Polymer and resin composition

By improving the polymer structure of the photosensitive resin composition and synthesizing a polymer with thioether groups using a specific reaction, the problems of low sensitivity and insufficient transparency of existing resin compositions have been solved, resulting in a resin curing material with high sensitivity and high transparency, suitable for the manufacture of color filters and black matrices.

CN114599686BActive Publication Date: 2024-11-12SUMITOMO BAKELITE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080072705.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-11
Filing Date
2020-10-14
Publication Date
2024-11-12
Estimated Expiration
2040-10-14

AI Technical Summary

Technical Problem

Existing photosensitive resin compositions have low sensitivity when forming color filters or black matrices, poor processability in alkaline developing solutions, and insufficient transparency of the cured products.

Method used

By improving the structure of the polymer in the photosensitive resin composition, a polymer precursor is reacted with a compound having hydroxyl and (meth)acryloyl groups in the presence of an alkaline catalyst to synthesize a polymer with thioether groups. The monomer composition of general formula (NBm) and maleic anhydride is polymerized in the presence of a mercaptan-containing compound with more than two functions to form a cured resin with high alkali solubility and low yellowing.

Benefits of technology

The sensitivity and developability of the photosensitive resin composition were improved, yellowing was reduced, and a highly transparent resin cured product was obtained, which is suitable for the manufacture of liquid crystal display devices and solid-state imaging elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114599686B_ABST
    Figure CN114599686B_ABST
Patent Text Reader

Abstract

A polymer obtained by reacting a polymer precursor with a compound having a hydroxyl group and two or more (meth)acryloyl groups and / or a compound having a hydroxyl group and one (meth)acryloyl group in the presence of a basic catalyst, wherein the polymer precursor is obtained by polymerizing a monomer composition containing a monomer represented by the following general formula (NBm) and maleic anhydride in the presence of a bifunctional or more thiol group-containing compound. 1 , R 2 , R 3 and R 4 Each is independently a hydrogen atom or an organic group having 1 to 30 carbon atoms, and a1 is 0, 1 or 2. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polymer and a resin composition containing the polymer. More specifically, the present invention relates to a polymer used as a material of a photosensitive resin composition used in the manufacture of a film, a color filter, a black matrix, a display device, and an imaging element, and a resin composition containing the polymer. Background Art

[0002] Liquid crystal display devices or solid-state imaging elements usually have color filters or black matrices. The color filter or black matrix is ​​formed on a substrate with a structure such as a coloring pattern or a protective film. As a method for forming a coloring pattern or a protective film in these structures, a method of forming by photolithography using a photosensitive resin composition has become the mainstream. Various studies have been conducted on photosensitive resin compositions. For example, Patent Document 1 describes a photosensitive resin composition containing an alkali-soluble resin, a polymerizable compound, and a photopolymerization initiator, wherein the alkali-soluble resin contains at least a group having an acidic group in a side chain and two or more polymerizable unsaturated groups that are different from each other. In addition, the following is described in the examples of Patent Document 1: a methacrylic acid / allyl methacrylate / glycidol adduct is synthesized as an alkali-soluble resin, and the photosensitive resin composition is prepared using the alkali-soluble resin.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent document 1: International Publication No. 2012 / 147706. Summary of the invention

[0006] Technical issues to be solved by the invention

[0007] A resin having the property of being cured by a polymerization reaction produced by light is used in the photosensitive resin composition for forming a color filter or a black matrix. The color filter or the black matrix is ​​made by curing the photosensitive resin composition after patterning it by exposure and development. In the photosensitive resin composition, "high sensitivity" is also considered to be a common subject, but with the complexity or popularization of display devices or camera devices, a higher level of high sensitivity is required. The higher the sensitivity of the photosensitive resin composition, the shorter the time required for exposure, thereby improving productivity. In addition, the photosensitive resin composition is required to have excellent processability in the development process using an alkaline developer. In addition, the cured product of the photosensitive resin composition is required to have high transparency.

[0008] Means for solving technical problems

[0009] The present inventors have found that a cured resin having good sensitivity, high alkali solubility and reduced yellowing can be obtained by improving the polymer used in the photosensitive resin composition or the formulation of the composition, thereby arriving at the present invention.

[0010] According to the present invention, a polymer is provided, wherein the polymer is obtained by reacting a polymer precursor with a compound having a hydroxyl group and two or more (meth)acryloyl groups and / or a compound having a hydroxyl group and one (meth)acryloyl group in the presence of a basic catalyst, and the polymer precursor is obtained by polymerizing a monomer composition containing a monomer represented by the following general formula (NBm) and maleic anhydride in the presence of a difunctional or more thiol-containing compound.

[0011]

[0012] (In the general formula (NBm), R 1 , R 2 , R 3 and R 4 are independently a hydrogen atom or an organic group having 1 to 30 carbon atoms, and a1 is 0, 1 or 2.

[0013] Furthermore, according to the present invention, a polymer having a structure represented by formula (P') is provided.

[0014]

[0015] (In the general formula (P'):

[0016] m is an integer from 0 to 5.

[0017] n is an integer from 1 to 6.

[0018] n+m is 1 to 6.

[0019] p, q and r represent the molar contents of A, B and C respectively, p+q+r=1, p is greater than 0, q is greater than 0, r is greater than 0, and p, q or r may be the same or different in each of the n structural units within [].

[0020] X is hydrogen or an organic group having 1 to 30 carbon atoms.

[0021] Y is a mono- to hexa-valent organic group having 1 to 30 carbon atoms and derived from a bifunctional or higher thiol group-containing compound.

[0022] A contains a structural unit represented by the general formula (NB).

[0023] B contains at least one structural unit selected from the group consisting of structural units represented by the general formula (1) and structural units represented by the general formula (2).

[0024] C contains a divalent structural unit derived from a copolymerizable compound having a double bond.

[0025] A plurality of A's, B's, or C's may be the same as or different from each other.

[0026] Q contains an organic group that is the same as or different from A, B, and C.)

[0027]

[0028] (In the general formula (NB), R 1 , R 2 , R 3 and R 4 are independently a hydrogen atom or an organic group having 1 to 30 carbon atoms, and a1 is 0, 1 or 2.

[0029]

[0030] (In general formula (1), R p A group having two or more (meth)acryloyl groups.

[0031]

[0032] (In general formula (2), R s A group having one (meth)acryloyl group.

[0033] Furthermore, according to the present invention, a resin composition containing the above-mentioned polymer is provided.

[0034] Effects of the Invention

[0035] According to the present invention, there is provided a polymer as a resin material for a photosensitive resin composition which has good sensitivity, high alkali solubility, excellent developability, and reduced yellowing. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a diagram (cross-sectional view) schematically showing an example of the structure of a liquid crystal display device and / or a solid-state imaging element. DETAILED DESCRIPTION

[0037] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. In addition, in all the drawings, the same symbols are marked for the same components, and the description is appropriately omitted. Moreover, all the drawings are for illustration only. The shapes or dimensional ratios of the components in the drawings do not necessarily correspond to actual items. In this specification, the expression "a to b" in the description of the numerical range means "above a and below b" unless otherwise specified. For example, "5 to 90%" means "above 5% and below 90%".

[0038] In the description of the group (group, atomic group) in this specification, the expression without the mark of substituted or unsubstituted includes both unsubstituted and substituted groups. For example, "alkyl" includes not only alkyl groups without substitution (unsubstituted alkyl groups) but also alkyl groups with substitution (substituted alkyl groups).

[0039] The term "(meth)acrylic acid" in this specification means a concept including both acrylic acid and methacrylic acid. The same applies to similar terms such as "(meth)acrylate".

[0040] In particular, the "(meth)acryloyl group" in the present specification is a concept including an acryloyl group represented by -C(=O)-CH=CH2 and a methacryloyl group represented by -C(=O)-C(CH3)=CH2.

[0041] (Polymer P)

[0042] The polymer of this embodiment (hereinafter referred to as "polymer P") is a polymer obtained by reacting a polymer precursor with a compound having a hydroxyl group and two or more (meth)acryloyl groups and / or a compound having a hydroxyl group and one (meth)acryloyl group in the presence of a basic catalyst, and the polymer precursor is obtained by polymerizing a monomer composition containing a monomer represented by the following general formula (NBm) and maleic anhydride in the presence of a difunctional or more thiol-containing compound.

[0043]

[0044] (In the general formula (NBm), R 1 , R 2 , R 3 and R 4 are independently a hydrogen atom or an organic group having 1 to 30 carbon atoms, and a1 is 0, 1 or 2.

[0045] The polymer P of the present embodiment obtained by the above method has a thioether group. By having a thioether group, the polymer P can provide a resin cured product that "has excellent sensitivity in photolithography and higher alkali solubility, and has reduced yellowing and excellent transparency". In addition, the polymer P of the present embodiment obtained by the above method has a structural unit derived from a norbornene monomer represented by formula (NBm). The structural unit derived from the norbornene monomer is chemically strong. Therefore, the polymer P containing it as a structural unit has a small weight loss when subjected to heat treatment and is stable.

[0046] The polymer P has a (meth)acryloyl group in addition to a thioether group. The polymer P may be, for example, a resin having a thioether group and a monofunctional (meth)acryloyl group, a resin having a thioether group and a polyfunctional (meth)acryloyl group, or a resin having a thioether group and a monofunctional (meth)acryloyl group and a polyfunctional (meth)acryloyl group.

[0047] From the viewpoint of the effects of the present invention, the polymer P is preferably a resin having a thioether group and a polyfunctional (meth)acryloyl group.

[0048] More specifically, the polymer P of the present embodiment may be a (meth)acrylic resin having a biphenyl skeleton and having one or more sulfide groups, a (meth)acrylic resin having a bisphenol skeleton and having one or more sulfide groups, a (meth)acrylic resin having a bisphenol skeleton containing a fluorene group and having one or more sulfide groups, a (meth)acrylic resin having a linear alkylene skeleton and having one or more sulfide groups, or a (meth)acrylic resin having a skeleton obtained by polymerization of maleic anhydride and norbornene-based monomers and having one or more sulfide groups.

[0049] The (meth)acrylic resin having a thioether group includes not only polymers of acrylate or methacrylate but also resins having a (meth)acryloyl group added to the side chain of the skeleton.

[0050] The polymer P having one or more thioether groups introduced into its structure can be obtained by a method of synthesizing a polymer in the presence of a thiol compound, or by a method of separately reacting a thiol compound after synthesizing the polymer. The thiol compound used to produce the polymer P of the present embodiment can be a conventionally known compound within the range that the effects of the present invention can be obtained.

[0051] From the viewpoint of the effects of the present invention, the polymer P of the present embodiment preferably contains a thioether group-containing (meth) acrylic resin having a structural unit derived from maleic anhydride (hereinafter referred to as a thioether group-containing (meth) acrylic resin (a)). The thioether group-containing (meth) acrylic resin (a) used as the polymer P of the present embodiment is described below.

[0052] <Thioether group-containing (meth)acrylic resin (a)>

[0053] The thioether group-containing (meth)acrylic resin (a) of the present embodiment has a structure represented by the following general formula (P′): The structural unit A and the structural unit B in the general formula (P′) typically constitute the main chain of the thioether group-containing (meth)acrylic resin (a).

[0054]

[0055] In the general formula (P'):

[0056] m is an integer of 0 to 5, preferably 0 or 1, and more preferably 0.

[0057] n is an integer of 1-6, preferably 3-6.

[0058] Here, n+m is 1-6, preferably 3-6.

[0059] p, q and r represent the molar contents of A, B and C, respectively, and p+q+r=1.

[0060] p is greater than 0, and preferably 0.25 to 0.75.

[0061] q is greater than 0, and preferably 0.25 to 0.75.

[0062] r is 0 or more, preferably 0 to 0.5, more preferably 0 to 0.3, and particularly preferably 0 to 0.1.

[0063] p, q or r may be the same or different in each of the n structural units in [].

[0064] X is hydrogen or an organic group having 1 to 30 carbon atoms.

[0065] Y is a mono- to hexavalent organic group (i) having 1 to 30 carbon atoms and derived from a bifunctional or higher thiol group-containing compound, and is bonded to the structural unit in []n and the structural unit in []m via a thiol group derived from the thiol group.

[0066] A contains a structural unit represented by the general formula (NB).

[0067] B contains at least one structural unit selected from the group consisting of structural units represented by the general formula (1) and structural units represented by the general formula (2).

[0068] C contains a structural unit derived from a copolymerizable compound having a double bond.

[0069] A plurality of A's, B's, or C's may be the same as or different from each other.

[0070] In the general formula (P'), the bonding order of A, B and C is not particularly limited, and any one of A, B and C may be bonded to Y.

[0071] Q contains an arbitrary organic group which is the same as or different from A, B and C.

[0072]

[0073] In formula (NB), R 1 , R2 , R 3 and R 4 Each of them is independently a hydrogen atom or an organic group having 1 to 30 carbon atoms; and a1 is 0, 1 or 2.

[0074]

[0075] In formula (1), R p It is a group having two or more (meth)acryloyl groups.

[0076]

[0077] In formula (2), R s It is a group having one (meth)acryloyl group.

[0078] In one embodiment, the thioether group-containing (meth)acrylic resin (a) of the present embodiment has a structure represented by the general formula (P) in which m is 0 in the structure represented by the general formula (P′).

[0079]

[0080] In formula (P):

[0081] n, p, q and r are the same as those defined in the general formula (P'), and X, Y, A, B and C are the same as those defined in the general formula (P').

[0082] The thioether group-containing (meth)acrylic resin (a) of the present embodiment contains a structural unit represented by the general formula (1) and / or a structural unit represented by the general formula (2) as the structural unit B. In other words, it contains either or both of the structural unit represented by the general formula (1) and the structural unit represented by the general formula (2) as the structural unit B. Therefore, the photosensitive resin composition containing the thioether group-containing (meth)acrylic resin (a) has excellent sensitivity when subjected to photolithography.

[0083] This is believed to be because the curing reaction (polymerization reaction) is promoted by the (meth)acryloyl group contained in the structural unit represented by the general formula (1) or the general formula (2). In addition, the (meth)acrylic resin (a) containing a thioether group contains a structural unit represented by the general formula (NB) as the structural unit A. The structural unit (NB) is chemically strong. Therefore, the (meth)acrylic resin (a) containing a thioether group containing it as a structural unit has a small weight loss when subjected to heat treatment and is stable. Therefore, in order to manufacture a film or filter used in a liquid crystal display device or a solid-state imaging element that requires heat resistance, a photosensitive resin composition containing a (meth)acrylic resin (a) containing a thioether group can be suitably used.

[0084] In a preferred embodiment, the thioether group-containing (meth)acrylic resin (a) contains a structural unit represented by the general formula (1) as an essential component. Since the structural unit represented by the general formula (1) has at least two (meth)acryloyl groups, the (meth)acrylic resin (a) containing the structural unit has high sensitivity in photolithography.

[0085] In one embodiment, the thioether group-containing (meth)acrylic resin (a) may contain a structural unit represented by the general formula (3) as the structural unit B in addition to the structural unit represented by the formula (1) or (2). By containing the structural unit represented by the general formula (3), the thioether group-containing (meth)acrylic resin (a) has high alkali solubility. As a result, the photosensitive resin composition containing the thioether group-containing (meth)acrylic resin (a) has excellent developability when subjected to photolithography using an alkaline aqueous solution as a developer.

[0086]

[0087] In one embodiment, the thioether group-containing (meth)acrylic resin (a) may contain a structural unit represented by the general formula (MA) as structural unit B in addition to the structural unit represented by formula (1) or formula (2). The structural unit represented by the general formula (MA) generates two carboxyl groups by ring opening in an alkaline developer. Therefore, the thioether group-containing (meth)acrylic resin (a) containing this structural unit has excellent developability. When the thioether group-containing (meth)acrylic resin (a) contains the structural unit represented by the general formula (MA), the proportion of the structural unit represented by the general formula (MA) in all the structural units of the thioether group-containing (meth)acrylic resin (a) is preferably 1 to 10 mol%, and more preferably 2 to 7 mol%.

[0088]

[0089] In one embodiment, the thioether group-containing (meth) acrylic resin (a) may contain a structural unit C derived from a monomer polymerizable with respect to the monomer represented by the general formula (NBm) and maleic anhydride. The structural unit C is, for example, a structural unit derived from the following compounds: substituted or unsubstituted, indene, maleimide, styrene, acenaphthene, norbornadiene, dihydrofuran, terpene compounds (e.g., pinene, limonene, etc.), linear olefins (e.g., pentene, etc.), cyclic olefins (e.g., cyclohexene, etc.), cyclododecatriene, tricycloundecene, dialkyl fumarate (e.g., dimethyl fumarate, ethyl fumarate, dibutyl fumarate, etc.), coumarin, (meth) acrylic acid compounds (e.g., methyl methacrylate, methyl acrylate), vinyl acetate, vinyl ether (e.g., 2-hydroxyethyl vinyl ether, etc.). Examples of substituents that these monomers may have include alkyl groups and aryl groups.

[0090] More specifically, examples of the substituted indene include methylindene and the like.

[0091] Examples of the substituted maleimide include cyclohexylmaleimide and phenylmaleimide, and examples of the substituted styrene include methylstyrene and vinyltoluene.

[0092] Among them, the structural unit C preferably contains a structural unit represented by the general formula (4) (a divalent structural unit derived from a substituted or unsubstituted indene), a structural unit represented by the general formula (5) (a divalent structural unit derived from a substituted or unsubstituted maleimide), a structural unit represented by the general formula (6) (a divalent structural unit derived from a substituted or unsubstituted styrene) or a structural unit represented by the general formula (7) (a divalent structural unit derived from a substituted or unsubstituted norbornadiene).

[0093]

[0094] In the general formula (4), R 1 and R 2 Each independently represents a hydrogen atom, an alkyl group or an aryl group. 3 represents a hydrogen atom, an alkyl group or an aryl group. 4 ~R 6 Each independently represents a hydrogen atom, an alkyl group or an aryl group. 7 ~R 10 Each independently represents a hydrogen atom, a hydroxyl group or an organic group having 1 to 30 carbon atoms.

[0095] Among the structural units represented by the general formula (NB) constituting the thioether group-containing (meth)acrylic resin (a), as the structural units that can constitute R 1 ~R 4 The organic group having 1 to 30 carbon atoms may include substituted or unsubstituted straight-chain or branched alkyl groups having 1 to 30 carbon atoms, and more specifically, may include alkyl groups, alkenyl groups, alkynyl groups, alkylene groups, aryl groups, aralkyl groups, alkaryl groups, cycloalkyl groups, alkoxy groups, heterocyclic groups, carboxyl groups, etc.

[0096] Examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl and decyl groups.

[0097] Examples of the alkenyl group include an allyl group, a pentenyl group, and a vinyl group.

[0098] Examples of the alkynyl group include ethynyl group and the like.

[0099] Examples of the alkylene group include a methylene group and an ethylene group.

[0100] Examples of the aryl group include tolyl, xylyl, phenyl, naphthyl and anthracenyl.

[0101] Examples of the aralkyl group include a benzyl group and a phenethyl group.

[0102] Examples of the alkaryl group include tolyl and xylyl groups.

[0103] Examples of the cycloalkyl group include adamantyl, cyclopentyl, cyclohexyl, and cyclooctyl.

[0104] Examples of the alkoxy group include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, a sec-butoxy group, an isobutoxy group, a tert-butoxy group, an n-pentoxy group, a neopentoxy group, and an n-hexyloxy group.

[0105] Examples of the heterocyclic group include an epoxy group and an oxetane group.

[0106] As R in the structural unit represented by the general formula (NB) 1 , R 2 , R 3 and R 4 , preferably hydrogen or alkyl, more preferably hydrogen.

[0107] In addition, R 1 , R 2 , R 3 and R 4 The hydrogen atoms in the organic group having 1 to 30 carbon atoms may be substituted by any atomic group. For example, they may be substituted by fluorine atoms, hydroxyl groups, carboxyl groups, etc. More specifically, R 1 , R 2 , R 3 and R 4 The organic group having 1 to 30 carbon atoms can be selected from fluorinated alkyl groups.

[0108] In the structural unit represented by the general formula (NB), a1 is preferably 0 or 1, and more preferably 0.

[0109] The ratio of the structural unit represented by the general formula (NB) in all structural units of the thioether group-containing (meth)acrylic resin (a) is preferably 10 to 90 mol %, more preferably 30 to 70 mol %, and further preferably 40 to 60 mol %.

[0110] In one embodiment, the thioether group-containing (meth)acrylic resin (a) has a structural unit represented by the general formula (1), in other words, has either or both of a structural unit containing two or more (meth)acryloyl groups (-C(=O)-CH=CH2 and a structural unit represented by the general formula (2), which is preferred because it can further improve the sensitivity of the thioether group-containing (meth)acrylic resin (a) in the exposure process.

[0111] In the structural unit represented by the general formula (1) that can constitute the thioether group-containing (meth)acrylic resin (a), R p It is a group containing two or more (meth)acryloyl groups, preferably a group containing 2 to 6 (meth)acryloyl groups, and more preferably a group containing 3 to 5 (meth)acryloyl groups. p The number of (meth)acryloyl groups contained can further improve the sensitivity of the sulfide group-containing (meth)acrylic resin (a) in the exposure process. In addition, it is easy to achieve a higher balance between the sensitivity and alkali solubility of the sulfide group-containing (meth)acrylic resin (a). In addition, the heat resistance of the sulfide group-containing (meth)acrylic resin (a) can be improved.

[0112] R in the general formula (1) p Preferably, the group is represented by the general formula (1b), the group is represented by the general formula (1c), or the group is represented by the general formula (1d), and at least one selected from these is contained. By using such a group, the above-mentioned various effects tend to be easily obtained.

[0113]

[0114] In formula (1b):

[0115] k is 2 or 3.

[0116] R is a hydrogen atom or a methyl group, and a plurality of Rs may be the same or different.

[0117] X 1 is a single bond, an alkylene group having 1 to 6 carbon atoms, or a group represented by -ZX- (Z is -O- or -OCO-, and X is an alkylene group having 1 to 6 carbon atoms), and there are multiple X 1 Can be the same or different.

[0118] X 1 ' is a single bond, an alkylene group having 1 to 6 carbon atoms, or a group represented by -X'-Z'- (X' is an alkylene group having 1 to 6 carbon atoms, and Z' is -O- or -COO-).

[0119] X 2 It is a k+1-valent organic group having 1 to 12 carbon atoms.

[0120] From the viewpoint of further improving sensitivity (easiness of polymerization) and the like, R is preferably a hydrogen atom.

[0121] k may be 2 or 3, but is preferably 3 from the viewpoint of further improving the availability of raw materials and the sensitivity.

[0122] When X 1 In the case of an alkylene group having 1 to 6 carbon atoms, the alkylene group may be linear or branched.

[0123] When X 1 When X is an alkylene group having 1 to 6 carbon atoms, 1 It is preferably a linear alkylene group, more preferably a linear alkylene group having 1 to 3 carbon atoms, and further preferably -CH2-(methylene group).

[0124] When X 1 In the case of a group represented by -ZX- (Z is -O- or -OCO-, and X is an alkylene group having 1 to 6 carbon atoms), the alkylene group having 1 to 6 carbon atoms in X may be linear or branched.

[0125] The alkylene group having 1 to 6 carbon atoms represented by X is preferably a linear alkylene group, more preferably a linear alkylene group having 1 to 3 carbon atoms, and further preferably -CH2-CH2-(ethylene) or -CH2-CH(CH3)-.

[0126] When X 1 ' is an alkylene group having 1 to 6 carbon atoms, and its specific embodiment is the same as X 1 same.

[0127] When X 1 When ' is a group represented by -X'-Z'-, the specific embodiment of X' is the same as that of X described above.

[0128] As X 2 The k+1-valent organic group having 1 to 12 carbon atoms may be any group formed by removing k+1 hydrogen atoms from any organic compound. The "any organic compound" herein is, for example, an organic compound having a molecular weight of 300 or less, preferably 200 or less, and more preferably 100 or less.

[0129] X 2 For example, it is a group formed by removing k+1 hydrogen atoms from a straight-chain or branched hydrocarbon having 1 to 12 carbon atoms (preferably 1 to 6 carbon atoms). More preferably, it is a group formed by removing k+1 hydrogen atoms from a straight-chain hydrocarbon having 1 to 3 carbon atoms. In addition, the hydrocarbon here may contain an oxygen atom (for example, an ether bond or a hydroxyl group). Furthermore, the hydrocarbon is preferably a saturated hydrocarbon.

[0130] As another way, X 2 The group containing a cyclic structure may be a group containing a cyclic structure. Examples of the group containing a cyclic structure include a group containing an alicyclic structure and a group containing a heterocyclic structure (for example, an isocyanuric acid structure).

[0131]

[0132] In formula (1c):

[0133] k, R, X 1 and X 2 Respectively with R, k, X in formula (1b) 1 and X 2 Synonymous, multiple R can be the same or different, multiple X 1 They may be the same as or different from each other.

[0134] X 3 It is a divalent organic group having 1 to 6 carbon atoms.

[0135] X 4 and X 5 Each independently represents a single bond or a divalent organic group having 1 to 6 carbon atoms.

[0136] X 6 It is a divalent organic group having 1 to 6 carbon atoms.

[0137] About R, k, and X 1 and X 2 The specific aspects, preferred aspects, etc. are the same as those described in the general formula (1b).

[0138] As X 3 and X 6 The divalent organic group having 1 to 6 carbon atoms may be, for example, a group obtained by removing two hydrogen atoms from a linear or branched hydrocarbon having 1 to 6 carbon atoms. In addition, the hydrocarbon here may contain an oxygen atom (for example, an ether bond or a hydroxyl group). Furthermore, the hydrocarbon is preferably a saturated hydrocarbon.

[0139] As X 4 and X 5 The divalent organic group having 1 to 6 carbon atoms includes a linear or branched alkylene group. The linear or branched alkylene group preferably has 1 to 3 carbon atoms.

[0140]

[0141] In the formula (1d), n is an integer of 2 to 5, and preferably 2 or 3.

[0142] Specific aspects, preferred aspects, etc. of R are the same as those described in the general formula (1b).

[0143] When the thioether group-containing (meth)acrylic resin (a) contains a structural unit represented by the general formula (1), the ratio of the structural unit represented by the general formula (1) in all the structural units of the thioether group-containing (meth)acrylic resin (a) is preferably 3 to 40 mol %, more preferably 3 to 30 mol %.

[0144] In the structural unit represented by the general formula (2) that can constitute the thioether group-containing (meth)acrylic resin (a), R S A group containing only one (meth)acryloyl group. In particular, in the design of a conventional photosensitive resin composition, when the curing property is increased in order to increase the sensitivity, the curing tends to be excessive and the developability tends to be deteriorated. On the other hand, when the developability is improved, the curing tends to be insufficient. Therefore, the thioether group-containing (meth)acrylic resin (a) preferably contains one or both of the structural unit represented by the general formula (1) and the structural unit represented by the general formula (2), thereby achieving both sensitivity and developability in a good balance.

[0145] R S For example, it is a group represented by the following formula (2a).

[0146]

[0147] In formula (2a), X 10 It is a divalent organic group, and R is a hydrogen atom or a methyl group.

[0148] X 10 The total number of carbon atoms in the moiety is preferably 1-30, more preferably 1-20, and even more preferably 1-10.

[0149] In formula (2a), X 10 It is a divalent organic group, and R is a hydrogen atom or a methyl group.

[0150] X 10 The total number of carbon atoms in the moiety is preferably 1-30, more preferably 1-20, and even more preferably 1-10.

[0151] As X 10 The divalent organic group is preferably an alkylene group. -CH2- as a part of the alkylene group may be an ether group (-O-). The alkylene group may be linear or branched, but is more preferably linear.

[0152] As X 10 The divalent organic group is preferably a linear alkylene group having 3 to 6 carbon atoms in total. 10 The number of carbon atoms (X 10The structural unit represented by formula (2) is easy to further participate in the cross-linking reaction, which can improve the sensitivity.

[0153] X 10 The divalent organic group (for example, alkylene) may be substituted by any substituent. Examples of the substituent include alkyl, aryl, alkoxy, and aryloxy groups.

[0154] And, X 10 The divalent organic group may be any group other than an alkylene group. For example, it may be a divalent group formed by linking one or more groups selected from an alkylene group, a cycloalkylene group, an arylene group, an ether group, a carbonyl group, a carboxyl group, and the like.

[0155] When the thioether group-containing (meth)acrylic resin (a) contains a structural unit represented by the general formula (2), the ratio of the structural unit represented by the general formula (2) in all the structural units of the thioether group-containing (meth)acrylic resin (a) is preferably 5 to 40 mol %, more preferably 10 to 30 mol %.

[0156] Furthermore, when the thioether group-containing (meth)acrylic resin (a) contains both the structural unit represented by the general formula (1) and the structural unit represented by the general formula (2), the total content of the structural unit represented by the general formula (1) and the structural unit represented by the general formula (2) in the thioether group-containing (meth)acrylic resin (a) is preferably 5 to 60 mol %, more preferably 10 to 50 mol %, and even more preferably 10 to 40 mol %, based on all the structural units constituting the thioether group-containing (meth)acrylic resin (a).

[0157] The content (ratio) of each structural unit contained in the thioether group-containing (meth)acrylic resin (a) can be determined by the charge amount (molar amount) of the raw materials used in synthesizing the polymer, the amount of the raw materials remaining after the synthesis, various spectra (e.g., IR spectrum, 1 H-NMR spectroscopy, 13 C-NMR spectrum) by estimating / calculating the presence and peak area of ​​peaks.

[0158] In the thioether group-containing (meth)acrylic resin (a) represented by the general formula (P'), X is hydrogen or an organic group having 1 to 30 carbon atoms. 1 ~R 4 The organic groups having 1 to 30 carbon atoms are the same.

[0159] In the thiol-containing (meth) acrylic resin (a) represented by the above general formula (P'), Y is an organic group (i) having 1 to 6 valencies and having 1 or more and 30 carbon atoms and derived from a difunctional or higher thiol-containing compound. In the present embodiment, the number of functional groups is the number of thiol groups. That is, the thiol-containing compound contains 2 or more thiol groups, and the organic group (i) is bonded to the structural units in []n and the structural units in []m via 1 to 6 thiol groups derived from the thiol groups. The organic group (i) may also have a thiol group that does not participate in the bonding with the structural units in []n and the structural units in []m, and the thiol-containing (meth) acrylic resin (a) can be obtained as a mixture of resins having n+m (number of bonds) of 1 to 6.

[0160] The organic group (i) having 1 to 30 carbon atoms is difunctional or more, preferably trifunctional or more. The upper limit is not particularly limited, but is hexafunctional or less.

[0161] From the viewpoint of the effect of the present invention, the valence of the organic group (i) having 1 to 30 carbon atoms is 1 to 6, preferably 2 to 6, and more preferably 3 to 6.

[0162] The monovalent to hexavalent organic group (i) having 1 to 30 carbon atoms may contain one or more atoms selected from O, N, S, P and Si. Examples of the monovalent to hexavalent organic group (i) having 1 to 30 carbon atoms include alkyl, alkenyl, alkynyl, alkylene, aryl, aralkyl, alkaryl, cycloalkyl, alkoxy and heterocyclic groups having 1 to 6 thioether groups (—S—* (* represents a connecting bond)).

[0163] Examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl and decyl. Examples of the alkenyl group include allyl, pentenyl and vinyl.

[0164] Examples of the alkynyl group include ethynyl group.

[0165] Examples of the alkylene group include a methylene group and an ethylene group. Examples of the aryl group include a tolyl group, a xylyl group, a phenyl group, a naphthyl group, and an anthracenyl group.

[0166] Examples of the aralkyl group include a benzyl group and a phenethyl group.

[0167] Examples of the alkaryl group include a tolyl group and a xylyl group.

[0168] Examples of the cycloalkyl group include adamantyl, cyclopentyl, cyclohexyl, and cyclooctyl.

[0169] Examples of the alkoxy group include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, a sec-butoxy group, an isobutoxy group, a tert-butoxy group, an n-pentoxy group, a neopentoxy group, and an n-hexoxy group.

[0170] Examples of the heterocyclic group include an epoxy group and an oxetane group.

[0171] Examples of the bifunctional or higher-functional thiol group-containing compound include compounds represented by the following chemical formulas (s-1) to (s-20).

[0172]

[0173]

[0174]

[0175] The difunctional or higher thiol group-containing compound may be used alone or in combination of two or more. Among them, tri- to hexafunctional (trivalent to hexavalent) thiol group-containing compounds having 3 to 6 thiol groups in one molecule are preferably used because of their excellent reactivity with other monomers.

[0176] The monovalent to hexavalent organic group (i) having 1 to 30 carbon atoms has a thiol group (-S-* (* is a linking bond)) derived from a thiol group of these thiol group-containing compounds at the terminal, and is bonded to the structural unit in []n and the structural unit in []m via the thiol group. The organic group (i) may have a thiol group that does not participate in the bond with the structural unit in []n and the structural unit in []m.

[0177] When a tetrafunctional (tetravalent) thiol group-containing compound represented by the chemical formula (s-2) is used as the bifunctional or higher-functional thiol group-containing compound, the thioether group-containing (meth)acrylic resin (a) of the present embodiment can have a structure represented by the following general formula (I), for example.

[0178]

[0179] In the general formula (I), A, B, C, X, p, q and r have the same meanings as in the general formula (P'). A, B, C, X, p, q and r contained in the structural units within the four [] may be the same or different.

[0180] In the general formula (I), the bonding order of A, B and C is not particularly limited, and any one of A, B and C may be bonded to the thioether group. In addition, in the general formula (I), an example is shown in which the thioether group derived from the compound represented by the chemical formula (s-2) is bonded to the 4 structural units in []. However, it may also be a structure in which 1 to 3 structural units in [] are bonded to the thioether group derived from the 4 thiols, and an organic group different from the structural units in [] is bonded to the remaining thioether group. In this embodiment, the (meth)acrylic resin (a) containing a thioether group can be obtained as a mixture containing at least one compound having 1 to 4 structures in [] bonded.

[0181] The weight average molecular weight Mw of the thioether group-containing (meth)acrylic resin (a) is, for example, 1,000 to 15,000, preferably 1,500 to 12,000, more preferably 2,000 to 10,000, and further preferably 3,000 to 8,000. By appropriately adjusting the weight average molecular weight, the sensitivity and solubility in an alkaline developer can be adjusted.

[0182] Furthermore, the dispersion degree (weight average molecular weight Mw / number average molecular weight Mn) of the sulfide group-containing (meth) acrylic resin (a) is preferably 1.0 to 5.0, more preferably 1.0 to 4.0, and further preferably 1.0 to 3.0. By appropriately adjusting the dispersion degree, the physical properties of the sulfide group-containing (meth) acrylic resin (a) can be made uniform, which is preferred. In addition, these values ​​can be obtained by measuring with gel permeation chromatography (GPC) using polystyrene as a standard substance.

[0183] The glass transition temperature of the thioether group-containing (meth) acrylic resin (a) is preferably 150 to 250°C, and more preferably 170 to 230°C. The thioether group-containing (meth) acrylic resin (a) has a relatively high glass transition temperature by mainly containing a structural unit represented by the general formula (NB). This is preferred from the viewpoint that a pattern formed on a substrate can be stably present when manufacturing a liquid crystal display device or a solid-state imaging element. In addition, the glass transition temperature can be obtained, for example, by differential thermal analysis (DTA).

[0184] The content (ratio) of each structural unit contained in the thioether group-containing (meth)acrylic resin (a) of the present embodiment can be determined based on the charge amount (molar amount) of the raw materials when synthesizing the polymer, the amount of the raw materials remaining after the synthesis, the peak areas of various spectra (for example, 1 H-NMR peak area) etc.

[0185] <Method for producing thioether group-containing (meth)acrylic resin (a)>

[0186] The method for producing the sulfide group-containing (meth)acrylic resin (a) will be described.

[0187] The (meth)acrylic resin (a) containing a thioether group can be produced (synthesized) by any method. The (meth)acrylic resin (a) containing a thioether group can be produced, for example, by the following steps: Step (I): a step of preparing a base polymer containing a structural unit represented by the general formula (NB), a structural unit represented by the general formula (MA) and the organic group (i) having a 1 to 6-valent carbon number of 1 or more and 30 or less; and Step (II): a step of making the base polymer obtained in step (I), a compound having a hydroxyl group and two or more (meth)acryloyl groups (hereinafter referred to as a "multifunctional (meth)acrylic monomer") and / or or a compound having a hydroxyl group and one (meth)acryloyl group (hereinafter referred to as a "monofunctional (meth)acrylic monomer"), in the presence of a basic catalyst, to react to prepare a thioether group-containing (meth)acrylic resin (a) containing a structural unit represented by the general formula (NB), the organic group (i) having a 1 to 6-valent carbon number of 1 to 30, a structural unit represented by the general formula (1) and / or a structural unit represented by the general formula (2), and optionally further containing a structural unit represented by the general formula (MA).

[0188] When the thioether group-containing (meth)acrylic resin (a) further contains a structural unit represented by the general formula (3), in step (II), a polymer containing a structural unit represented by the general formula (NB), a structural unit represented by the general formula (1) and / or a structural unit represented by the general formula (2) and a structural unit represented by the general formula (MA) is prepared, and then a step of treating the polymer with water in the presence of a base catalyst is carried out (step (III)).

[0189] When both a polyfunctional (meth)acrylic monomer and a monofunctional (meth)acrylic monomer are used in step (II), it is preferred to first react the polyfunctional (meth)acrylic monomer with the base polymer and then react the monofunctional (meth)acrylic monomer with the obtained reaction mixture.

[0190] (Step (I))

[0191] The step of preparing a base polymer containing a structural unit represented by the general formula (NB), a structural unit represented by the general formula (MA), and the organic group (i) having a 1 to 6-valent carbon number of 1 or more and 30 or less can be carried out by polymerizing (addition polymerization) a monomer composition containing a monomer represented by the general formula (NBm) and maleic anhydride in the presence of the thiol group-containing compound having two or more functional groups.1 , R 2 , R 3 and R 4 The definition of a1 is the same as that of the general formula (NB). The preferred embodiments are also the same.

[0192]

[0193] Examples of the monomer represented by the formula (NBm) include norbornene, bicyclo[2.2.1]-hept-2-ene (common name: 2-norbornene), 5-methyl-2-norbornene, 5-ethyl-2-norbornene, 5-butyl-2-norbornene, 5-hexyl-2-norbornene, 5-decyl-2-norbornene, 5-allyl-2-norbornene, 5-(2-propenyl)-2-norbornene, 5-(1-methyl-4-pentenyl)-2-norbornene, 5-ethynyl-2-norbornene, 5-benzyl-2-norbornene, 5-phenethyl-2-norbornene, 2-acetyl-5-norbornene, 5-norbornene-2-carboxylic acid methyl ester, and 5-norbornene-2,3-dicarboxylic anhydride. In the polymerization, the monomer represented by the formula (NBm) may be used alone or in combination of two or more.

[0194] In addition to containing the above-mentioned monomers, the monomer composition may also contain other monomers. As other monomers, as long as it is a copolymerizable compound with a double bond, it is not particularly limited and known compounds can be used, which can be polymerized with the monomer represented by the general formula (NBm) and maleic anhydride. As other monomers, substituted or unsubstituted indene, maleimide, styrene, acenaphthene, norbornadiene, dihydrofuran, terpene compounds (for example, pinene, limonene, etc.), straight-chain olefins (for example, pentene, etc.), cyclic olefins (cyclohexene, etc.), cyclododecatriene, tricycloundecene, dialkyl fumarate (for example, dimethyl fumarate, ethyl fumarate, dibutyl fumarate, etc.), coumarin, (meth) acrylic acid compounds (for example, methyl methacrylate, methyl acrylate), vinyl acetate, vinyl ether (for example, 2-hydroxyethyl vinyl ether, etc.), etc. can be cited. In step (I), the monomer represented by general formula (NBm), maleic anhydride, and, if necessary, other monomers can be polymerized (addition polymerization) in the presence of the bifunctional or higher-functional thiol group-containing compound.

[0195] Examples of the bifunctional or higher thiol group-containing compound include, but are not limited to, the compounds represented by the chemical formulae (s-1) to (s-20). The bifunctional or higher thiol group-containing compound may be used alone or in combination of two or more.

[0196] The polymerization method is not limited, but free radical polymerization using a free radical polymerization initiator is preferred. As the polymerization initiator, for example, an azo compound, an organic peroxide, etc. can be used.

[0197] Specific examples of the azo compound include azobisisobutyronitrile (AIBN), 2,2′-azobis(2-methylpropionic acid)dimethyl ester, and 1,1′-azobis(cyclohexanecarbonitrile) (ABCN).

[0198] Examples of the organic peroxide include hydrogen peroxide, di(tertiary)butyl peroxide (DTBP), benzoyl peroxide (BPO), and methyl ethyl ketone peroxide (MEKP).

[0199] The polymerization initiator may be used alone or in combination of two or more.

[0200] As the solvent used in the polymerization reaction, for example, an organic solvent such as diethyl ether, tetrahydrofuran, toluene, methyl ethyl ketone, etc. can be used. The polymerization solvent may be a single solvent or a mixed solvent.

[0201] The synthesis of the base polymer can be carried out by dissolving the monomer represented by formula (NBm), maleic anhydride and a polymerization initiator in a solvent and placing the mixture in a reaction vessel, followed by heating and dropwise addition polymerization of the bifunctional or higher thiol group-containing compound. The heating temperature is, for example, 50 to 80° C., and the heating time is, for example, 5 to 20 hours.

[0202] The molar ratio of the monomer represented by the formula (NBm) to maleic anhydride when charged into the reaction container is preferably 0.5:1 to 1:0.5. From the viewpoint of controlling the molecular structure, the molar ratio is preferably 1:1.

[0203] Furthermore, from the viewpoint of controlling the sulfide group content in the base polymer and the molecular weight of the base polymer, the amount of the bifunctional or higher thiol group-containing compound charged is preferably 0.5 to 10 mol %, particularly preferably 1 to 8 mol %, and further preferably 2 to 6 mol %, relative to the total molar amount of the monomer represented by the formula (NBm) and maleic anhydride charged into the reaction container.

[0204] Through such steps, a "base polymer" can be obtained.

[0205] In addition, the base polymer may be any of a random copolymer, an alternating copolymer, a block copolymer, a periodic copolymer, etc. A typical example is a random copolymer or an alternating copolymer. In addition, maleic anhydride is generally known as a monomer with strong alternating copolymerizability.

[0206] After the raw material polymer is synthesized, a step of removing low molecular weight components such as unreacted monomers, oligomers, and residual polymerization initiators may be performed.

[0207] Specifically, the organic phase containing the synthesized base polymer and low molecular weight components is concentrated, and then mixed with an organic solvent such as tetrahydrofuran (THF) to obtain a solution. Then, the solution is mixed with a poor solvent such as methanol to precipitate the monomer. The precipitate is filtered and dried, thereby improving the purity of the base polymer.

[0208] (Step (II))

[0209] The base polymer obtained in step (I) is reacted with a polyfunctional (meth)acrylic monomer and / or a monofunctional (meth)acrylic monomer in the presence of a basic catalyst to ring-open a portion of the structural unit represented by formula (MA) contained in the base polymer to form a structural unit represented by formula (1) and / or a structural unit represented by formula (2), thereby obtaining a thioether group-containing (meth)acrylic resin (a) comprising a structural unit represented by general formula (NB), the monovalent to hexavalent organic group (i) having 1 to 30 carbon atoms, and a structural unit represented by general formula (1) and / or a structural unit represented by general formula (2), and optionally a structural unit represented by formula (MA).

[0210] More specifically, first, a solution is prepared by dissolving the base polymer in an appropriate organic solvent. As the organic solvent, a single solvent or a mixed solvent such as methyl ethyl ketone (MEK), propylene glycol monomethyl ether acetate (PGMEA), dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), tetrahydrofuran (THF) can be used, but it is not limited to these, and various organic solvents used in the synthesis of organic compounds or polymers can be used.

[0211] When a polymer containing a structural unit represented by the general formula (NB) and both a structural unit represented by the general formula (1) and a structural unit represented by the general formula (2) is obtained, a multifunctional (meth)acrylic monomer is then added to the above solution. A basic catalyst is further added. Then, the solution is appropriately mixed to form a uniform solution, thereby obtaining a polymer having a structure containing at least a structural unit of the general formula (NB) and a structural unit of the general formula (1) and the organic group (i) having 1 to 30 carbon atoms bonded via 1 to 6 thioether groups (step (II-i)).

[0212] Examples of the polyfunctional (meth)acrylic monomer that can be used herein include compounds represented by formula (1b-m), compounds represented by formula (1c-m), and compounds represented by formula (1d-m).1 , X 1 ' and X 2 The definition and specific method of are the same as those in the above formula (1b). In addition, k, R, X in formula (1c-m) 1 , X 2 , X 3 , X 4 , X 5 and X 6 The definition and specific form of are the same as those in the above formula (1c). n and R in formula (1d-m) are the same as those in the above formula (1d).

[0213]

[0214] Next, a monofunctional (meth)acrylic monomer is reacted with the polymer obtained in step (II-i) in the presence of a basic catalyst, thereby obtaining a polymer having a structure containing at least a structural unit of the general formula (NB), a structural unit of the general formula (1), and a structural unit of the general formula (2), and the organic group (i) having 1 to 30 carbon atoms bonded via 1 to 6 thioether groups (step (II-ii)).

[0215] As the basic catalyst, an amine compound or a nitrogen-containing heterocyclic compound known in the field of organic synthesis can be appropriately used. For example, an amine compound or a nitrogen-containing heterocyclic compound such as triethylamine, pyridine, or dimethylaminopyridine can be used as a catalyst. The amount of the basic catalyst used can be set to about 10 to 60 parts by mass, for example, relative to 100 parts by mass of the base polymer. In addition, it should be noted that if the basic catalyst is excessively used, the amount of acid required for neutralization increases, and purification may become complicated.

[0216] The ring-opening of the structural unit of the general formula (MA) contained in the base polymer and the formation of the structural unit of the general formula (1) are carried out by heating the above solution preferably at 60 to 80° C. for about 3 to 9 hours.

[0217] Furthermore, for example, by additionally adding a monofunctional (meth)acrylic compound having a hydroxyl group to the reaction system during the heating, the structural unit represented by the general formula (3) can be generated in the thioether group-containing (meth)acrylic resin (a).

[0218] From the viewpoint of steric hindrance of the reaction, etc., a monofunctional (meth)acrylic compound having a hydroxyl group tends to react with the base polymer more easily than a polyfunctional (meth)acrylic compound having a hydroxyl group. Therefore, when the structural unit represented by the general formula (3) is generated in the thioether group-containing (meth)acrylic resin (a), it is preferred that the monofunctional (meth)acrylic compound having a hydroxyl group is not charged into the reaction system from the beginning but is additionally added to the reaction system.

[0219] Examples of the monofunctional (meth)acrylic compound having a hydroxyl group include compounds represented by the following general formula (2a-m).

[0220] In the general formula (2a-m), with respect to X 10 and R are defined as in the general formula (2a).

[0221]

[0222] Specific examples of the compound represented by the general formula (2a-m) include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and 2-(meth)acryloyloxyethyl-2-hydroxyethyl-phthalic acid.

[0223] When a polymer containing a structural unit represented by formula (NB), the organic group (i) having a 1-6 valence and having 1 to 30 carbon atoms, and any one selected from the structural unit represented by formula (1) and the structural unit represented by formula (2) is obtained, after step (I), only one of step (II-i) and step (II-ii) may be performed.

[0224] (Step (III))

[0225] When the step (III) is carried out, a step of treating the polymer obtained in the step (II) with water in the presence of a basic catalyst is used. By the step (III), the structural unit represented by the general formula (MA) contained in the polymer obtained in the step (II) is ring-opened to form the structural unit represented by the general formula (3), thereby producing a thioether group-containing (meth)acrylic resin (a) containing a structural unit represented by the general formula (NB), a structural unit represented by the general formula (1) and / or a structural unit represented by the general formula (2), and a structural unit represented by the general formula (3). When a part of the structural unit represented by the general formula (MA) is ring-opened and a part of the structural unit of the general formula (MA) remains without ring-opening, the thioether group-containing (meth)acrylic resin (a) contains a structural unit represented by the general formula (MA) in addition to the structural unit of the general formula (NB), the general formula (1) and / or the general formula (2), the organic group (i) having a valence of 1 to 6 and having 1 or more and 30 or less carbon atoms, and the structural unit of the general formula (3).

[0226] Examples of the basic catalyst used in step (III) include amine compounds such as triethylamine, pyridine, and dimethylaminopyridine, and nitrogen-containing heterocyclic compounds.

[0227] In step (III), water is added to the reaction system containing the polymer obtained in step (II), and the obtained reaction solution is preferably heated at 60 to 80° C. for about 0.25 to 6 hours, thereby the structural unit of formula (MA) contained in the polymer is ring-opened to generate the structural unit represented by formula (3). The basic catalyst can directly use the catalyst remaining in the reaction system obtained in step (II). Therefore, step (III) is preferably implemented by adding water to the reaction mixture in situ without performing any post-treatment on the reaction mixture obtained in step (II).

[0228] The sulfide group-containing (meth)acrylic resin (a) of the present embodiment can be obtained through the above steps. However, from the viewpoint of the effect of the present invention, the following steps may be further appropriately performed in order to remove unnecessary components other than the desired polymer.

[0229] First, the reaction solution diluted with an organic solvent and added with an acid (e.g., formic acid) is vigorously stirred for at least 3 minutes using a separatory funnel. The reaction solution is allowed to stand for more than 30 minutes to separate into an organic phase and an aqueous phase, and the aqueous phase is removed. In this way, an organic solution of a polymer is obtained.

[0230] The obtained organic solution of the sulfide group-containing (meth)acrylic resin (a) is purified by a reprecipitation method or a liquid-liquid extraction method. In the reprecipitation method, the obtained organic solution of the sulfide group-containing (meth)acrylic resin (a) is added to an excess of toluene or water to reprecipitate a polymer. Furthermore, the polymer powder obtained by the reprecipitation is further washed multiple times with toluene or water.

[0231] Furthermore, in order to remove formic acid or the alkaline catalyst, the operation of washing the obtained polymer powder with ion-exchanged water is repeated several times (about 1 to 3 times).

[0232] A high-purity polymer can be obtained by drying the polymer powder washed with ion-exchanged water at, for example, 30 to 60° C. for 16 hours or more.

[0233] In the liquid-liquid extraction method, water is added to the obtained organic solution of the (meth) acrylic resin (a) containing a thioether group, and vigorously stirred for at least 3 minutes with a separatory funnel. It is left to stand for more than 30 minutes, separated into an organic phase and an aqueous phase, and the aqueous phase is removed. Water is further added to the organic solution of the polymer after the aqueous phase is removed, and vigorously stirred for at least 3 minutes with a separatory funnel. It is left to stand for more than 30 minutes, separated into an organic phase and an aqueous phase, and the aqueous phase is removed. In this way, an organic solution of the polymer is obtained. If necessary, the steps of adding water and removing the aqueous phase can be further performed.

[0234] The obtained polymer organic solution is concentrated by heating under reduced pressure using a rotary evaporator, and then repeatedly adding a final solvent (PGMEA, etc.) to dilute the solution, thereby obtaining a polymer solution of the thioether group-containing (meth)acrylic resin (a) dissolved in the final solvent.

[0235] Furthermore, the polymer solution may contain a monofunctional (meth)acrylic compound used when synthesizing the thioether group-containing (meth)acrylic resin (a). When the polymer solution contains the monofunctional (meth)acrylic compound, by setting the peak area derived from the monofunctional (meth)acrylic compound in the gel permeation chromatography (GPC) chart to 5 to 50%, particularly 10 to 35%, relative to the peak area of ​​the thioether group-containing (meth)acrylic resin (a), it is possible to achieve a good balance between alkali solubility and sensitivity of the obtained photosensitive resin composition.

[0236] (Resin composition)

[0237] The resin composition of the present embodiment contains the above-mentioned polymer P. In a preferred embodiment, the resin composition of the present embodiment contains a thioether group-containing (meth)acrylic resin (a). Furthermore, the resin composition of the present embodiment can contain various components depending on its application.

[0238] Hereinafter, each component will be described.

[0239] When the resin composition of the present embodiment is used as a photosensitive resin composition, it contains the above-mentioned thioether group-containing (meth)acrylic resin (a) and a photosensitizer.

[0240] Hereinafter, a resin composition containing a photosensitizer is referred to as a photosensitive resin composition.

[0241] Examples of the photosensitizer for imparting photosensitivity to the resin composition of the present embodiment include a photoradical polymerization initiator.As the photoradical polymerization initiator, a known compound can be used, for example, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propane-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropane-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4- benzophenone compounds such as benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, etc.; thioxanthone compounds such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, etc.; 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-ethyl)- halogenated methylated triazine compounds such as 2-(4-ethoxycarbonylnaphthyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-ethoxycarbonylnaphthyl)-4,6-bis(trichloromethyl)-s-triazine; halogenated methylated oxadiazole compounds such as 2-trichloromethyl-5-(2'-benzofuranyl)-1,3,4-oxadiazole, 2-trichloromethyl-5-[β-(2'-benzofuranyl)vinyl]-1,3,4-oxadiazole, 4-oxadiazole, 2-trichloromethyl-5-furanyl-1,3,4-oxadiazole; 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4-dichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole , 2,2'-bis(2,4,6-trichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole and other biimidazole compounds; 1,2-octanedione, 1-〔4-(phenylthio)-2-(O-benzoyl oxime)〕, ethyl ketone (ethanone), 1-〔9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl〕-1-(O-acetyl oxime) and other oxime ester compounds; bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium and other titanocene compounds; benzoic acid ester compounds such as p-dimethylaminobenzoic acid and p-diethylaminobenzoic acid; acridine compounds such as 9-phenylacridine, etc.The photoradical polymerization initiator may be used alone or in combination of two or more.

[0242] The photoradical polymerization initiator is used in an amount of, for example, 1 to 20 parts by mass, and preferably 3 to 10 parts by mass, based on 1000 parts by mass of the polymer P.

[0243] The photosensitive resin composition of the present embodiment has high sensitivity in photolithography by containing the above-mentioned components, and has excellent alkali solubility. Therefore, the photosensitive resin composition has excellent developability and excellent processability in photolithography. In addition, since the yellowing of the photosensitive resin composition is suppressed, the article obtained by curing the photosensitive resin composition has transparency.

[0244] The photosensitive resin composition of this embodiment may contain a compound having two or more (meth)acryloyl groups (multifunctional (meth)acrylic compound). By containing such a compound, the alkali solubility of the photosensitive resin composition is improved, and the yellowing of the photosensitive resin composition is reduced, thereby obtaining a cured product with excellent transparency.

[0245] Examples of the polyfunctional (meth)acrylic compound that can be used in the photosensitive resin composition of the present embodiment include, but are not limited to, the compounds represented by the following formula (1b-p), the compounds represented by the following formula (1c-p), and the compounds represented by the following formula (1d-p). 1 , X 1 ' and X 2 The definition and specific method of are the same as those in the above formula (1b). In addition, k, R, X in formula (1c-p) 1 , X 2 , X 3 , X 4 , X 5 and X 6 The definition and specific method of are the same as those in the above formula (1c). n and R in formula (1d-p) are the same as those in the above formula (1d). Y in formula (1b-p), formula (1c-p) and formula (1d-p) is a hydrogen atom or a (meth)acryloyl group or a combination thereof.

[0246]

[0247] The photosensitive resin composition of the present embodiment may contain a compound having one (meth)acryloyl group (monofunctional (meth)acrylic compound). By containing the monofunctional (meth)acrylic compound, the alkali solubility of the obtained resin composition is improved, and yellowing is further reduced.

[0248] Examples of the monofunctional (meth)acrylic compound that can be used in the photosensitive resin composition of the present embodiment include compounds represented by the following formula (2a-m). 10 and R are defined the same as in formula (2a).

[0249]

[0250] Specific examples of the compound represented by formula (2a-m) include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and 2-(meth)acryloyloxyethyl-2-hydroxyethyl-phthalic acid.

[0251] When the polyfunctional (meth)acrylic compound is added to the photosensitive resin composition of the present embodiment, it is preferably added in an amount such that the peak area derived from the polyfunctional (meth)acrylic compound in the gel permeation chromatography (GPC) chart of the photosensitive resin composition is 5 to 100%, more preferably 10 to 90%, and even more preferably 15 to 80%. By adding the polyfunctional (meth)acrylic compound in the above range, the obtained photosensitive resin composition has excellent alkali solubility.

[0252] When a monofunctional (meth)acrylic compound is added to the photosensitive resin composition of the present embodiment, the amount thereof is preferably such that the peak area derived from the monofunctional (meth)acrylic compound in the gel permeation chromatography (GPC) chart of the photosensitive resin composition is 5 to 50%, and more preferably 10 to 35%. By adding the monofunctional (meth)acrylic compound in the above range, the obtained photosensitive resin composition has excellent alkali solubility.

[0253] When a polyfunctional (meth)acrylic compound and / or a monofunctional (meth)acrylic compound is added to the photosensitive resin composition of the present embodiment, these (meth)acrylic compounds may be monomers remaining when synthesizing a resin having a (meth)acrylic group, or may be separately added to the resin composition.

[0254] The photosensitive resin composition of the present embodiment may also contain a thiol-containing compound. As the thiol-containing compound, the thiol-containing compound may be used. The photosensitive resin composition containing the thiol-containing compound may be prepared by adding a thiol-containing compound after synthesizing the (meth) acrylic resin (a) containing a thiol group, or a reaction solution containing an unreacted thiol-containing compound remaining after the mercapto group introduction reaction may be used. As a result, the yellowing of the photosensitive resin composition is suppressed and the heat discoloration resistance is improved. In order to improve the heat discoloration resistance of the obtained photosensitive resin composition, it is preferred to use a compound having more than two thiol groups. Among them, in order to further improve the heat discoloration resistance, it is more preferred to use a multifunctional thiol-containing compound having 3 to 6 thiol groups. The thiol-containing compound may be primary or secondary. In addition, the thiol-containing compound may be used alone or in combination of two or more.

[0255] When the thiol group-containing compound is added to the photosensitive resin composition of the present embodiment, the amount thereof is 0.25 to 20% by mass, preferably 0.5 to 15% by mass, and more preferably 1 to 12% by mass, relative to the polymer P.

[0256] By using the thiol group-containing compound in an amount within the above range, the sensitivity of the photosensitive resin composition can be maintained and the heat discoloration resistance can be improved.

[0257] As one embodiment, the photosensitive resin composition may contain a colorant. By containing a colorant, it can be preferably used as a material for forming a color filter of a liquid crystal display device or a solid-state imaging element. As the colorant, various pigments or dyes can be used.

[0258] As the pigment, an organic pigment or an inorganic pigment can be used.

[0259] As organic pigments, azo pigments, phthalocyanine pigments, quinacridone pigments, perylene pigments, perinone pigments, isoindolinone pigments, isoindolinone pigments, dioxazine pigments, thioindigo pigments, anthraquinone pigments, quinophthalone pigments, metal complex pigments, diketopyrrolopyrrole pigments, xanthene pigments, pyrromethene pigments, dye lake pigments, etc. can be used.

[0260] As inorganic pigments, white / extender pigments (titanium oxide, zinc oxide, zinc sulfide, clay, talc, barium sulfate, calcium carbonate, etc.), colored pigments (chrome yellow, cadmium series, chrome vermilion, nickel titanium, chrome titanium, yellow iron oxide, hematite (Bengala), zinc chromate, red lead, ultramarine, iron blue, cobalt blue, chrome green, chromium oxide, bismuth vanadate, etc.), brightening material pigments (pearlescent pigments, aluminum pigments, bronze pigments, etc.), fluorescent pigments (zinc sulfide, strontium sulfide, strontium aluminate, etc.) can be used.

[0261] As the dye, for example, known dyes described in Japanese Patent Application Laid-Open No. 2003-270428, Japanese Patent Application Laid-Open No. 9-171108, Japanese Patent Application Laid-Open No. 2008-50599, etc. can be used.

[0262] When the photosensitive resin composition contains a colorant, the photosensitive resin composition may contain only one type of colorant, or may contain two or more types of colorants.

[0263] Colorants (especially pigments) can have an appropriate average particle size depending on the purpose or application. When transparency such as a color filter is particularly required, a small average particle size of less than 0.1 μm is preferably used. In addition, when hiding properties such as coatings are required, a large average particle size of more than 0.5 μm is preferably used.

[0264] The colorant may be subjected to surface treatment such as rosin treatment, surfactant treatment, resin dispersant treatment, pigment derivative treatment, oxide film treatment, silica coating, wax coating, etc. depending on the purpose or use.

[0265] When the photosensitive resin composition contains a colorant, the amount thereof may be appropriately set depending on the purpose or application, but from the viewpoint of achieving both color concentration and dispersion stability of the colorant, the amount is preferably 3 to 70% by mass, more preferably 5 to 60% by mass, and even more preferably 10 to 50% by mass, relative to the total non-volatile components (components other than the solvent) of the photosensitive resin composition.

[0266] As one embodiment, the photosensitive resin composition may contain a light-shielding agent. By containing a light-shielding agent, it can be preferably used as a material for forming a black matrix of a liquid crystal display device or a solid-state imaging element.

[0267] As the light shielding agent, a known light shielding agent can be used without particular limitation. For example, black pigments such as carbon black, bone black, graphite, iron black, and titanium black can be used as the light shielding agent.

[0268] When the photosensitive resin composition contains a light-shielding agent, the photosensitive resin composition may contain only one type of light-shielding agent, or may contain two or more types.

[0269] When the photosensitive resin composition contains a light-shielding agent, the amount thereof may be appropriately set depending on the purpose or application. However, from the viewpoint of achieving both light-shielding performance and dispersion stability of the light-shielding agent, the amount is preferably 3 to 70% by mass, more preferably 5 to 60% by mass, and even more preferably 10 to 50% by mass, relative to the total non-volatile components (components other than the solvent) of the photosensitive resin composition.

[0270] The photosensitive resin composition typically contains a solvent. As the solvent, an organic solvent can be preferably used. Specifically, one or more of ketone solvents, ester solvents, ether solvents, alcohol solvents, lactone solvents, carbonate solvents, etc. can be used.

[0271] Examples of solvents include propylene glycol monomethyl ether (PGME), propylene glycol monomethyl ether acetate (PGMEA), ethyl lactate, methyl isobutyl carbinol (MIBC), γ-butyrolactone (GBL), N-methylpyrrolidone (NMP), methyl n-amyl ketone (MAK), diethylene glycol monomethyl ether, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, cyclohexanone or a mixture thereof.

[0272] The amount of the solvent used is not particularly limited, and the solvent is used in an amount such that the concentration of the nonvolatile component becomes, for example, 10 to 70% by mass, preferably 15 to 60% by mass.

[0273] As one embodiment, the photosensitive resin composition may contain a crosslinking agent.

[0274] The crosslinking agent is not particularly limited as long as it can crosslink the polymer (can chemically bond with the polymer) by the action of active chemical species generated from the photopolymerization initiator. The crosslinking agent can not only chemically bond with the polymer, but also react with each other to form a bond.

[0275] The crosslinking agent is preferably a polyfunctional compound having two or more polymerizable double bonds in one molecule, and more preferably a polyfunctional (meth)acrylic compound having two or more (meth)acryloyl groups in one molecule (however, the crosslinking agent does not belong to the polymer). From the viewpoints of uniform curability and further improvement of sensitivity, it is preferred to use a crosslinking agent having the same type of crosslinking group (polymerizable double bond) as the crosslinking group (polymerizable double bond) possessed by the polymer.

[0276] The upper limit of the number of functions (the number of polymerizable double bonds) per molecule of the cross-linking agent is not particularly limited, but is, for example, 8 or less, and preferably 6 or less.

[0277] Specific examples of the cross-linking agent include the following.

[0278] Ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, bisphenol A alkylene oxide di(meth)acrylate, bisphenol F alkylene oxide di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, glycerol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ethylene oxide addition trimethylolpropane tri(meth)acrylate, ethylene oxide addition Polyfunctional (meth)acrylates such as ditrimethylolpropane tetra(meth)acrylate, ethylene oxide added pentaerythritol tetra(meth)acrylate, ethylene oxide added dipentaerythritol hexa(meth)acrylate, propylene oxide added trimethylolpropane tri(meth)acrylate, propylene oxide added ditrimethylolpropane tetra(meth)acrylate, propylene oxide added pentaerythritol tetra(meth)acrylate, propylene oxide added dipentaerythritol hexa(meth)acrylate, ε-caprolactone added trimethylolpropane tri(meth)acrylate, ε-caprolactone added ditrimethylolpropane tetra(meth)acrylate, ε-caprolactone added pentaerythritol tetra(meth)acrylate, and ε-caprolactone added dipentaerythritol hexa(meth)acrylate.

[0279] Ethylene glycol divinyl ether, diethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, butanediol divinyl ether, hexanediol divinyl ether, bisphenol A alkylene oxide divinyl ether, bisphenol F alkylene oxide divinyl ether, trimethylolpropane trivinyl ether, ditrimethylolpropane tetravinyl ether, propylene glycol trivinyl ether, pentaerythritol tetravinyl ether, dipentaerythritol pentavinyl ether, dipentaerythritol hexavinyl ether, ethylene oxide added trimethylolpropane trivinyl ether, ethylene oxide added ditrimethylolpropane tetravinyl ether, ethylene oxide added pentaerythritol tetravinyl ether, ethylene oxide added dipentaerythritol hexavinyl ether and other multifunctional vinyl ethers.

[0280] (Meth)acrylic acid esters containing a vinyl ether group, such as 2-vinyloxyethyl (meth)acrylate, 3-vinyloxypropyl (meth)acrylate, 1-methyl-2-vinyloxyethyl (meth)acrylate, 2-vinyloxypropyl (meth)acrylate, 4-vinyloxybutyl (meth)acrylate, 4-vinyloxycyclohexyl (meth)acrylate, 5-vinyloxypentyl (meth)acrylate, 6-vinyloxyhexyl (meth)acrylate, 4-vinyloxymethylcyclohexylmethyl (meth)acrylate, p-vinyloxymethylphenylmethyl (meth)acrylate, 2-(vinyloxyethoxy)ethyl (meth)acrylate, and 2-(vinyloxyethoxyethoxyethoxy)ethyl (meth)acrylate.

[0281] Ethylene glycol diallyl ether, diethylene glycol diallyl ether, polyethylene glycol diallyl ether, propylene glycol diallyl ether, butanediol diallyl ether, hexanediol diallyl ether, bisphenol A alkylene oxide diallyl ether, bisphenol F alkylene oxide diallyl ether, trimethylolpropane triallyl ether, ditrimethylolpropane tetraallyl ether, glycerol triallyl ether, pentaerythritol tetraallyl ether, dipentaerythritol pentaallyl ether, dipentaerythritol hexaallyl ether, ethylene oxide addition trimethylolpropane triallyl ether, ethylene oxide addition ditrimethylolpropane tetraallyl ether, ethylene oxide addition pentaerythritol tetraallyl ether, ethylene oxide addition dipentaerythritol hexaallyl ether and other multifunctional allyl ethers.

[0282] (Meth)acrylates containing an allyl group, such as allyl (meth)acrylate.

[0283] Isocyanurates containing a polyfunctional (meth)acryloyl group such as tris(acryloyloxyethyl)isocyanurate, tris(methacryloyloxyethyl)isocyanurate, alkylene oxide-added tris(acryloyloxyethyl)isocyanurate, and alkylene oxide-added tris(methacryloyloxyethyl)isocyanurate.

[0284] Polyfunctional allyl group-containing isocyanurates such as triallyl isocyanurate.

[0285] Polyfunctional amine ester (meth)acrylates obtained by reacting a polyfunctional isocyanate such as tolylene diisocyanate, isophorone diisocyanate, or xylene diisocyanate with a hydroxyl group-containing (meth)acrylate such as 2-hydroxyethyl (meth)acrylate or 2-hydroxypropyl (meth)acrylate.

[0286] Polyfunctional aromatic vinyls such as divinylbenzene.

[0287] Among them, trifunctional (meth)acrylates such as trimethylolpropane tri(meth)acrylate and pentaerythritol tri(meth)acrylate, tetrafunctional (meth)acrylates such as pentaerythritol tetra(meth)acrylate and ditrimethylolpropane tetra(meth)acrylate, and hexafunctional (meth)acrylates such as dipentaerythritol hexa(meth)acrylate are preferred.

[0288] When the photosensitive resin composition contains a crosslinking agent, the photosensitive resin composition may contain only one crosslinking agent or may contain two or more crosslinking agents. When the photosensitive resin composition contains a crosslinking agent, the amount thereof may be appropriately set according to the purpose or use. As an example, the amount of the crosslinking agent is generally 30 to 70 parts by mass relative to 100 parts by mass of the polymer P, and preferably can be set to about 40 to 60 parts by mass.

[0289] The photosensitive resin composition may contain fillers, binder resins other than the above-mentioned polymers, acid generators, heat resistance improvers, developing aids, plasticizers, polymerization inhibitors, ultraviolet absorbers, antioxidants, matting agents, defoaming agents, leveling agents, surfactants, antistatic agents, dispersants, lubricants, surface modifiers, thixotropic agents, thixotropic aids, silane coupling agents, polyvalent phenol compounds and other ingredients according to various purposes or required properties.

[0290] (film, color filter, black matrix, liquid crystal display device, and solid-state imaging element)

[0291] By using the above-mentioned photosensitive resin composition to form a film, and exposing / developing the film to form a pattern, a film with a pattern can be obtained. The film is suitable for a color filter or a black matrix, etc. That is, by using a photosensitive resin composition containing a colorant to form a pattern, a color filter can be obtained. And, by using a photosensitive resin composition containing a light-shielding agent to form a pattern, a black matrix can be obtained. Then, a liquid crystal display device or a solid-state imaging element with a color filter or a black matrix can be manufactured.

[0292] A typical procedure for forming a pattern is described.

[0293] (Formation of Photosensitive Resin Film)

[0294] For example, the photosensitive resin composition is applied onto an arbitrary substrate and dried as necessary, thereby firstly obtaining a photosensitive resin film.

[0295] The substrate to which the composition is applied is not particularly limited, and examples thereof include a glass substrate, a silicon wafer, a ceramic substrate, an aluminum substrate, a SiC wafer, a GaN wafer, and a copper-clad laminate.

[0296] The substrate may be an unprocessed substrate or a substrate with electrodes or elements formed on the surface. In order to improve adhesion, the substrate may be subjected to surface treatment.

[0297] The method for applying the photosensitive resin composition is not particularly limited, and the composition can be applied by spin coating using a spinner, spray coating using a spray coater, dipping, printing, roll coating, inkjet method, or the like.

[0298] The photosensitive resin composition applied on the substrate is typically dried by heating using a hot plate, hot air, an oven, etc. The heating temperature is usually 80 to 140° C., preferably 90 to 120° C. The heating time is usually 30 to 600 seconds, preferably about 30 to 300 seconds.

[0299] The thickness of the photosensitive resin film is not particularly limited and may be appropriately adjusted according to the final pattern to be obtained, and is usually 0.5 to 10 μm, preferably 1 to 5 μm. The film thickness can be adjusted by the content of the solvent in the photosensitive resin composition, the coating method, and the like.

[0300] (exposure)

[0301] The exposure is typically performed by irradiating the photosensitive resin film with active light through an appropriate mask.

[0302] As active light, for example, X-rays, electron beams, ultraviolet rays, visible light, etc. can be cited. In terms of wavelength, light of 200 to 500 nm is preferred. From the perspective of pattern resolution or operability, the light source is preferably g-rays, h-rays or i-rays of a mercury lamp, and i-rays are particularly preferred. In addition, two or more rays can be mixed and used. As an exposure device, a contact aligner, a mirror projection aligner or a stepper is preferred.

[0303] The amount of light for exposure can be appropriately adjusted according to the amount of photosensitizer in the photosensitive resin film, and is, for example, 100 to 500 mJ / cm 2 about.

[0304] In addition, after exposure, the photosensitive resin film may be heated again as needed (post-exposure heating: PostExposure Bake). The temperature is, for example, 70 to 150° C., preferably 90 to 120° C., and the time is, for example, 30 to 600 seconds, preferably 30 to 300 seconds. Post-exposure heating promotes the reaction based on free radicals generated from the photo-free radical polymerization initiator, further promoting the curing reaction.

[0305] (development)

[0306] By developing the exposed photosensitive resin film with an appropriate developer, a pattern can be obtained, and a substrate having a pattern can be manufactured.

[0307] In the development step, a suitable developer can be used to perform development by, for example, dipping, immersion, or spin spraying. By development, the exposed portion (in the case of a positive type) or the unexposed portion (in the case of a negative type) of the photosensitive resin film is dissolved and removed to obtain a pattern.

[0308] The developer that can be used is not particularly limited, and for example, an alkaline aqueous solution or an organic solvent can be used.

[0309] Specific examples of the aqueous alkali solution include (i) aqueous solutions of inorganic alkalis such as sodium hydroxide, sodium carbonate, sodium silicate, and ammonia; (ii) aqueous solutions of organic amines such as ethylamine, diethylamine, triethylamine, and triethanolamine; and (iii) aqueous solutions of quaternary ammonium salts such as tetramethylammonium hydroxide and tetrabutylammonium hydroxide.

[0310] Specific examples of the organic solvent include ketone solvents such as cyclopentanone, ester solvents such as propylene glycol monomethyl ether acetate (PGMEA) and butyl acetate, and ether solvents such as propylene glycol monomethyl ether.

[0311] To the developer, for example, a water-soluble organic solvent such as methanol or ethanol, a surfactant, etc. may be added.

[0312] In this embodiment, as the developer, an aqueous alkali solution is preferably used, and tetramethylammonium hydroxide, an aqueous sodium carbonate solution, or an aqueous potassium hydroxide solution is more preferably used.

[0313] The concentration of the aqueous alkali solution is preferably 0.1 to 10% by mass, more preferably 0.5 to 5% by mass.

[0314] Through the above steps, a pattern can be obtained / a substrate having a pattern can be manufactured, but various treatments may be performed after development.

[0315] For example, after development, the pattern and the substrate can be cleaned using a rinse solution. Examples of the rinse solution include distilled water, methanol, ethanol, isopropanol, propylene glycol monomethyl ether, etc. These can be used alone or in combination of two or more.

[0316] Furthermore, the obtained pattern can be heated to be fully cured. The heating temperature is typically 150 to 400° C., preferably 160 to 300° C., and more preferably 200 to 250° C. The heating time is not particularly limited, and is, for example, in the range of 15 to 300 minutes. The heat treatment can be performed using a hot plate, an oven, a temperature-raising oven capable of setting a temperature program, and the like. The ambient gas used for the heat treatment may be air, or an inert gas such as nitrogen or argon. Furthermore, the heating can be performed under reduced pressure.

[0317] An example of the structure of a liquid crystal display device and / or a solid-state imaging element having a color filter and / or a black matrix is ​​schematically shown in Figure 1 .

[0318] A black matrix 11 and a color filter 12 are formed on the substrate 10. A protective film 13 and a transparent electrode layer 14 are provided on the black matrix 11 and the color filter 12.

[0319] The substrate 10 is generally made of a material that allows light to pass, such as glass, polyester, polycarbonate, polyolefin, polysulfone, cyclic olefin polymer, etc. The substrate 10 may be subjected to corona discharge treatment, ozone treatment, chemical treatment, etc. as necessary.

[0320] The substrate 10 is preferably made of glass.

[0321] The black matrix 11 is composed of, for example, a cured product of a photosensitive resin composition containing a light-shielding agent.

[0322] There are generally three colors of red, green, and blue as the color filter 12. The color filter 12 is composed of a cured product of a photosensitive resin composition containing a colorant corresponding to each color.

[0323] The embodiments of the present invention are described above, but these are examples of the present invention, and various configurations other than the above can be adopted. In addition, the present invention is not limited to the above embodiments, and modifications and improvements within the scope of achieving the purpose of the present invention are included in the present invention.

[0324] [Example]

[0325] Embodiments of the present invention will be described in detail based on Examples and Comparative Examples. However, the present invention is not limited to Examples.

[0326] The compounds used in the Examples may be represented by the following abbreviations or trade names.

[0327] MA: maleic anhydride.

[0328] NB: 2-Norbornene.

[0329] MEK: Methyl Ethyl Ketone.

[0330] 4-HBA: 4-hydroxybutyl acrylate.

[0331] A-TMM-3LM-N: A mixture of the following two compounds, the amount of the left compound in the mixture measured by gas chromatography is about 57% (manufactured by Shin-Nakamura Chemical Co., Ltd.).

[0332]

[0333] TMMP: trimethylolpropane tris(3-mercaptopropionate), a thiol group-containing compound of the above formula (s-1) (manufactured by SC Organic Chemical Co., Ltd.).

[0334] PEMP: pentaerythritol tetrakis(3-mercaptopropionate), a thiol group-containing compound of the above formula (s-2) (manufactured by SC Organic Chemical Co., Ltd.).

[0335] DPMP: dipentaerythritol hexa(3-mercaptopropionate), a thiol group-containing compound of the above formula (s-3) (manufactured by SC Organic Chemical Co., Ltd.).

[0336] TEMPIC: tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, a thiol group-containing compound of the above formula (s-5) (manufactured by SC Organic Chemical Co., Ltd.).

[0337] PEPT: trimethylolpropane tris(3-mercaptopropionate), a thiol group-containing compound of the above formula (s-6) (manufactured by SC Organic Chemical Co., Ltd.).

[0338] Karenz MT (registered trademark) PE1: pentaerythritol tetrakis(3-mercaptobutyrate), a thiol group-containing compound of the above formula (s-9) (manufactured by SHOWA DENKO KK).

[0339] EGMP-4: Tetraethylene glycol bis(3-mercaptopropionate), a thiol group-containing compound of the above formula (s-4) (manufactured by SC Organic Chemical Co., Ltd.).

[0340] <Synthesis of base polymer>

[0341] (Synthesis of Base Polymer 1)

[0342] 588.36 g (6.0 mol) of maleic anhydride, 564.90 g (6.0 mol) of 2-norbornene, and 55.26 g (0.24 mol) of dimethyl 2,2'-azobis(2-methylpropionate) were weighed and placed in a reaction vessel of appropriate size equipped with a stirrer and a cooling tube, and these were dissolved in a mixed solvent consisting of 1716.8 g of methyl ethyl ketone and 188.3 g of toluene to prepare a solution.

[0343] Nitrogen was passed through the solution for 30 minutes to remove oxygen, and then the solution was heated at 65° C. for 1.5 hours while being stirred, and then further heated at 80° C. for 6 hours to polymerize maleic anhydride and 2-norbornene to prepare a polymerization solution.

[0344] The obtained polymerization solution was added dropwise to 14230.2 g of methanol to precipitate a white solid. The obtained white solid was further washed with 3557.5 g of methanol and then vacuum dried at 120° C. to obtain 1027.2 g of a polymer (raw polymer 1) having a structural unit derived from 2-norbornene and a structural unit derived from maleic anhydride.

[0345] The obtained polymer was measured by gel permeation chromatography (GPC). As a result, the weight average molecular weight Mw was 7236 and the polydispersity (weight average molecular weight Mw) / (number average molecular weight Mn) was 1.83.

[0346] (Synthesis of Base Polymer 2)

[0347] 50.21 g of a 75% toluene solution of 2-norbornene (37.66 g, 0.400 mol in terms of 2-norbornene), maleic anhydride (MAN, 39.22 g, 0.400 mol) and 191.47 g of methyl ethyl ketone (MEK) were added to a reaction vessel equipped with a stirrer, a cooling tube and a dropping funnel, and stirred and dissolved. Next, the dissolved oxygen in the system was removed by nitrogen bubbling, and the temperature was raised. When the internal temperature reached 80°C, a solution of 2,2'-azobisisobutyric acid dimethyl ester (Wako Pure Chemical Industries, Ltd., trade name: V-601, 3.68 g, 0.016 mol) and TMMP (6.38 g, 0.016 mol) dissolved in MEK 16.23 g was added over 1 hour. After that, the mixture was further reacted at 80°C for 7 hours. Next, the reaction mixture was cooled to room temperature. The obtained polymerization solution was added dropwise to 1228.8 g of methanol to precipitate a white solid. The obtained white solid was further washed with 307.2 g of methanol and then vacuum dried at 120° C. to obtain 67.0 g of a polymer (raw polymer 2) having a structural unit derived from 2-norbornene and a structural unit derived from maleic anhydride.

[0348] The obtained polymer was measured by gel permeation chromatography (GPC). As a result, the weight average molecular weight Mw was 3300 and the polydispersity (weight average molecular weight Mw) / (number average molecular weight Mn) was 1.74.

[0349] [Sulfur content in base polymer]

[0350] The amount of sulfur in the obtained polymer was confirmed by elemental analysis based on flask combustion and ion chromatography, and it was confirmed that sulfur element was present in the polymer. In addition, in the GPC measurement of the reaction solution before the dropwise addition of methanol, it was also confirmed that the peak derived from TMMP had disappeared, and TMMP was absorbed into the polymer.

[0351] The elemental analysis method is as follows.

[0352] - Experimental Project

[0353] Quantification of total sulfur by flask combustion-ion chromatography

[0354] -Test methods

[0355] Flask combustion ~ ion chromatography

[0356] (1) About 50 mg of a sample is completely burned in a sealed flask replaced with oxygen.

[0357] (2) The generated gas is captured in the hydrogen peroxide absorbing liquid previously added to the flask, and the volume is fixed to 50 ml as a test solution.

[0358] (3) The test solution and the standard solution are introduced into an ion chromatography analyzer, and the concentration of sulfate ions is determined by the calibration curve method to calculate the amount of sulfur contained in the sample.

[0359] -Device used

[0360] Dionex ICS-3000 Ion Chromatograph

[0361] (Synthesis of Base Polymer 3)

[0362] 50.21 g of a 75% toluene solution of 2-norbornene (37.66 g, 0.400 mol in terms of 2-norbornene), maleic anhydride (MAN, 39.22 g, 0.400 mol) and 193.75 g of methyl ethyl ketone (MEK) were added to a reaction vessel equipped with a stirrer, a cooling tube and a dropping funnel, and stirred / dissolved. Then, the dissolved oxygen in the system was removed by nitrogen bubbling, and the temperature was raised. When the internal temperature reached 80°C, a solution of 2,2'-azobisisobutyric acid dimethyl ester (Wako Pure Chemical Industries, Ltd., trade name: V-601, 3.68 g, 0.016 mol) and PEMP (3.91 g, 0.008 mol) dissolved in MEK 16.42 g was added over 1 hour. After that, it was further reacted at 80°C for 7 hours. Then, the reaction mixture was cooled to room temperature. The obtained polymerization solution was added dropwise to 1228.8 g of methanol to precipitate a white solid. The obtained white solid was further washed with 307.2 g of methanol and then vacuum dried at 120° C. to obtain 64.8 g of a polymer (raw polymer 3) having a structural unit derived from 2-norbornene and a structural unit derived from maleic anhydride.

[0363] The obtained polymer was measured by gel permeation chromatography (GPC). As a result, the weight average molecular weight Mw was 3400 and the polydispersity (weight average molecular weight Mw) / (number average molecular weight Mn) was 1.87.

[0364] The sulfur content in the obtained polymer was confirmed by elemental analysis based on flask combustion and ion chromatography, and the presence of sulfur element in the polymer was confirmed. In addition, in the GPC measurement of the reaction solution before the dropwise addition of methanol, it was also confirmed that the peak derived from PEMP had disappeared, and PEMP was absorbed into the polymer.

[0365] (Synthesis of Base Polymer 4)

[0366] 602.56 g of a 75% toluene solution of 2-norbornene (451.92 g, 4.8 mol in terms of 2-norbornene), maleic anhydride (MAN, 470.69 g, 4.8 mol) and methyl ethyl ketone (MEK) 2281.74 g were added to a reaction vessel equipped with a stirrer, a cooling tube and a dropping funnel, and stirred / dissolved. Next, the dissolved oxygen in the system was removed by nitrogen bubbling, and the temperature was raised. When the internal temperature reached 80°C, a solution of 2,2'-azobisisobutyric acid dimethyl ester (Wako Pure Chemical Industries, Ltd., trade name: V-601, 44.21 g, 0.19 mol) and PEMP (93.82 g, 0.19 mol) dissolved in MEK 193.4 g was added over 1 hour. After that, it was further reacted at 80°C for 7 hours. Next, the reaction mixture was cooled to room temperature. The obtained polymerization solution was added dropwise to 3686.4 g of methanol to precipitate a white solid. The obtained white solid was further washed with 3686.4 g of methanol and then vacuum dried at 120° C. to obtain 910.1 g of a polymer (raw polymer 4) having a structural unit derived from 2-norbornene and a structural unit derived from maleic anhydride.

[0367] The obtained polymer was measured by gel permeation chromatography (GPC). As a result, the weight average molecular weight Mw was 3500 and the polydispersity (weight average molecular weight Mw) / (number average molecular weight Mn) was 1.62.

[0368] [Confirmation of thioether structure contained in base polymer 4]

[0369] The PEMP monomer represented by the following chemical formula 13 In C-NMR measurement, peak a derived from carbon a was confirmed at around 19.0 ppm, and peak b derived from carbon b was confirmed at around 62.0 ppm.

[0370]

[0371] In the case of using PEMP to synthesize the raw polymer 1 13 In C-NMR measurement, peak b derived from carbon b was observed at around 62.0 ppm. In GPC measurement of the reaction solution, no peak of PEMP monomer was observed and no unreacted PEMP remained, which confirmed that PEMP was absorbed into the base polymer 4.

[0372] Furthermore, in the raw polymer 1 13In the C-NMR measurement, peak a derived from carbon a was not confirmed, but peak c corresponding to thioether (RS-R') appeared at around 28 ppm. The integral value of peak c was about twice that of peak b, so the base polymer 4 had a skeleton having a thioether group as described below, and the thiol group had disappeared. It is believed that the polymers of the examples synthesized using the base polymer 4 also have the same skeleton.

[0373]

[0374] 13 The conditions for C-NMR measurement are as follows.

[0375] (Test Conditions) The measurement sample was prepared by adding a measurement solvent to a weighed sample to adjust the concentration, and then injecting a predetermined amount into a sample tube for NMR measurement.

[0376] Measurement device: JNM-ECA400 superconducting FT-NMR device from JEOL Ltd.

[0377] Resonance frequency: 100.53MHz.

[0378] Measurement core: 13 C.

[0379] Measurement method: NNE measurement (Negative Gating Decoupling method).

[0380] Pulse width: 3.83μsec.

[0381] Pulse repetition waiting time: 30s.

[0382] Cumulative number of times: 4096 times.

[0383] Measuring temperature: room temperature.

[0384] Measuring solvent: DMSO-d6 (deuterated dimethyl sulfoxide).

[0385] Sample concentration: 20% (w / v) The sulfur content in the obtained polymer was confirmed by elemental analysis based on flask combustion and ion chromatography, and the presence of sulfur element in the polymer was confirmed. In addition, in the GPC measurement of the reaction solution before the addition of methanol, it was also confirmed that the peak derived from PEMP had disappeared, and PEMP was absorbed into the polymer.

[0386] Elemental analysis was conducted, and as a result, the sulfur content in the base polymer 4 was 2.4 wt %.

[0387] (Synthesis of Base Polymer 5)

[0388] 50.21 g of a 75% toluene solution of 2-norbornene (37.66 g, 0.400 mol in terms of 2-norbornene), maleic anhydride (MAN, 39.22 g, 0.400 mol) and 182.94 g of methyl ethyl ketone (MEK) were added to a reaction vessel equipped with a stirrer, a cooling tube and a dropping funnel, and stirred / dissolved. Next, the dissolved oxygen in the system was removed by nitrogen bubbling, and the temperature was raised. When the internal temperature reached 80°C, a solution of 2,2'-azobisisobutyric acid dimethyl ester (Wako Pure Chemical Industries, Ltd., trade name: V-601, 3.68 g, 0.016 mol) and PEMP (15.64 g, 0.032 mol) dissolved in MEK15.51 g was added over 1 hour. After that, it was further reacted at 80°C for 7 hours. Next, the reaction mixture was cooled to room temperature. The obtained polymerization solution was added dropwise to 1228.8 g of methanol to precipitate a white solid. The obtained white solid was further washed with 307.2 g of methanol and then vacuum dried at 120° C. to obtain 72.8 g of a polymer (raw polymer 5) having a structural unit derived from 2-norbornene and a structural unit derived from maleic anhydride.

[0389] The obtained polymer was measured by gel permeation chromatography (GPC). As a result, the weight average molecular weight Mw was 2000 and the polydispersity (weight average molecular weight Mw) / (number average molecular weight Mn) was 1.58.

[0390] The sulfur content in the obtained polymer was confirmed by elemental analysis based on flask combustion and ion chromatography, and the presence of sulfur element in the polymer was confirmed. In addition, in the GPC measurement of the reaction solution before the dropwise addition of methanol, it was also confirmed that the peak derived from PEMP had disappeared, and PEMP was absorbed into the polymer.

[0391] (Base polymer 6)

[0392] 50.21 g of a 75% toluene solution of 2-norbornene (37.66 g, 0.400 mol in terms of 2-norbornene), maleic anhydride (MAN, 39.22 g, 0.400 mol) and 185.80 g of methyl ethyl ketone (MEK) were added to a reaction container equipped with a stirrer, a cooling tube and a dropping funnel, and stirred and dissolved. Then, the dissolved oxygen in the system was removed by nitrogen bubbling, and the temperature was raised. When the internal temperature reached 80°C, a solution of 2,2'-azobisisobutyric acid dimethyl ester (Wako Pure Chemical Industries, Ltd., trade name: V-601, 3.68 g, 0.016 mol) and DPMP (12.53 g, 0.016 mol) dissolved in MEK15.75 g was added over 1 hour. After that, the mixture was further reacted at 80°C for 7 hours. Then, the reaction mixture was cooled to room temperature. The obtained polymerization solution was added dropwise to 1228.8 g of methanol to precipitate a white solid. The obtained white solid was further washed with 307.2 g of methanol and then vacuum dried at 120° C. to obtain 77.3 g of a polymer (raw polymer 6) having a structural unit derived from 2-norbornene and a structural unit derived from maleic anhydride.

[0393] The obtained polymer was measured by gel permeation chromatography (GPC). As a result, the weight average molecular weight Mw was 3100 and the polydispersity (weight average molecular weight Mw) / (number average molecular weight Mn) was 1.71.

[0394] The sulfur content in the obtained polymer was confirmed by elemental analysis based on flask combustion and ion chromatography, and it was confirmed that sulfur element existed in the polymer. In addition, in the GPC measurement of the reaction solution before the addition of methanol, it was also confirmed that the peak derived from DPMP disappeared, and DPMP was absorbed into the polymer.

[0395] (Base polymer 7)

[0396] 50.21 g of a 75% toluene solution of 2-norbornene (37.66 g, 0.400 mol in terms of 2-norbornene), maleic anhydride (MAN, 39.22 g, 0.400 mol) and 189.60 g of methyl ethyl ketone (MEK) were added to a reaction vessel equipped with a stirrer, a cooling tube and a dropping funnel, and stirred and dissolved. Next, the dissolved oxygen in the system was removed by nitrogen bubbling, and the temperature was raised. When the internal temperature reached 80°C, a solution of 2,2'-azobisisobutyric acid dimethyl ester (Wako Pure Chemical Industries, Ltd., trade name: V-601, 3.68 g, 0.016 mol) and TEMPIC (8.41 g, 0.016 mol) dissolved in MEK 15.75 g was added over 1 hour. After that, the mixture was further reacted at 80°C for 7 hours. Next, the reaction mixture was cooled to room temperature. The obtained polymerization solution was added dropwise to 1228.8 g of methanol to precipitate a white solid. The obtained white solid was further washed with 307.2 g of methanol and then vacuum dried at 120° C. to obtain 71.1 g of a polymer (raw polymer 7) having a structural unit derived from 2-norbornene and a structural unit derived from maleic anhydride.

[0397] The obtained polymer was measured by gel permeation chromatography (GPC). As a result, the weight average molecular weight Mw was 3120 and the polydispersity (weight average molecular weight Mw) / (number average molecular weight Mn) was 1.80.

[0398] The amount of sulfur in the obtained polymer was confirmed by elemental analysis based on flask combustion and ion chromatography, and it was confirmed that sulfur element existed in the polymer. In addition, in the GPC measurement of the reaction solution before the addition of methanol, it was also confirmed that the peak derived from TEMPIC disappeared, indicating that TEMPIC was absorbed into the polymer.

[0399] (Base polymer 8)

[0400] 50.21 g of a 75% toluene solution of 2-norbornene (37.66 g, 0.400 mol in terms of 2-norbornene), maleic anhydride (MAN, 39.22 g, 0.400 mol) and 192.06 g of methyl ethyl ketone (MEK) were added to a reaction vessel equipped with a stirrer, a cooling tube and a dropping funnel, and stirred / dissolved. Next, the dissolved oxygen in the system was removed by nitrogen bubbling, and the temperature was raised. When the internal temperature reached 80°C, a solution of 2,2'-azobisisobutyric acid dimethyl ester (Wako Pure Chemical Industries, Ltd., trade name: V-601, 3.68 g, 0.016 mol) and PEPT (5.74 g, 0.016 mol) dissolved in MEK15.75 g was added over 1 hour. After that, it was further reacted at 80°C for 7 hours. Next, the reaction mixture was cooled to room temperature. The obtained polymerization solution was added dropwise to 1228.8 g of methanol to precipitate a white solid. The obtained white solid was further washed with 307.2 g of methanol and then vacuum dried at 120° C. to obtain 65.2 g of a polymer (raw polymer 8) having a structural unit derived from 2-norbornene and a structural unit derived from maleic anhydride.

[0401] The obtained polymer was measured by gel permeation chromatography (GPC). As a result, the weight average molecular weight Mw was 3536 and the polydispersity (weight average molecular weight Mw) / (number average molecular weight Mn) was 1.64.

[0402] The sulfur content in the obtained polymer was confirmed by elemental analysis based on flask combustion and ion chromatography, and the presence of sulfur element in the polymer was confirmed. In addition, in the GPC measurement of the reaction solution before the dropwise addition of methanol, it was also confirmed that the peak derived from PEPT had disappeared, and PEPT was absorbed into the polymer.

[0403] (Base polymer 9)

[0404] 50.21 g of a 75% toluene solution of 2-norbornene (37.66 g, 0.400 mol in terms of 2-norbornene), maleic anhydride (MAN, 39.22 g, 0.400 mol) and 193.34 g of methyl ethyl ketone (MEK) were added to a reaction container equipped with a stirrer, a cooling tube and a dropping funnel, and stirred and dissolved. Next, the dissolved oxygen in the system was removed by nitrogen bubbling, and the temperature was raised. When the internal temperature reached 80°C, a solution of 2,2'-azobisisobutyric acid dimethyl ester (Wako Pure Chemical Industries, Ltd., trade name: V-601, 3.68 g, 0.016 mol) and KarenzMT (registered trademark) PE1 (4.36 g, 0.008 mol) dissolved in MEK15.75 g was added over 1 hour. After that, the mixture was further reacted at 80°C for 7 hours. Next, the reaction mixture was cooled to room temperature. The polymerization solution obtained above was added dropwise to 1228.8 g of methanol to precipitate a white solid. The obtained white solid was further washed with 307.2 g of methanol and then vacuum dried at a temperature of 120° C., thereby obtaining 65.4 g of a polymer (raw polymer 9) having a structural unit derived from 2-norbornene and a structural unit derived from maleic anhydride.

[0405] The obtained polymer was measured by gel permeation chromatography (GPC). As a result, the weight average molecular weight Mw was 3120 and the polydispersity (weight average molecular weight Mw) / (number average molecular weight Mn) was 1.76.

[0406] The amount of sulfur in the obtained polymer was confirmed by elemental analysis based on flask combustion and ion chromatography, and it was confirmed that sulfur element existed in the polymer. In addition, in the GPC measurement of the reaction solution before the dropwise addition of methanol, it was also confirmed that the peak derived from Karenz MT (registered trademark) PE1 disappeared, and Karenz MT (registered trademark) PE1 was absorbed into the polymer.

[0407] (Base polymer 10)

[0408] 50.21 g of a 75% toluene solution of 2-norbornene (37.66 g, 0.400 mol in terms of 2-norbornene), maleic anhydride (MAN, 39.22 g, 0.400 mol) and 189.32 g of methyl ethyl ketone (MEK) were added to a reaction container equipped with a stirrer, a cooling tube and a dropping funnel, and stirred and dissolved. Next, the dissolved oxygen in the system was removed by nitrogen bubbling, and the temperature was raised. When the internal temperature reached 80°C, a solution of 2,2'-azobisisobutyric acid dimethyl ester (Wako Pure Chemical Industries, Ltd., trade name: V-601, 3.68 g, 0.016 mol) and KarenzMT (registered trademark) PE1 (8.72 g, 0.016 mol) dissolved in MEK 15.75 g was added over 1 hour. After that, the mixture was further reacted at 80°C for 7 hours. Next, the reaction mixture was cooled to room temperature. The polymerization solution obtained above was added dropwise to 1228.8 g of methanol to precipitate a white solid. The obtained white solid was further washed with 307.2 g of methanol and then vacuum dried at a temperature of 120° C., thereby obtaining 64.5 g of a polymer (raw polymer 10) having a structural unit derived from 2-norbornene and a structural unit derived from maleic anhydride.

[0409] The obtained polymer was measured by gel permeation chromatography (GPC). As a result, the weight average molecular weight Mw was 2848 and the polydispersity (weight average molecular weight Mw) / (number average molecular weight Mn) was 1.45.

[0410] The amount of sulfur in the obtained polymer was confirmed by elemental analysis based on flask combustion and ion chromatography, and it was confirmed that sulfur element existed in the polymer. In addition, in the GPC measurement of the reaction solution before the dropwise addition of methanol, it was also confirmed that the peak derived from Karenz MT (registered trademark) PE1 disappeared, and Karenz MT (registered trademark) PE1 was absorbed into the polymer.

[0411] (Base polymer 11)

[0412] 50.21 g of a 75% toluene solution of 2-norbornene (37.66 g, 0.400 mol in terms of 2-norbornene), maleic anhydride (MAN, 39.22 g, 0.400 mol) and 181.28 g of methyl ethyl ketone (MEK) were added to a reaction container equipped with a stirrer, a cooling tube and a dropping funnel, and stirred and dissolved. Next, the dissolved oxygen in the system was removed by nitrogen bubbling, and the temperature was raised. When the internal temperature reached 80°C, a solution of 2,2'-azobisisobutyric acid dimethyl ester (Wako Pure Chemical Industries, Ltd., trade name: V-601, 3.68 g, 0.016 mol) and KarenzMT (registered trademark) PE1 (17.43 g, 0.032 mol) dissolved in MEK 15.75 g was added over 1 hour. After that, the mixture was further reacted at 80°C for 7 hours. Next, the reaction mixture was cooled to room temperature. The polymerization solution obtained above was added dropwise to 1228.8 g of methanol to precipitate a white solid. The obtained white solid was further washed with 307.2 g of methanol and then vacuum dried at a temperature of 120° C., thereby obtaining 67.3 g of a polymer (raw polymer 11) having a structural unit derived from 2-norbornene and a structural unit derived from maleic anhydride.

[0413] The obtained polymer was measured by gel permeation chromatography (GPC). As a result, the weight average molecular weight Mw was 2005 and the polydispersity (weight average molecular weight Mw) / (number average molecular weight Mn) was 1.45.

[0414] The amount of sulfur in the obtained polymer was confirmed by elemental analysis based on flask combustion and ion chromatography, and it was confirmed that sulfur element existed in the polymer. In addition, in the GPC measurement of the reaction solution before the dropwise addition of methanol, it was also confirmed that the peak derived from Karenz MT (registered trademark) PE1 disappeared, and Karenz MT (registered trademark) PE1 was absorbed into the polymer.

[0415] (Base polymer 12)

[0416] In a reaction vessel equipped with a stirrer, a cooling tube, and a dropping funnel, 50.21 g of a 75% toluene solution of 2-norbornene (37.66 g, 0.400 mol in terms of 2-norbornene), maleic anhydride (MAN, 39.22 g, 0.400 mol), and 202.18 g of methyl ethyl ketone (MEK) were added and stirred and dissolved. Then, the dissolved oxygen in the system was removed by nitrogen bubbling, and the temperature was raised. When the internal temperature reached 80°C, a solution prepared by dissolving dimethyl 2,2'-azobisisobutyrate (Wako Pure Chemical Industries, Ltd., trade name: V-601, 3.68 g, 0.016 mol) and EGMP-4 (11.90 g, 0.032 mol) in 16.23 g of MEK was added over 1 hour. After that, the mixture was further reacted at 80°C for 7 hours. Next, the reaction mixture was cooled to room temperature. The polymerization solution obtained above was added dropwise to 1228.8 g of methanol to precipitate a white solid. The obtained white solid was further washed with 307.2 g of methanol and then vacuum dried at a temperature of 120° C., thereby obtaining 64.5 g of a polymer (raw polymer 12) having a structural unit derived from 2-norbornene and a structural unit derived from maleic anhydride.

[0417] The obtained polymer was measured by gel permeation chromatography (GPC). As a result, the weight average molecular weight Mw was 2926 and the polydispersity (weight average molecular weight Mw) / (number average molecular weight Mn) was 2.57.

[0418] The sulfur content in the obtained polymer was confirmed by elemental analysis based on flask combustion and ion chromatography, and the presence of sulfur in the polymer was confirmed. In addition, in the GPC measurement of the reaction solution before the addition of methanol, it was also confirmed that the peak derived from EGMP-4 had disappeared, and EGMP-4 was absorbed into the polymer.

[0419] <Preparation of resin composition>

[0420] (Mixture Example 1)

[0421] A resin mixture containing a polymer P1 obtained by ring-opening the MA unit of the base polymer 1 with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound, and water was prepared. The details are described below.

[0422] First, 99.71 g of MEK was added to 60.00 g of the base polymer 1 (0.312 mol in terms of MA) to prepare a dissolving solution. Next, 38.75 g of A-TMM-3LM-N was added to the dissolving solution, and then 18.00 g of triethylamine (0.178 mol) was added, and the mixture was reacted at a temperature of 70° C. for 2 hours. Then, 56.27 g of 4-HBA (0.390 mol) was further added, and the mixture was reacted at a temperature of 70° C. for 4 hours to prepare a reaction solution.

[0423] Next, 3.00 g (0.167 mol) of water was added to the obtained reaction solution without post-treatment, and the reaction was carried out at 70° C. for 2 hours. The obtained reaction solution was diluted with MEK and treated with an aqueous formic acid solution and an aqueous citric acid solution to remove the aqueous phase from the reaction solution. Furthermore, liquid-liquid extraction was carried out by the following steps, followed by solvent replacement.

[0424] Liquid-liquid extraction: The reaction solution was diluted with MEK, and then water was added to remove the aqueous phase from the reaction solution. The same operation was then performed once more.

[0425] Solvent replacement: The obtained reaction mixture was subjected to solvent removal at 50°C under reduced pressure using a rotary evaporator. The solid content concentration of the polymer solution was confirmed to be 27±2% by mass in the measurement based on a heated drying moisture meter, and the operation of removing the solvent was interrupted. Thereafter, PGMEA was added to make the solid content concentration 18% by mass and mixed until uniform. By the same operation, the solvent was removed under reduced pressure at 50°C, and after the solid content concentration was adjusted to 27±2% by mass in the measurement based on a heated drying moisture meter, the operation of further adding PGMEA to make the solid content concentration 18% by mass and mixing until uniform was repeated 2 times. Thereafter, the operation of removing the solvent or adding PGMEA to make the solid content concentration 30±3% by mass and stirring until uniform was performed. Through the above operation, the solvent used in the reaction is removed and the solvent is replaced with PGMEA.

[0426] Through the above, a resin mixture (resin composition) 1 containing a polymer P1 in which the structural units derived from maleic anhydride in the base polymer were ring-opened with A-TMM-3LM-N, 4-HBA and water, and residual (free) A-TMM-3LM-N and residual (free) 4-HBA was obtained.

[0427] The obtained resin composition 1 was analyzed by gel permeation chromatography to measure the amount of polymer P1, free polyfunctional (meth)acrylic compound and free monofunctional (meth)acrylic compound contained in the composition, and the weight average molecular weight and polydispersity of polymer P1. The results are shown in Table 1. In addition, the amount of free (meth)acrylic compound is expressed as the ratio (%) of the peak area of ​​free (meth)acrylic compound to the peak area of ​​polymer P in the gel permeation chromatography (GPC) chart of the resin mixture.

[0428] In addition, the measurement conditions of gel permeation chromatography are as follows.

[0429] As a GPC measurement apparatus, HLC-8320GPC EcoSEC manufactured by TOSOH CORPORATION was used. The column temperature was set to 40.0°C, and the pump flow rate was set to 0.350 mL / min.

[0430] Peak position (holding time)

[0431] -Polymer P: a peak detected before 20 minutes (a peak with a shorter retention time and a larger molecular weight than A-TMM-3LM-N and 4-HBA).

[0432] -A-TMM-3LM-N: The sum of two peaks at 20.0 to 20.6 minutes and 20.6 to 21.5 minutes.

[0433] -4-HBA: 21.7~22.4 minutes.

[0434] · Measurement conditions: The analysis was performed using a differential refractive index detector (RI detector).

[0435] (Mixture Example 2)

[0436] Resin composition 2 containing polymer P2 obtained by ring-opening MA units of base polymer 2 with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water was prepared in the same manner as in Preparation Example 1 except that base polymer 2 was used instead of base polymer 1.

[0437] The obtained resin composition 2 was subjected to GPC measurement to measure the weight average molecular weight and polydispersity of the polymer P2.

[0438] Furthermore, the amount of the free (meth)acrylic acid compound contained in the obtained resin composition 2 was measured by gel permeation chromatography.

[0439] (Mixture Example 3)

[0440] Resin composition 3 containing polymer P3 obtained by ring-opening the MA unit of base polymer 2 with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water was prepared in the same manner as in Preparation Example 1 except that base polymer 3 was used instead of base polymer 1.

[0441] The obtained resin composition 3 was subjected to GPC measurement to measure the weight average molecular weight and polydispersity of the polymer P3.

[0442] Furthermore, the amount of the free (meth)acrylic acid compound contained in the obtained resin composition 3 was measured by gel permeation chromatography.

[0443] (Mixture Example 4)

[0444] Resin composition 4 containing polymer P4 obtained by ring-opening MA units of base polymer 2 with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water was prepared in the same manner as in Preparation Example 1 except that base polymer 4 was used instead of base polymer 1.

[0445] The obtained resin composition 4 was subjected to GPC measurement to measure the weight average molecular weight and polydispersity of the polymer P4.

[0446] Furthermore, the amount of the free (meth)acrylic acid compound contained in the obtained resin composition 4 was measured by gel permeation chromatography.

[0447] (Preparation Example 5)

[0448] Resin composition 5 containing polymer P5 obtained by ring-opening MA units of base polymer 2 with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water was prepared in the same manner as in Preparation Example 1 except that base polymer 5 was used instead of base polymer 1.

[0449] The obtained resin composition 5 was subjected to GPC measurement to measure the weight average molecular weight and polydispersity of the polymer P5.

[0450] Furthermore, the amount of the free (meth)acrylic acid compound contained in the obtained resin composition 5 was measured by gel permeation chromatography.

[0451] (Preparation Example 6)

[0452] Resin composition 6 containing polymer P6 obtained by ring-opening the MA unit of base polymer 2 with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water was prepared in the same manner as in Preparation Example 1 except that base polymer 6 was used instead of base polymer 1.

[0453] The obtained resin composition 6 was subjected to GPC measurement to measure the weight average molecular weight and polydispersity of the polymer P6.

[0454] Furthermore, the amount of free (meth)acrylic acid compound contained in the obtained resin composition 6 was measured by gel permeation chromatography.

[0455] (Preparation Example 7)

[0456] A polymer P7 was prepared in which the MA unit of the base polymer 1 was ring-opened with a monofunctional (meth)acrylic acid compound. The details are described below.

[0457] First, 18.44 g of MEK was added to 10.00 g (0.052 mol in terms of MA) of base polymer 1 to prepare a dissolving solution, and then 9.38 g (0.065 mol) of 4-HBA was added to the dissolving solution, followed by 3.00 g (0.030 mol) of triethylamine, and the mixture was reacted at 70° C. for 6 hours to prepare a reaction solution.

[0458] The obtained reaction solution was diluted with MEK and treated with an aqueous citric acid solution, thereby removing the aqueous phase from the reaction solution. Thereafter, the polymer was purified by the following steps.

[0459] The polymer was reprecipitated with excess water. The polymer powder obtained by reprecipitation was washed with excess water twice. The obtained reaction product was dried at 40° C. for 12 hours.

[0460] As described above, 9.5 g of a polymer P7 in which the structural unit derived from maleic anhydride in the base polymer was ring-opened with 4-HBA was obtained.

[0461] The obtained polymer P7 was subjected to GPC measurement to measure the weight average molecular weight and polydispersity of the polymer P7. The results are shown in Table 1.

[0462] Furthermore, the disappearance of the peak of the monofunctional (meth)acrylic compound used was confirmed by GPC measurement of the polymer P7. Therefore, it was confirmed that the obtained polymer P7 did not contain an unreacted monofunctional (meth)acrylic compound.

[0463] (Mixture Example 8)

[0464] A polymer P8 was prepared in which the MA unit of the base polymer 4 was ring-opened with a monofunctional (meth)acrylic acid compound. The details are described below.

[0465] First, 18.44 g of MEK was added to 10.00 g (0.052 mol in terms of MA) of base polymer 4 to prepare a dissolving solution, and then 9.38 g (0.065 mol) of 4-HBA was added to the dissolving solution, followed by 3.00 g (0.030 mol) of triethylamine, and the mixture was reacted at 70° C. for 6 hours to prepare a reaction solution.

[0466] The obtained reaction solution was diluted with MEK and treated with an aqueous citric acid solution, thereby removing the aqueous phase from the reaction solution. Thereafter, the polymer was purified by the following steps.

[0467] The polymer was reprecipitated with excess water. The polymer powder obtained by reprecipitation was washed with excess water twice. The obtained reaction product was dried at 40° C. for 12 hours.

[0468] As described above, 8.7 g of a polymer P8 in which the structural unit derived from maleic anhydride in the base polymer was ring-opened with 4-HBA was obtained.

[0469] The obtained polymer P8 was subjected to GPC measurement to measure the weight average molecular weight and polydispersity of the polymer P8. The results are shown in Table 1.

[0470] Furthermore, the disappearance of the peak of the monofunctional (meth)acrylic compound used was confirmed by GPC measurement of the polymer P8. Therefore, it was confirmed that the obtained polymer P8 did not contain an unreacted monofunctional (meth)acrylic compound.

[0471] (Mixture Example 9)

[0472] A resin mixture containing a polymer P9 in which the MA unit of the base polymer 4 was ring-opened with a monofunctional (meth)acrylic compound was prepared. The details are described below.

[0473] First, 18.44 g of MEK was added to 10.00 g (0.052 mol in terms of MA) of base polymer 1 to prepare a dissolving solution, and then 9.38 g (0.065 mol) of 4-HBA was added to the dissolving solution, followed by 3.00 g (0.030 mol) of triethylamine, and the mixture was reacted at 70° C. for 6 hours to prepare a reaction solution.

[0474] The obtained reaction solution was diluted with MEK and treated with an aqueous formic acid solution and an aqueous citric acid solution to remove the aqueous phase from the reaction solution. Furthermore, liquid-liquid extraction was performed in the same manner as in Preparation Example 1, followed by solvent replacement to obtain a resin composition 9.

[0475] The obtained resin composition 9 was subjected to GPC measurement to measure the amount of polymer P9 and free monofunctional (meth)acrylic compound contained in the composition, and the weight average molecular weight and polydispersity of polymer P9.

[0476] (Preparation Example 10)

[0477] A resin composition 10 containing a polymer P10 obtained by ring-opening the MA unit of the base polymer 2 with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water was prepared in the same manner as in Preparation Example 1 except that the base polymer 7 was used instead of the base polymer 1.

[0478] The obtained resin composition 10 was subjected to GPC measurement to measure the weight average molecular weight and polydispersity of the polymer P10.

[0479] Furthermore, the amount of the free (meth)acrylic acid compound contained in the obtained resin composition 10 was measured by gel permeation chromatography.

[0480] (Preparation Example 11)

[0481] A resin composition 11 containing a polymer P11 obtained by ring-opening the MA unit of the base polymer 2 with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water was prepared in the same manner as in Preparation Example 1 except that the base polymer 8 was used instead of the base polymer 1.

[0482] The obtained resin composition 11 was subjected to GPC measurement to measure the weight average molecular weight and polydispersity of the polymer P11.

[0483] Furthermore, the amount of the free (meth)acrylic acid compound contained in the obtained resin composition 11 was measured by gel permeation chromatography.

[0484] (Mixture Example 12)

[0485] A resin composition 12 containing a polymer P12 obtained by ring-opening the MA unit of the base polymer 2 with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water was prepared in the same manner as in Preparation Example 1 except that the base polymer 9 was used instead of the base polymer 1.

[0486] The obtained resin composition 12 was subjected to GPC measurement to measure the weight average molecular weight and polydispersity of the polymer P12.

[0487] Furthermore, the amount of free (meth)acrylic acid compound contained in the obtained resin composition 12 was measured by gel permeation chromatography. The results are shown in Table 1.

[0488] (Preparation Example 13)

[0489] Resin composition 13 containing polymer P13 obtained by ring-opening the MA unit of base polymer 2 with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water was prepared in the same manner as in Preparation Example 1 except that base polymer 10 was used instead of base polymer 1.

[0490] The obtained resin composition 13 was subjected to GPC measurement to measure the weight average molecular weight and polydispersity of the polymer P13.

[0491] Furthermore, the amount of the free (meth)acrylic acid compound contained in the obtained resin composition 13 was measured by gel permeation chromatography. The results are shown in Table 1.

[0492] (Preparation Example 14)

[0493] A resin composition 14 containing a polymer P14 obtained by ring-opening the MA unit of the base polymer 2 with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water was prepared in the same manner as in Preparation Example 1 except that the base polymer 11 was used instead of the base polymer 1.

[0494] The obtained resin composition 14 was subjected to GPC measurement to measure the weight average molecular weight and polydispersity of the polymer P14.

[0495] Furthermore, the amount of free (meth)acrylic acid compound contained in the obtained resin composition 14 was measured by gel permeation chromatography. The results are shown in Table 1.

[0496] (Preparation Example 15)

[0497] A resin composition 15 containing a polymer P15 obtained by ring-opening the MA unit of the base polymer 4 with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water was prepared. The details are described below.

[0498] First, 100.30 g of MEK was added to 60.00 g of the base polymer 4 (0.312 mol in terms of MA) to prepare a dissolving solution. Next, 58.12 g of A-TMM-3LM-N was added to the dissolving solution, and then 18.00 g of triethylamine (0.178 mol) was added, and the mixture was reacted at a temperature of 70° C. for 2 hours. Then, 56.27 g of 4-HBA (0.390 mol) was further added, and the mixture was reacted at a temperature of 70° C. for 4 hours to prepare a reaction solution.

[0499] Next, without performing post-treatment on the obtained reaction solution, 3.00 g (0.167 mol) of water was added to the reaction solution, and the mixture was reacted at 70° C. for 2 hours.

[0500] The obtained reaction solution was diluted with MEK and treated with an aqueous formic acid solution and an aqueous citric acid solution, thereby removing the aqueous phase from the reaction solution. Further, liquid-liquid extraction was performed by the same steps as in Preparation Example 1, followed by solvent replacement to obtain a resin composition 15. The obtained resin composition 15 was subjected to GPC measurement to measure the amount of polymer P15, free multifunctional (meth) acrylic acid compound and free monofunctional (meth) acrylic acid compound contained in the composition, and the weight average molecular weight and polydispersity of polymer P15. The results are shown in Table 1.

[0501] (Preparation Examples 16 to 29)

[0502] Resin compositions 16 to 29 were prepared by mixing the additives described in Table 1 in the amounts shown in "Additive Amounts" of Table 1 with resin composition 15. The amounts of the additives were mixed in terms of weight % relative to the solid content (polymer P15, polyfunctional (meth)acrylic compound) in resin composition 15.

[0503] In addition, the details of the "additives" shown in Table 1 are as follows.

[0504] -PEMP: pentaerythritol tetrakis(3-mercaptopropionate), a thiol group-containing compound of the above formula (s-2) (manufactured by SC Organic Chemical Co., Ltd.).

[0505] -TMMP: trimethylolpropane tris(3-mercaptopropionate), a thiol group-containing compound of the above formula (s-1) (manufactured by SC Organic Chemical Co., Ltd.).

[0506] -Karenz MT (registered trademark) PE1: pentaerythritol tetrakis(3-mercaptobutyrate), a thiol group-containing compound of the above formula (s-9) (manufactured by SHOWA DENKO KK).

[0507] -Karenz MT (registered trademark) TPMB: trimethylolpropane tris(3-mercaptobutyrate), a thiol group-containing compound of the above formula (s-8) (manufactured by SHOWA DENKO KK).

[0508] -LIGHT ESTER P-1M: 2-methacryloyloxyethyl acid phosphate, manufactured by Kyoeisha Chemical Co., Ltd.

[0509] -KBM-3066: 1,6-bis(trimethoxysilyl)hexane, manufactured by Shin-Etsu Chemical Co., Ltd.

[0510] -KBM-5103: 3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.

[0511] (Mixture Example 30)

[0512] A resin composition 30 containing a polymer P16 in which the MA unit of the base polymer 4 was ring-opened with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water was prepared. The details are described below.

[0513] First, 100.30 g of MEK was added to 60.00 g of the base polymer 12 (0.312 mol in terms of MA) to prepare a dissolving solution. Next, 58.12 g of A-TMM-3LM-N was added to the dissolving solution, and then 18.00 g of triethylamine (0.178 mol) was added, and the mixture was reacted at a temperature of 70° C. for 2 hours. Then, 56.27 g of 4-HBA (0.390 mol) was further added, and the mixture was reacted at a temperature of 70° C. for 4 hours to prepare a reaction solution.

[0514] Next, without performing post-treatment on the obtained reaction solution, 3.00 g (0.167 mol) of water was added to the reaction solution, and the mixture was reacted at 70° C. for 2 hours.

[0515] The obtained reaction solution was diluted with MEK and treated with an aqueous formic acid solution and an aqueous citric acid solution, thereby removing the aqueous phase from the reaction solution. Further, liquid-liquid extraction was performed by the same steps as in Formulation Example 1, followed by solvent replacement to obtain a resin composition 30. The obtained resin composition 30 was subjected to GPC measurement to measure the amount of polymer P16, free multifunctional (meth) acrylic acid compound and free monofunctional (meth) acrylic acid compound contained in the composition, and the weight average molecular weight and polydispersity of polymer P16. The results are shown in Table 1.

[0516] (Mixture Example 31)

[0517] A resin composition 31 containing a polymer P17 in which the MA unit of the base polymer 2 was ring-opened with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water was prepared. The details are described below.

[0518] First, 99.93 g of MEK was added to 60.00 g of the base polymer 4 (0.312 mol in terms of MA) to prepare a dissolving solution. Next, 77.49 g of A-TMM-3LM-N was added to the dissolving solution, and then 18.00 g of triethylamine (0.178 mol) was added, and the mixture was reacted at a temperature of 70° C. for 2 hours. Then, 56.27 g of 4-HBA (0.390 mol) was further added, and the mixture was reacted at a temperature of 70° C. for 4 hours to prepare a reaction solution.

[0519] Next, without performing post-treatment on the obtained reaction solution, 3.00 g (0.167 mol) of water was added to the reaction solution, and the mixture was reacted at 70° C. for 2 hours.

[0520] The obtained reaction solution was diluted with MEK and treated with an aqueous formic acid solution and an aqueous citric acid solution to remove the aqueous phase from the reaction solution. Furthermore, liquid-liquid extraction was performed by the same steps as in Preparation Example 1, followed by solvent replacement. Thereafter, purification was further performed by the following steps.

[0521] • The polymer was reprecipitated with excess toluene.

[0522] The operation of washing the polymer powder obtained by reprecipitation with an excess amount of toluene was repeated twice.

[0523] The polymer powder after the above washing twice was washed with an excess amount of water three times.

[0524] The obtained reaction product was dried at 40°C for 12 hours.

[0525] As described above, a polymer P17 was prepared in which the MA unit of the base polymer 2 was ring-opened with a trifunctional (meth)acrylic compound, a monofunctional (meth)acrylic compound and water.

[0526] The obtained polymer P17 was subjected to GPC measurement to measure the weight average molecular weight and polydispersity of the polymer P17. The results are shown in Table 1.

[0527] Furthermore, the disappearance of the peaks of the polyfunctional (meth)acrylic compound and the monofunctional (meth)acrylic compound used was confirmed by GPC measurement of the polymer P17. Thus, it was confirmed that the obtained polymer P17 did not contain unreacted polyfunctional (meth)acrylic compound and monofunctional (meth)acrylic compound.

[0528] The following Table 1 shows the components used in each synthesis example and their charged amounts (in terms of maleic anhydride (MA)).

[0529]

[0530] (Examples 1 to 13, 28 to 29, Comparative Examples 1 to 3)

[0531] In each of the Examples and Comparative Examples, a resin composition was prepared and evaluated on the following items.

[0532] <Evaluation>

[0533] [Alkali dissolution rate of resin composition]

[0534] The polymers P7, P8, and P17 obtained in Preparation Examples 7, 8, and 31 were dissolved in propylene glycol monomethyl ether acetate (PGMEA) to prepare solutions having a solid content concentration of 30% by mass.

[0535] Next, the above solution or the resin compositions 1 to 6, 9 to 15, 30 obtained in formulation examples 1 to 6, 9 to 15, 30 were spin-coated on the wafer, PGMEA was dried, and then pre-baked at 100° C. for 2 minutes to prepare a resin film with a film thickness of about 2 μm.

[0536] The resin film together with the wafer was immersed in a 2% sodium carbonate aqueous solution at a temperature of 23° C., and the dissolution rate of the resin film was measured.

[0537] The dissolution rate was calculated by visually observing the immersed wafer, measuring the time until the resin film was dissolved and the interference pattern was no longer visible, and dividing the film thickness by the time. The results are shown in Table 1. If the alkali dissolution rate is 140nm / s or more, it can be used as a photosensitive material without any problem. In particular, if it is 350nm / s or more, it can be considered particularly good.

[0538] [Evaluation of Sensitivity of Photosensitive Resin Composition 1 (Exposure Amount at Which Residual Film Ratio Becomes 90% or More)]

[0539] First, the following components were dissolved in propylene glycol monomethyl ether acetate (PGMEA) so that the total solid content concentration would be 30% by mass, thereby obtaining a photosensitive resin composition.

[0540] Polymer P7, P8, P17 (polymer P7, P8, P17 of formulation examples 7, 8, 31) or resin compositions 1 to 6, 9 to 15, 30: 100 parts by mass.

[0541] (Here, resin compositions 1 to 6, 9 to 15, and 30 were weighed so that the total amount of the solid content (polymers P1 to P6, P9 to 15, and P16) and the polyfunctional (meth)acrylic compound was 100 parts by mass.)

[0542] · Multifunctional acrylate (dipentaerythritol hexaacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd., A-DPH): 50 parts by mass.

[0543] Photopolymerization initiator (Ingacure OXE01 manufactured by BASF): 5 parts by mass.

[0544] Adhesion aid (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.): 1 part by mass.

[0545] Surfactant (DIC Corporation, F-556): 0.5 parts by mass.

[0546] The obtained photosensitive resin composition was spin-coated on a 3-inch silicon wafer treated with HMDS (hexamethyldisilazane) and baked on a hot plate at 100° C. for 120 seconds to obtain a thin film A with a thickness of about 3.0 μm (±0.3 μm).

[0547] The film A was irradiated at 100 mJ / cm2 using a g+h+i ray mask aligner (PLA-501F) manufactured by Canon Inc. through a mask having a gradation of 1 to 100% of light shielding rate. 2 The exposure amount of g+h+i rays was used.

[0548] After exposure, the film was developed in a 2.0 mass % sodium carbonate aqueous solution at 23° C. for 60 seconds (along with wafer immersion), thereby obtaining a 1 to 100 mJ / cm 2 Film B was exposed and developed at various exposure amounts.

[0549] The residual film ratio was calculated from the film thicknesses of the thin film A and the thin film B obtained by the above method using the following formula.

[0550] Remaining film rate (%) = (film thickness of film B at each exposure dose / film thickness of film Af) × 100

[0551] Then, the exposure dose at which the residual film rate becomes 90% or more is taken as the sensitivity of each photosensitive resin composition. The results are shown in Table 1. The exposure dose at which the residual film rate becomes 90% or more is 50 mJ / cm 2 Below 30 mJ / cm, it can be used as a photosensitive composition without any problem. 2 The following can be considered to be particularly good.

[0552] [Evaluation of sensitivity of resin composition 2 (residual film ratio after exposure at low exposure dose)]

[0553] (5mJ / cm 2 Residual film rate of exposure dose)

[0554] The photosensitive resin composition prepared in the above sensitivity evaluation 1 was spin-coated on a 3-inch silicon wafer treated with HMDS (hexamethyldisilazane) and baked on a hot plate at 100° C. for 120 seconds to obtain a film A with a thickness of 3.0 μm (±0.3 μm).

[0555] The film was irradiated at 5 mJ / cm2 using a g+h+i ray mask aligner (PLA-501F) manufactured by Canon Inc. through a mask having a grayscale of 1 to 100% light shielding rate. 2 The exposure amount of g+h+i rays was used.

[0556] After the exposure, the film was developed in a 2.0 mass % sodium carbonate aqueous solution at 23° C. for 60 seconds (along with the wafer immersion), whereby a film B was obtained.

[0557] The residual film ratio was calculated from the film thicknesses of the thin film A and the thin film B obtained by the above method using the following formula.

[0558] Residual film rate (%) = (thickness of film B at each exposure amount / thickness of film A) × 100

[0559] (10mJ / cm 2 Residual film rate of exposure dose)

[0560] The photosensitive resin composition prepared in the above sensitivity evaluation 1 was spin-coated on a 3-inch silicon wafer treated with HMDS (hexamethyldisilazane) and baked on a hot plate at 100° C. for 120 seconds to obtain a film A with a thickness of 3.0 μm (±0.3 μm).

[0561] The film A was irradiated at 10 mJ / cm2 using a g+h+i ray mask aligner (PLA-501F) manufactured by Canon Inc. through a mask having a grayscale of 1 to 100% light shielding. 2 The exposure amount of g+h+i rays was used.

[0562] After the exposure, the film was developed in a 2.0 mass % sodium carbonate aqueous solution at 23° C. for 60 seconds (along with the wafer immersion), whereby a film B was obtained.

[0563] The residual film ratio was calculated from the film thicknesses of the thin film A and the thin film B obtained by the above method using the following formula.

[0564] Residual film rate (%) = (thickness of film B at each exposure amount / thickness of film A) × 100

[0565] [Alkali dissolution rate of photosensitive resin composition (2.0 mass % sodium carbonate aqueous solution)]

[0566] The photosensitive resin composition prepared in the above-mentioned sensitivity evaluation 1 was spin-coated on a wafer, and PGMEA was dried and then pre-baked at a temperature of 100° C. for 2 minutes to prepare a resin film having a film thickness of about 2 μm.

[0567] The resin film together with the wafer was immersed in a 2% sodium carbonate aqueous solution at a temperature of 23° C., and the dissolution rate of the resin film was measured.

[0568] The dissolution rate was calculated by visually observing the immersed wafer, measuring the time until the resin film was dissolved and the interference pattern was no longer visible, and dividing the film thickness by the time. The results are shown in Table 1. If the alkali dissolution rate is 250 nm / s or more, it can be used as a photosensitive material without any problem, and if it is 400 nm / s or more, it can be considered that the developability is good.

[0569] [Yellow Index]

[0570] The photosensitive resin composition prepared in the above sensitivity evaluation 1 was spin-coated on EAGLE XG glass (manufactured by Corning Incorporated Co., Ltd., thickness 0.5 mm) and baked on a hot plate at 100° C. for 120 seconds to obtain a thin film with a thickness of about 3.0 μm (±0.1 μm).

[0571] Next, the film was irradiated with a g+h+i ray mask aligner (PLA-600F) manufactured by Canon Inc. at 100 mJ / cm 2 The exposure amount of g+h+i rays was used.

[0572] After exposure, the film was developed in a 2.0 mass % sodium carbonate aqueous solution at 23° C. for 60 seconds (along with wafer immersion), thereby obtaining a 100 mJ / cm 2 The film was exposed and developed with an exposure amount of .

[0573] The film was heated at 230° C. in air for 30 minutes. After cooling the film at room temperature in air, the film was heated again at 230° C. in air for 30 minutes. The same operation was repeated for a total of 3 times for heating in air for 30 minutes.

[0574] The yellowness index (YI) of the film obtained by the above method was measured 3 times by changing the measurement position using a colorimeter CR-5 (manufactured by Konica Minolta, Inc.), and the average value was taken as the value of YI. The measurement type was transmission measurement, and 100% calibration used uncoated EAGLE XG glass (manufactured by Corning Incorporated Co., Ltd., thickness 0.5 mm). The results are shown in Table 1. If the yellowness index is 1.20 or less, it can be considered that the heat discoloration resistance is good, if it is 1.10 or less, it can be considered to be better, and if it is 0.90 or less, it can be considered to be particularly good.

[0575] (Examples 14 to 27)

[0576] First, the following components were dissolved in propylene glycol monomethyl ether acetate (PGMEA) so that the total solid content concentration would be 30% by mass, thereby obtaining a photosensitive resin composition.

[0577] Resin compositions 16 to 29: 100 parts by mass.

[0578] (Weighing was performed so that the total amount of the solid content (polymer P15, polyfunctional (meth)acrylic compound, additives described in Table 1) became 100 parts by mass.)

[0579] · Multifunctional acrylate (dipentaerythritol hexaacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd., A-DPH): 50 parts by mass.

[0580] Photopolymerization initiator (Ingacure OXE01 manufactured by BASF): 5 parts by mass.

[0581] Adhesion aid (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.): 1 part by mass.

[0582] Surfactant (DIC Corporation, F-556): 0.5 parts by mass.

[0583] The obtained photosensitive resin composition was measured and evaluated in the same manner as above with respect to the “Sensitivity evaluation 1 of the photosensitive resin composition (exposure amount at which the residual film rate becomes 90% or more)”, “Sensitivity evaluation 2 of the resin composition (residual film rate after exposure at a low exposure amount)”, “Alkali dissolution rate of the photosensitive resin composition (2.0 mass % sodium carbonate aqueous solution)” and “Yellowness index”.

[0584] Table 2 shows the results of the developability evaluation and the sensitivity evaluation.

[0585] [Table 2]

[0586]

[0587] The photosensitive resin composition of the example has a good alkali dissolution rate and thus has excellent developability. The exposure dose at which the residual film rate of the photosensitive resin composition of the example becomes 90% or more is 50 mJ / cm 2 In other words, curing at low exposure can be said to have high sensitivity. Therefore, the photosensitive resin composition of the embodiment has a good balance of high developability, high sensitivity, and low yellow index. In addition, according to the comparison of Examples 14 to 21 in which a thiol-containing compound is used as an additive and Examples 22 to 27 (for reference) in which a compound other than a thiol-containing compound is used as an additive, it can be seen that by adding a thiol-containing compound to the photosensitive resin composition, yellowing is further suppressed, heat discoloration resistance is further improved, and the exposure amount at which the residual film rate becomes more than 90% is smaller, so the sensitivity is further improved.

[0588] <Color filter production>

[0589] A colored photosensitive resin composition was prepared by further adding an appropriate amount of pigment dispersion NX-061 (manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd., green) to the photosensitive resin composition prepared in Examples 1 to 21.

[0590] This is formed into a film on a substrate, and subjected to exposure, alkali development treatment, etc., to form a green color filter.

[0591] Furthermore, by using NX-053 (blue) or NX-032 (red) or the like manufactured by the same company instead of NX-061 as the pigment dispersion, a blue or red color filter can be formed.

[0592] <Making Black Matrix>

[0593] A black photosensitive resin composition was prepared by further adding an appropriate amount of carbon black dispersion NX-595 (manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd.) to the photosensitive resin composition prepared in Examples 1 to 21.

[0594] This is formed into a film on a substrate, and subjected to exposure, alkali development treatment, etc., to form a black matrix.

[0595] This application claims the benefit of priority based on Japanese patent application No. 2019-189164 filed on October 16, 2019 and Japanese patent application No. 2020-135597 filed on August 11, 2020, and all the disclosed contents of these applications are incorporated herein.

Claims

1. A polymer, It is characterized in that The polymer is obtained by reacting a polymer precursor with a compound having a hydroxyl group and two or more (meth)acryloyl groups and / or a compound having a hydroxyl group and one (meth)acryloyl group in the presence of a basic catalyst, and the polymer precursor is obtained by polymerizing a monomer composition containing a monomer represented by the following general formula (NBm) and maleic anhydride in the presence of a bifunctional or more thiol group-containing compound, In the general formula (NBm), R 1 , R 2 , R 3 and R 4 are independently a hydrogen atom or an organic group having 1 to 30 carbon atoms, a 1 Is 0, 1, or 2.

2. The polymer according to claim 1, It is characterized in that The monomer composition contains at least one selected from substituted or unsubstituted indene, maleimide, styrene and norbornadiene.

3. The polymer according to claim 1, It is characterized in that The polymer is obtained by further treating the polymer precursor with water in the presence of a basic catalyst to ring-open the structural unit derived from maleic anhydride contained in the polymer precursor.

4. The polymer according to claim 1, It is characterized in that The bifunctional or higher thiol group-containing compound contains at least one compound selected from the following chemical formulas (s-1) to (s-20), 5. The polymer according to claim 1, It is characterized in that The weight average molecular weight is 1,000 or more and 15,000 or less.

6. A resin composition, It is characterized in that The resin composition contains the polymer according to any one of claims 1 to 5.

7. The resin composition according to claim 6, It is characterized in that The resin composition further contains a compound having two or more (meth)acryloyl groups.

8. The resin composition according to claim 6, It is characterized in that The resin composition further contains a compound having one (meth)acryloyl group.

9. The resin composition according to claim 6, It is characterized in that The resin composition further contains a compound having a thiol group.

10. The resin composition according to claim 9, It is characterized in that The compound having a thiol group is a compound having at least two thiol groups.

11. The resin composition according to any one of claims 6 to 10, It is characterized in that The resin composition is used to form a color filter or a black matrix.

12. A polymer, It is characterized in that The polymer has a structure represented by formula (P'), In the general formula (P'), m is an integer from 0 to 5, n is an integer from 1 to 6, n+m is 1 to 6, p, q and r represent the molar contents of A, B and C respectively, p+q+r=1, p is greater than 0, q is greater than 0, r is greater than 0, p, q or r is the same or different in each of the structural units in n []. X is hydrogen or an organic group having 1 to 30 carbon atoms, Y is a monovalent to hexavalent organic group having 1 to 30 carbon atoms and derived from a bifunctional or higher thiol group-containing compound, A contains a structural unit represented by the general formula (NB), B contains at least one structural unit selected from the structural unit represented by the general formula (1) and the structural unit represented by the general formula (2), C contains a divalent structural unit derived from a copolymerizable compound having a double bond, There are multiple A's, B's, or C's that are identical or different from each other. Q contains an organic group that is the same as or different from A, B, and C, In the general formula (NB), R 1 , R 2 , R 3 and R 4 are independently a hydrogen atom or an organic group having 1 to 30 carbon atoms, a 1 is 0, 1, or 2, In the general formula (1), R p is a group having two or more (meth)acryloyl groups, In the general formula (2), R s It is a group having one (meth)acryloyl group.

13. The polymer according to claim 12, It is characterized in that The structure represented by the general formula (P') is the structure represented by the formula (P), In the general formula (P), n, p, q and r have the same meanings as in the general formula (P'), X, Y, A, B and C have the same meanings as in the general formula (P').

14. The polymer according to claim 12, It is characterized in that The bifunctional or higher thiol group-containing compound contains at least one compound selected from the following chemical formulas (s-1) to (s-20), 15. The polymer according to claim 12, It is characterized in that The B further contains a structural unit represented by formula (3), 16. The polymer according to claim 12, It is characterized in that The B further contains a structural unit represented by formula (MA), 17. The polymer according to claim 12, It is characterized in that The C contains a divalent structural unit derived from at least one compound selected from the group consisting of substituted or unsubstituted indene, maleimide, styrene, and norbornadiene.

18. The polymer according to claim 12, It is characterized in that The weight average molecular weight is 1,000 or more and 15,000 or less.

19. A resin composition, It is characterized in that The resin composition contains the polymer according to any one of claims 12 to 18.

20. The resin composition according to claim 19, It is characterized in that The resin composition further contains a compound having two or more (meth)acryloyl groups.

21. The resin composition according to claim 19, It is characterized in that The resin composition further contains a compound having one (meth)acryloyl group.

22. The resin composition according to claim 19, It is characterized in that The resin composition further contains a compound having a thiol group.

23. The resin composition according to claim 22, It is characterized in that The compound having a thiol group is a compound having at least two thiol groups.

24. The resin composition according to any one of claims 19 to 23, It is characterized in that The resin composition is used to form a color filter or a black matrix.