Silicon-based negative electrode composite material for lithium-ion battery, preparation method and lithium-ion battery

The dual-phase structure of Si/SiO+M composite material alleviates the volume expansion and conductivity of the silicon-based anode material of lithium-ion batteries, and improves the cycle stability and rate performance, while ensuring the safety and environmental protection of the preparation process.

CN114597375BActive Publication Date: 2024-11-26ZHEJIANG TAIKE NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210281774.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-21
Publication Date
2024-11-26
Estimated Expiration
2042-03-21

AI Technical Summary

Technical Problem

The silicon-based anode material of lithium-ion batteries has severe volume expansion during the deintercalation process, which leads to mechanical powdering and the growth of SEI film, which in turn consumes lithium sources, limits the improvement of battery capacity, and the preparation process of existing porous silicon materials Unsafe and environmentally friendly.

Method used

Si/SiO+M composite material is used to generate silicon oxide and nanometals through in-situ solid reaction between silicon and metal oxides, forming a biphasic structure, alleviating volume expansion and improving conductivity, and the preparation process is carried out with high energy under the protection of argon Ball milling and heat treatment.

Benefits of technology

It effectively reduces volume expansion, improves cycle stability and rate performance, and is safe and environmentally friendly in the preparation process, and meets the requirements of green energy conservation and emission reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114597375B_ABST
    Figure CN114597375B_ABST
Patent Text Reader

Abstract

The present invention provides a silicon-based negative electrode composite material for a lithium-ion battery. The silicon-based negative electrode composite material is a Si / SiO+M composite material. The Si / SiO+M composite material has silicon (Si) as a core, silicon oxide (SiO) and nano-metal (M) are attached to the surface of the silicon, thereby forming a dual-phase structure of silicon oxide + nano-metal on the surface of the silicon; wherein the metal oxide is M x O, x=1 or 2, M is a transition metal. The present invention also provides a method for preparing a silicon-based negative electrode composite material for a lithium ion battery and a lithium ion battery. The silicon-based negative electrode composite material of the present invention can alleviate the volume expansion of silicon negative electrode materials, has good electrochemical properties, and the preparation process is environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of energy storage battery materials, and in particular to a silicon-based negative electrode composite material for a lithium ion battery, a preparation method and a lithium ion battery. Background Art

[0002] As one of the most important energy storage technologies, lithium-ion batteries have been playing a key role in promoting the rapid development of portable electronic products and electric vehicles. However, the capacity of traditional negative electrode materials dominated by graphite has gradually approached the theoretical value of 372mAh / g, making it difficult to further increase the battery energy density. In order to meet the needs of the new generation of energy, it is urgent to develop new lithium battery negative electrode technology. Therefore, the development of new negative electrode materials with high capacity and high safety has become a hot spot and direction in the research of negative electrode materials for lithium-ion batteries.

[0003] The negative electrode materials of lithium-ion batteries are mostly based on silicon, but the silicon-based negative electrode has a serious volume expansion (about 300-400%) during the process of lithium insertion and extraction. The stress generated by the repeated insertion and extraction of lithium ions can easily cause mechanical pulverization of silicon particles, thereby causing the fresh silicon surface to be exposed to the electrolyte and regenerating the SEI film. As charging and discharging proceed, the continuous growth of the SEI film will consume the limited lithium source in the battery, ultimately causing the battery capacity to rapidly decay.

[0004] In the prior art, a relatively effective means to alleviate the volume expansion of silicon negative electrode materials is to prepare porous silicon negative electrode materials. However, the Si / MgO silicon negative electrode material prepared by the magnesium thermal reduction reaction of SiO2 in the first step requires the use of highly dangerous magnesium powder as a raw material, and the second step also uses highly corrosive hydrofluoric acid (HF) to treat the product. Although a porous silicon structure is obtained, it does not meet the purpose of safety, green, energy saving and emission reduction. Summary of the invention

[0005] The present invention aims to provide a silicon-based negative electrode composite material for lithium-ion batteries in view of the deficiencies in the prior art. The silicon-based negative electrode composite material can alleviate the volume expansion of silicon negative electrode materials, has good electrochemical properties, and has an environmentally friendly preparation process.

[0006] According to a first aspect of the present invention, a novel silicon-based negative electrode composite material for a lithium-ion battery is provided, wherein the silicon-based negative electrode composite material is a Si / SiO+M composite material, wherein the Si / SiO+M composite material has silicon (Si) as a core, and silicon monoxide (SiO) and nanometal (M) are attached to the surface of the silicon, thereby forming a dual-phase structure of silicon monoxide + nanometal on the surface of the silicon;

[0007] Wherein, the metal oxide is M x O, x=1 or 2, and M is a transition metal.

[0008] Preferably, M is Ag, Cu, Ni, Fe or Co.

[0009] Preferably, the metal oxide is Ag2O, CuO, NiO, FeO or CoO.

[0010] Preferably, in the Si / SiO+M composite material, the molar ratio of each substance is n Si :n SiO :n M =(1~11):1:1.

[0011] According to a second aspect of the present invention, there is provided a method for preparing the aforementioned silicon-based negative electrode composite material for a lithium ion battery, comprising the following steps:

[0012] Under argon protection, silicon powder and metal oxide are subjected to an in-situ solid phase reaction by a high-energy ball milling process to obtain a first composite material;

[0013] heat treating the first composite material to obtain a Si / SiO+M composite material;

[0014] Wherein, the metal oxide is Ag2O, CuO, NiO, FeO or CoO.

[0015] Preferably, the molar mass ratio of the silicon powder to the metal oxide is (2-12):1, and the particle size of the silicon powder is in the micron level.

[0016] Preferably, the ball-to-material ratio of high-energy ball milling is (20-60):1.

[0017] Preferably, the ball milling speed of the high energy ball milling is 300-600 rpm, and the ball milling time is 3-15 hours.

[0018] Preferably, the heat treatment process of the first composite material is as follows:

[0019] The first composite material is placed in an argon protected tubular furnace for calcination, wherein the calcination temperature is 300 to 900° C. and the calcination time is 0.5 to 5 hours;

[0020] The calcined material is immediately placed in a medium for quenching treatment; wherein the quenching medium is one or more of water, oil and inorganic salt solution.

[0021] According to a third aspect of the present invention, a lithium-ion battery is provided, wherein the negative electrode of the battery adopts the silicon-based negative electrode composite material of the lithium-ion battery mentioned above.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The novel silicon negative electrode composite material of the present invention reduces metal oxides (M x O) in situ generation of silicon dioxide and nano-metal M to synthesize Si-SiO-M composite materials, successfully converting Si (~400%) with a larger volume expansion during lithium insertion and extraction into SiO (~200%) material with a smaller volume expansion through an in situ reaction, thereby alleviating the volume expansion of the composite material during lithium insertion and extraction, thereby improving the cycle stability; at the same time, the metal oxide with poor conductivity is converted into nano-metal with good conductivity and uniformly dispersed in the composite material, and the uniformly dispersed nano-metal M serves as a conductive phase, which increases the conductivity of the silicon negative electrode material, thereby improving the rate performance.

[0024] 2. The novel silicon negative electrode composite material of the present invention is composed of excess silicon and metal oxide (M x O) In-situ solid-state reaction, Si+M occurs on the surface of silicon (Si) particles x O→SiO+xM solid-state reaction, the whole process is safe, environmentally friendly and economical, in line with the principles of safety, green, energy conservation and emission reduction. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1a It is a SEM scanning image of the silicon powder of the present invention.

[0026] Figure 1b This is a SEM scan of the Si / SiO+Ag negative electrode composite material of Example 1 of the present invention.

[0027] Figure 2a This is a TEM morphology image of the Si / SiO+Ag composite material of Example 1 of the present invention.

[0028] Figure 2b 3 is the O element distribution diagram of the Si / SiO+Ag composite material of Example 1 of the present invention.

[0029] Figure 2c 3 is a Si element distribution diagram of the Si / SiO+Ag composite material of Example 1 of the present invention.

[0030] Figure 2d This is the Ag element distribution diagram of the Si / SiO+Ag composite material of Example 1 of the present invention.

[0031] Figure 3 This is the XRD diagram of the Si / SiO+Ag composite material of Example 1 of the present invention.

[0032] Figure 4 It is a comparison chart of the cycle data of the Si / SiO+Ag composite material of Example 1 of the present invention and the comparative example material.

[0033] Figure 5This is a rate performance test diagram of the Si / SiO+Ag composite material of Example 1 of the present invention. DETAILED DESCRIPTION

[0034] In order to better understand the technical content of the present invention, specific embodiments are given and described as follows in conjunction with the accompanying drawings.

[0035] Various aspects of the present invention are described in this disclosure with reference to the accompanying drawings, in which many illustrative embodiments are shown. The embodiments of the present disclosure are not necessarily intended to include all aspects of the present invention. It should be understood that the various concepts and embodiments introduced above, as well as those described in more detail below, can be implemented in any of many ways.

[0036] In the prior art, the most commonly used method for preparing porous silicon negative electrode materials is the magnesium thermal reduction method, which uses silicon dioxide (SiO2) and metallic magnesium as raw materials, wherein magnesium is a reducing agent. The two are subjected to a reduction reaction by high-temperature heating under the protection of an inert gas to generate a Si / MgO composite product. The generated product is subjected to processes such as hydrofluoric acid corrosion, cleaning, filtration and drying to obtain a pure porous silicon negative electrode material.

[0037] Si / MgO composite materials alleviate the volume expansion of silicon negative electrode materials to a certain extent and thus improve their cycle stability, but the material requires the use of magnesium powder as raw material and the use of highly corrosive hydrofluoric acid (HF) during the preparation process, which is not in line with the principles of safety, greenness, energy conservation and emission reduction.

[0038] In view of this, the present invention provides a silicon-based negative electrode composite material for a lithium-ion battery, which plays the role of low expansion buffer and conductivity through the dual-phase products of silicon dioxide and nanometal, thereby achieving the dual goals of improving cycle stability and increasing rate.

[0039] In an exemplary embodiment of the present invention, a silicon-based negative electrode composite material for a lithium-ion battery is provided, wherein the silicon-based negative electrode composite material is a Si / SiO+M composite material, wherein the Si / SiO+M composite material has silicon (Si) as a core, silicon monoxide (SiO) and nanometal (M) are attached to the surface of the silicon, thereby forming a dual-phase structure of silicon monoxide + nanometal on the surface of the silicon;

[0040] Wherein, the metal oxide is M x O, x=1 or 2, and M is a transition metal.

[0041] In a preferred embodiment, M is Ag, Cu, Ni, Fe or Co.

[0042] In a preferred embodiment, the metal oxide is Ag2O, CuO, NiO, FeO or CoO.

[0043] In a preferred embodiment, the molar ratio of each substance in the Si / SiO+M composite material is n Si :n SiO :n M =(1~11):1:1.

[0044] In another exemplary embodiment, a method for preparing the aforementioned silicon-based negative electrode composite material for a lithium-ion battery is provided, wherein excess silicon and metal oxide (M x O) In-situ solid-state reaction occurs on the surface of silicon (Si) particles Si+M x O→SiO+xM solid state reaction obtains a dual-phase (SiO+M) structure on the silicon surface.

[0045] In a specific embodiment, a method for preparing a silicon-based negative electrode composite material for a lithium ion battery is provided, comprising the following steps:

[0046] Under argon protection, silicon powder and metal oxide are subjected to an in-situ solid phase reaction by a high-energy ball milling process to obtain a first composite material;

[0047] heat treating the first composite material to obtain a Si / SiO+M composite material;

[0048] Wherein, the metal oxide is Ag2O, CuO, NiO, FeO or CoO.

[0049] In a preferred embodiment, the molar mass ratio of the silicon powder to the metal oxide is (2-12):1, and the particle size of the silicon powder is micrometer-level, and the silicon powder with a particle size of 1-20 μm is particularly preferred.

[0050] Due to the excess silicon, the metal oxide is completely reacted, so the molar ratio of SiO and M is 1:1, and the molar mass ratio of silicon powder and metal oxide is (2-12):1. Therefore, the molar ratio of each substance in the Si / SiO+M composite material is n Si :n SiO :n M =(1~11):1:1.

[0051] In a preferred embodiment, the ball-to-material ratio of high-energy ball milling is (20-60):1.

[0052] In a preferred embodiment, the ball milling speed of the high energy ball milling is 300-600 rpm, and the ball milling time is 3-15 hours.

[0053] In a preferred embodiment, the heat treatment process of the first composite material is as follows:

[0054] The first composite material is placed in an argon protected tubular furnace for calcination, wherein the calcination temperature is 300 to 900° C. and the calcination time is 0.5 to 5 hours;

[0055] The calcined material is immediately placed in a medium for quenching treatment; wherein the quenching medium is one or more of water, oil and inorganic salt solution.

[0056] The electrochemical performance of the material is improved by heat treatment means such as calcining and quenching the first composite material.

[0057] When oil is used as the quenching medium, rapid quenching oil, UHA, or common (normal) quenching oil, UHB, can be selected; sodium chloride aqueous solution can be selected as the inorganic salt solution.

[0058] It should be understood that oil and inorganic salt solution are both commonly used quenching media in the art, and the type can be selected according to the common methods in the art, which will not be described in detail here.

[0059] In another exemplary embodiment, a battery is provided, wherein the negative electrode of the battery adopts the silicon-based negative electrode composite material of the above-mentioned lithium-ion battery.

[0060] The above preparation process and the prepared silicon-based negative electrode composite material for lithium-ion batteries are experimentally tested in combination with specific examples.

[0061] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, etc. used in the following embodiments can be obtained from commercial sources unless otherwise specified.

[0062] [Example 1]

[0063] Micron-sized Si powder and silver oxide (Ag2O) were weighed separately at a molar mass ratio of 6:1, and ball-milled at a high-energy ball milling speed of 500 rpm for 5 hours in a stainless steel ball mill filled with argon gas, with a ball-to-material ratio of 40:1, so that silver oxide (Ag2O) undergoes an in-situ solid-state reaction Si+Ag2O→SiO+Ag on the surface of silicon (Si) particles to obtain a first composite material.

[0064] The first composite material is placed in an argon protected tubular furnace for calcination, wherein the calcination temperature is 850° C. and the calcination time is 2 hours.

[0065] The calcined material was immediately taken out and placed in water for quenching to obtain a silicon-based negative electrode composite material Si / SiO+Ag.

[0066] [Example 2]

[0067] Micron-sized Si powder and copper oxide (CuO) were weighed separately at a molar mass ratio of 12:1, and ball-milled at a high-energy ball milling speed of 500 rpm for 5 hours in a stainless steel ball mill filled with argon, with a ball-to-material ratio of 40:1, so that copper oxide (CuO) undergoes an in-situ solid-state reaction Si+CuO→SiO+Cu on the surface of silicon (Si) particles to obtain a first composite material.

[0068] The first composite material is placed in an argon protected tubular furnace for calcination, wherein the calcination temperature is 300° C. and the calcination time is 5 hours.

[0069] The calcined material is immediately taken out and placed in rapid quenching oil for quenching to obtain a silicon-based negative electrode composite material Si / SiO+Cu.

[0070] [Example 3]

[0071] Micron-sized Si powder and nickel oxide (NiO) were weighed separately at a molar mass ratio of 2:1, and ball-milled at a high-energy ball milling speed of 500 rpm for 5 hours in a stainless steel ball mill filled with argon. The ball-to-material ratio was 40:1, so that the nickel oxide (NiO) underwent an in-situ solid-state reaction Si+NiO→SiO+Ni on the surface of the silicon (Si) particles to obtain a first composite material.

[0072] The first composite material is placed in an argon protected tubular furnace for calcination, wherein the calcination temperature is 900° C. and the calcination time is 0.5 h.

[0073] The calcined material was immediately taken out and placed in a sodium chloride aqueous solution for quenching treatment to obtain a silicon-based negative electrode composite material Si / SiO+Ni.

[0074] [Example 4]

[0075] Micron-sized Si powder and iron oxide (FeO) were weighed separately at a molar mass ratio of 10:1, and ball-milled at a high-energy ball milling speed of 300 rpm for 15 hours in a stainless steel ball mill filled with argon gas, with a ball-to-material ratio of 60:1, so that the iron oxide (FeO) undergoes an in-situ solid-state reaction Si+FeO→SiO+Fe on the surface of the silicon (Si) particles to obtain a first composite material.

[0076] The first composite material is placed in an argon protected tubular furnace for calcination, wherein the calcination temperature is 800° C. and the calcination time is 3 hours.

[0077] The calcined material was immediately taken out and placed in water for quenching to obtain a silicon-based negative electrode composite material Si / SiO+Fe.

[0078] [Example 5]

[0079] Micron-sized Si powder and cobalt oxide (CoO) were weighed separately at a molar mass ratio of 4:1, and ball-milled at a high-energy ball milling speed of 600 rpm for 5 hours in a stainless steel ball mill filled with argon gas, with a ball-to-material ratio of 20:1, so that cobalt oxide (CoO) undergoes an in-situ solid-state reaction Si+CoO→SiO+Co on the surface of silicon (Si) particles to obtain a first composite material.

[0080] The first composite material is placed in an argon protected tubular furnace for calcination, wherein the calcination temperature is 850° C. and the calcination time is 2 hours.

[0081] The calcined material was immediately taken out and placed in water for quenching to obtain a silicon-based negative electrode composite material Si / SiO+Co.

[0082] SEM

[0083] The silicon-based negative electrode composite material Si / SiO+Ag in Example 1 was subjected to SEM test. Figure 1a ) and silicon-based negative electrode composite materials Si / SiO+Ag( Figure 1b ) comparison shows that the silicon particles before the reaction are coarse and irregular polygonal shapes, while the particles after the reaction present an agglomerated microporous structure composed of relatively fine particles, proving that the morphology of the silicon particles has changed before and after the reaction.

[0084] TEM

[0085] The Si / SiO+Ag negative electrode composite material in Example 1 was subjected to TEM test. Figure 2a It can be seen that silicon dioxide and nanometal are attached to the surface of the composite material and combined with Figure 2b-2d According to the EDS element distribution analysis results, the silicon negative electrode composite material is mainly composed of Si, SiO and Ag phases. Therefore, combined with the SEM image, it can be shown that the present invention successfully prepared the Si / SiO+M composite material.

[0086] XRD

[0087] The Si / SiO+Ag negative electrode composite material in Example 1 was subjected to XRD test. Figure 3 It can be seen that amorphous non-crystalline SiO (enlarged rectangular box) and Ag peaks appeared, indicating that Si and Ag2O underwent a Si+Ag2O→SiO+Ag solid-state chemical reaction, which further proves that the silicon negative electrode composite material of Example 1 is mainly composed of Si, SiO and Ag phases, further proving that the present invention successfully prepared the Si / SiO+M composite material.

[0088] Performance Testing

[0089] Preparation of button cells

[0090] Take the negative electrode material (the Si / SiO+Ag negative electrode composite material of Example 1, and the pure silicon negative electrode material is taken as the control sample), conductive carbon black Super-P and binder sodium alginate are mixed in a mass ratio of 6:2:2, add an appropriate amount of deionized water as a solvent, mix evenly in an agate mortar to prepare a slurry, and apply it evenly on the copper foil with a scraper.

[0091] After vacuum drying at 120°C for 12 h, a circular electrode sheet with a diameter of 13 mm was punched out using a mold. The sample electrode was used as the research electrode and the metal lithium sheet was used as the counter electrode to assemble into a 2032-type button battery in a glove box.

[0092] Electrochemical cycle test

[0093] The electrochemical cycle test was carried out using the Xinwei battery testing system, with a charge and discharge current density of 100mA / g, a charge and discharge cut-off voltage of 0.01-1.5V, and a test temperature of 25°C maintained at room temperature.

[0094] The test results are as follows:

[0095] At a current density of 100 mA / g, when the Si / SiO+Ag silicon negative electrode composite material half-cell and the pure Si negative electrode material half-cell are cycled for 20 cycles, Figure 4 shown.

[0096] from Figure 4 It can be seen that at the 20th cycle, the Si / SiO+Ag composite material exhibits a high capacity cycling stability of about 1200 mAh / g, while pure Si rapidly decays below 100 mAh / g. Their reversible discharge capacities are 86.2% and 3.8% of the discharge capacity of the first cycle, respectively.

[0097] Rate performance test

[0098] The Si / SiO+Ag silicon anode composite half-cells were -1 , 0.55A·g -1 , 1.11A·g -1 , 2.77A·g -1 , 1.11A·g -1 , 0.55A·g -1 and 0.28A·g -1 Charge and discharge tests were carried out at different current densities.

[0099] The test results are as follows:

[0100] Combination Figure 5 , Si / SiO+Ag silicon negative electrode composite material was subjected to 0.28A·g-1 , 0.55A·g -1 , 1.11A·g -1 and 2.77A·g -1 After cycling at different current densities, the current density returned to 1.11 A g -1 , 0.55A·g -1 and 0.28A·g -1 During the current density charge and discharge test, its charge and discharge capacity can basically recover to the charge and discharge capacity at the corresponding current density, which shows that the Si / SiO+Ag silicon negative electrode composite material has good rate performance. This good rate performance is attributed to the nano silver particles in the Si / SiO+Ag silicon negative electrode composite material as a conductive phase, which increases the conductive transmission performance of the silicon negative electrode composite material.

[0101] Therefore, the battery using the composite material of the present invention has good cycle life and good rate performance, excellent electrochemical performance, and the preparation process is environmentally friendly and simple to operate.

[0102] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the claims.

Claims

1. A silicon-based negative electrode composite material for a lithium-ion battery, It is characterized in that The silicon-based negative electrode composite material is a Si / SiO+M composite material, wherein the Si / SiO+M composite material has silicon (Si) as the core, silicon dioxide (SiO) and nano-metal (M) are attached to the surface of the silicon, thereby forming a dual-phase structure of silicon dioxide + nano-metal on the surface of the silicon; wherein M is a transition metal; The method for preparing the silicon-based negative electrode composite material comprises the following steps: Under argon protection, silicon powder and metal oxide are subjected to an in-situ solid phase reaction by a high-energy ball milling process to obtain a first composite material; wherein the metal oxide is Ag 2 O, CuO, NiO, FeO or CoO; The first composite material is placed in an argon-protected tubular furnace for calcination, and the calcined material is immediately placed in a medium for quenching treatment to obtain a Si / SiO+M composite material; wherein the quenching medium is one or more of water, oil and inorganic salt solution.

2. The silicon-based negative electrode composite material for lithium-ion batteries according to claim 1, It is characterized in that M is Ag, Cu, Ni, Fe or Co.

3. The silicon-based negative electrode composite material for a lithium-ion battery according to claim 1, It is characterized in that In the Si / SiO+M composite material, the molar ratio of each substance is n Si :n SiO :n M =(1~11):1:

1.

4. The silicon-based negative electrode composite material for a lithium-ion battery according to claim 1, It is characterized in that The molar mass ratio of the silicon powder to the metal oxide is (2-12):1, and the particle size of the silicon powder is in the micron level.

5. The silicon-based negative electrode composite material for lithium-ion batteries according to claim 1, It is characterized in that The ball-to-material ratio of high energy ball milling is (20~60):

1.

6. The silicon-based negative electrode composite material for a lithium-ion battery according to claim 1, It is characterized in that The ball milling speed of high-energy ball milling is 300~600 rpm, and the ball milling time is 3~15 h.

7. The silicon-based negative electrode composite material for a lithium-ion battery according to claim 1, It is characterized in that The heat treatment process of the first composite material is as follows: The first composite material is placed in an argon protected tubular furnace for calcination, wherein the calcination temperature is 300 to 900° C. and the calcination time is 0.5 to 5 hours; The calcined material is immediately placed in a medium for quenching treatment; wherein the quenching medium is one or more of water, oil and inorganic salt solution.

8. A lithium ion battery, It is characterized in that The negative electrode of the battery adopts the silicon-based negative electrode composite material of the lithium-ion battery according to any one of claims 1 to 3.