chloride, dioctadecyldimethylammonium chloride, and ester-based quaternary ammonium salt.
[0056] Preferably, the dispersant is sodium alkylbenzene sulfonate.
[0057] Preferably, the alkane oil is at least one of white oil, dimethyl silicone oil and hydroxy silicone oil.
[0058] Preferably, the alkane oil is white oil.
[0059] The second aspect of the present invention provides a method for preparing a multifunctional textile softening composition, comprising the following steps:
[0060] S1: mixing and stirring inorganic particles, carbon material and dispersant to obtain a mixture;
[0061] S2: adding alkane oil into a mixing container, heating and stirring evenly, and then cooling the reaction to obtain the antibacterial composition.
[0062] Preferably, in step S2, the stirring temperature is 200-220° C., and the stirring time is 1-2 hours.
[0063] The present invention is described in detail below by way of examples. It is necessary to point out here that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by professionals and technicians in this field based on the content of the present invention above still belong to the scope of protection of the present invention.
[0064] Example 1
[0065] Provided is a multifunctional textile softening composition, the raw materials of which include: 3wt% modified basic zinc carbonate, 3wt% modified titanium dioxide, 3wt% graphene, 0.3wt% sodium dodecylbenzene sulfonate, and the balance made up of white oil.
[0066] The modified basic zinc carbonate is basic zinc carbonate modified by barium sulfate, and the modification steps are as follows:
[0067] (1) Weigh 2 g of basic zinc carbonate solid and add 150 ml of deionized water to prepare a suspension;
[0068] (2) Add 20 ml of saturated aqueous solution of barium chloride to the suspension system, stir in an electric magnetic stirrer at 60° C., and then add 35 ml of saturated aqueous solution of sodium sulfate dropwise;
[0069] (3) After the dropwise addition is completed, the mixture is kept at 90° C. and stirred for 3 hours to allow the generated barium sulfate to precipitate on the surface of the basic zinc carbonate to obtain a modified basic zinc carbonate suspension;
[0070] (4) After the reaction is completed, the suspension is filtered and washed, and then the filtrate is dried at 105° C. to a constant mass, and ground to obtain a powdered modified basic zinc carbonate.
[0071] The modified titanium dioxide is amorphous silicon dioxide coated modified titanium dioxide, and the modification steps are as follows:
[0072] (1) Mix 1.2 g of titanium dioxide with 7.5 mL of aqueous ammonia, then add it into 180 mL of anhydrous ethanol and stir until evenly mixed;
[0073] (2) 2.4 mL of tetraethyl orthosilicate and 60 mL of anhydrous ethanol were prepared into a dropwise solution, which was added dropwise to the mixed solution in step (1) while stirring. The stirring and dropping reaction time was 3 hours.
[0074] (3) After the addition is completed, the temperature is kept constant for 25 minutes. After the reaction is completed, the product is centrifuged and dried to obtain silica-coated modified titanium dioxide particles.
[0075] Among them, titanium dioxide was purchased from Ningbo Jiwei Nano New Material Technology Co., Ltd., model: MZT-A1.
[0076] The average particle size of the prepared modified titanium dioxide is 30 nm.
[0077] The average thickness of the silica coating layer of the prepared modified titanium dioxide was 3.5 nm.
[0078] The graphene is graphene that has been ball-milled and ultrasonically pretreated, and the steps are as follows:
[0079] (1) Place 2 g of graphene in an automatic ball mill and mill for 10 minutes;
[0080] (2) taking out the ball-milled graphene, using a 1000W high-power probe ultrasound for 2 hours, and then drying;
[0081] (3) Repeat the first two steps three times until the average fineness of the graphene is 150 nm, thereby obtaining pretreated graphene.
[0082] Among them, graphene was purchased from the Sixth Element Materials Technology Co., Ltd., and the graphene particle size is 800-1500nm.
[0083] Among them, white oil was purchased from Beijing Zhongshi Zhuoli New Energy Technology Co., Ltd., model: 10#.
[0084] Also provided is a method for preparing a multifunctional textile softening composition, comprising the following steps:
[0085] S1: mixing and stirring modified basic zinc carbonate, modified titanium dioxide, graphene, and sodium dodecylbenzene sulfonate to obtain a mixture;
[0086] S2: adding white oil into a mixing container, stirring at 220° C. for 1.5 hours, and then cooling the reaction mixture to obtain the antibacterial composition.
[0087] Example 2
[0088] A multifunctional textile softening composition is provided, and a preparation method of the multifunctional textile softening composition is also provided. The raw materials of the softening composition include: 2wt% modified basic zinc carbonate, 4wt% modified titanium dioxide, 2wt% graphene, 0.5wt% sodium dodecylbenzene sulfonate, and the balance is supplemented by white oil. The specific implementation method is the same as that of Example 1, except that the modified basic zinc carbonate is basic zinc carbonate modified by composite coating of barium sulfate and zinc hydroxide.
[0089] The basic zinc carbonate modified by the composite coating of barium sulfate and zinc hydroxide is modified in the following steps:
[0090] (1) Weigh 2 g of basic zinc carbonate solid and add 150 ml of deionized water to prepare a suspension;
[0091] (2) Add 20 ml of saturated aqueous solution of barium chloride to the suspension system, stir in an electric magnetic stirrer at 60° C., and then add 35 ml of saturated aqueous solution of sodium sulfate dropwise;
[0092] (3) After the dropwise addition is completed, 40 ml of a 20 wt % sodium hydroxide aqueous solution is continued to be added dropwise, and then 20 ml of a 45 wt % zinc nitrate aqueous solution is added dropwise;
[0093] (4) maintaining the temperature at 90° C. and continuing stirring for 3 hours to allow the generated barium sulfate and zinc hydroxide to precipitate on the surface of the basic zinc carbonate to obtain a modified basic zinc carbonate suspension;
[0094] (4) After the reaction is completed, the suspension is filtered and washed, and then the filtrate is dried at 105° C. to a constant mass, and ground to obtain a powdered modified basic zinc carbonate.
[0095] Example 3
[0096] Provided are a multifunctional textile softening composition and a preparation method of the multifunctional textile softening composition. The raw materials of the softening composition include: 1wt% modified basic zinc carbonate, 3wt% modified titanium dioxide, 2wt% graphene, 1wt% sodium dodecylbenzene sulfonate, and the balance of dimethyl silicone oil.
[0097] Comparative Example 1
[0098] Provided are a multifunctional textile softening composition and a preparation method of the multifunctional textile softening composition. The specific implementation method is the same as that of Example 1, except that the temperature of the heat preservation and stirring in the step of barium sulfate-modified basic zinc carbonate is 50°C, and the stirring is performed for 3 hours.
[0099] Comparative Example 2
[0100] Provided are a multifunctional textile softening composition and a preparation method of the multifunctional textile softening composition. The specific implementation method is the same as that of Example 1, except that the basic zinc carbonate is not modified.
[0101] Comparative Example 3
[0102] Provided are a multifunctional textile softening composition and a method for preparing the multifunctional textile softening composition. The specific implementation method is the same as that in Example 1, except that, during the preparation of the modified titanium dioxide, the reaction time of adding dropwise while stirring is 7 hours, and the average thickness of the amorphous silicon dioxide coating layer of the obtained modified titanium dioxide is 5 nm.
[0103] Comparative Example 4
[0104] Provided are a multifunctional textile softening composition and a method for preparing the multifunctional textile softening composition. The specific implementation manner is the same as that of Example 1, except that the titanium dioxide is not modified.
[0105] Comparative Example 5
[0106] Provided are a multifunctional textile softening composition and a preparation method of the multifunctional textile softening composition. The specific implementation method is the same as that of Example 1, except that the graphene is 1 wt%.
[0107] Comparative Example 6
[0108] Provided are a multifunctional textile softening composition and a method for preparing the multifunctional textile softening composition. The specific implementation manner is the same as that of Example 1, except that the graphene is not subjected to ball milling and ultrasonic pretreatment.
[0109] Comparative Example 7
[0110] Provided are a multifunctional textile softening composition and a preparation method of the multifunctional textile softening composition. The specific implementation method is the same as that of Example 1, except that modified titanium dioxide is not added.
[0111] Performance Testing
[0112] The same textiles softened by the softening compositions prepared in the above examples and comparative examples were tested for antibacterial effect, UV resistance and stain resistance.
[0113] 1. Antibacterial effect.
[0114] The antibacterial effect test was conducted with reference to GB / T 20944.2-2007. The textiles softened by the softening compositions prepared in the examples and comparative examples were cut into strips of the same size and quality, placed in a glass bottle, sterilized by high pressure, and sealed for storage. The bacterial solution (C1) with a measured concentration was quantitatively added to the glass bottle, and then the liquid culture medium was added, and cultured at 37°C for 24 hours. The concentration of the bacterial solution (C2) after 24 hours of culture was measured, and the antibacterial rate was calculated.
[0115] Antibacterial rate = (C1-C2) / C1*100%.
[0116] 2. Anti-ultraviolet test.
[0117] Refer to GB / T 30669-2014 and use ultraviolet light to test the anti-yellowing of textiles.
[0118] 3. Anti-fouling test.
[0119] Refer to GB / T 30159.1-2013 for anti-fouling test.
[0120] The above test data are recorded in Table 1.
[0121] Table 1
[0122]
[0123]
[0124] The above is only a preferred embodiment of the present invention and is not intended to limit the invention in other forms. Any technician familiar with the profession may use the technical content disclosed above to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A multifunctional textile softening composition, characterized in that: The raw materials of the softening composition include inorganic particles, carbon material, dispersant, and alkane oil; the content of the inorganic particles is 4-6wt%; the content of the carbon material is 2-3wt%; the content of the dispersant is 0.1-0.5wt%; and the alkane oil is the balance; The inorganic particles are barium sulfate-coated modified basic zinc carbonate and modified titanium dioxide; The weight ratio of the modified basic zinc carbonate to the carbon material is (1-6): (2-3); the fineness of the modified basic zinc carbonate is 50-100 nm; The particle size of the modified titanium dioxide is 25 to 30 nm; the average thickness of the silicon dioxide coating layer of the modified titanium dioxide is 1.5 to 3.5 nm; the modified titanium dioxide is titanium dioxide modified by coating amorphous silicon dioxide; The weight ratio of the modified titanium dioxide to the carbon material is (3-4): (2-3); The carbon material is graphene; The graphene is graphene that has been ball-milled and ultrasonically pretreated; The fineness of the graphene after ball milling and ultrasonic pretreatment is 100-300 nm; The preparation method of the barium sulfate-coated modified basic zinc carbonate comprises the following steps: S1. Weigh basic zinc carbonate solid and add deionized water to prepare a suspension; S2, adding a saturated aqueous solution of barium chloride to the suspension system, placing it in an electric heating magnetic stirrer for stirring, and then dropping an aqueous solution of sodium sulfate; S3, after the dropwise addition is completed, the temperature is kept and stirring is continued for a period of time, so that the generated barium sulfate is deposited on the surface of the basic zinc carbonate to obtain a modified basic zinc carbonate suspension; S4, after the reaction is completed, the suspension is filtered and washed, and then the filtrate is dried at 105° C. to a constant mass, and ground to obtain a powdered modified basic zinc carbonate; In the preparation method of the modified basic zinc carbonate, the insulation temperature is 70 to 90° C. and the insulation time is 2 to 4 hours; The preparation method of the modified titanium dioxide comprises the following steps: (1) Mix titanium dioxide and ammonia water, and then add a certain amount of ethanol and stir to mix evenly; (2) preparing a dropwise solution of ethyl orthosilicate and a certain amount of ethanol, and dropping the solution into the mixed solution in step (1) while stirring; (3) After the dropwise addition is completed, the temperature is kept constant for 20 to 30 minutes. After the reaction is completed, the product is centrifuged and dried to obtain silica-coated modified titanium dioxide particles.
2. The softening composition according to claim 1, characterized in that The dispersant is at least one of alkylbenzene sulfonate, dodecyldimethylbenzyl ammonium chloride, dioctadecyldimethylammonium chloride and ester-based quaternary ammonium salt.
3. The softening composition according to claim 1, characterized in that The alkane oil is at least one of white oil, dimethyl silicone oil and hydroxy silicone oil.
4. A method for preparing a softening composition according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: mixing and stirring inorganic particles, carbon material and dispersant to obtain a mixture; S2: adding alkane oil into a mixing container, heating and stirring evenly, and then cooling the reaction to obtain the softening composition.
5. The preparation method according to claim 4, characterized in that: In step S2, the stirring temperature is 200-220° C., and the stirring time is 1-2 hours.