Light diffusion film, and polarizing plate having the same
By introducing a shaper layer and a light diffusion layer into the light diffusion film, and using light diffusion particles, the durability and optical performance problems of the light diffusion film during bonding are solved, and excellent processability and humidification durability are achieved.
Patent Information
- Application Number
- CN202080074336.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-24
- Filing Date
- 2020-10-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-10-14
AI Technical Summary
It is difficult for the existing light diffusion film to take into account excellent processability and optical properties when directly bonded, especially the durability is insufficient under humidified conditions and the like is prone to fracture.
A light diffusion film having an extrusion layer and a light diffusion layer is used. The extrusion layer includes a base material portion and a concave and convex portion. The light diffusion layer is arranged on the base material portion side of the extrusion layer and is laminated by an adhesive layer or an adhesive layer. The light diffusion layer includes light diffusible particles having a volume average particle size of 2 μm to 30 μm, which enhances the durability and optical properties of the film.
Excellent processability and optical characteristics are achieved, and humidification durability is improved in the optical laminate, preventing moisture from intrusion, and ensuring the stability of the light diffusion film and the brightness field angle.
Smart Images

Figure CN114600008B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a light-diffusing film and a polarizing plate including the light-diffusing film. Background Art
[0002] In recent years, there has been a strong desire for thinning and improving the design (e.g., narrowing the frame) of image display devices (e.g., liquid crystal display devices, organic EL display devices). Along with this, the desire for the integration and / or functional integration of optical components and / or optical films used in image display devices is also increasing. As an example of such integration or functional integration, a scheme has been proposed to directly bond a light-diffusing film to a specified optical component to impart a light-diffusing function. For a light-diffusing film, excellent optical properties and processability, as well as durability (especially humidification durability) of an optical laminate having the light-diffusing film are sometimes required, but in a light-diffusing film used by direct bonding, it is difficult to meet these properties in a good balance. In particular, a light-diffusing film composed of light-diffusing particles often breaks during film formation, making it difficult to produce stably and to have both processability and other properties (e.g., optical properties).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2012-118235
[0006] Patent Document 2: Japanese Patent Application Publication No. 2009-025774 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] The present invention has been made to solve the above-mentioned conventional problems, and its main object is to provide a light diffusing film which has excellent processability and optical properties and can contribute to the durability (particularly humidity durability) of an optical layered body when it is combined with other films to form an optical layered body.
[0009] Solutions for solving problems
[0010] The light diffusion film of the present invention comprises a shaped layer including a substrate and a concavo-convex portion disposed on one surface of the shaped layer, and a light diffusion layer disposed on the substrate side of the shaped layer.
[0011] In one embodiment, the light diffusion layer and the shaped layer are laminated via a pressure-sensitive adhesive layer or an adhesive layer.
[0012] In one embodiment, the light diffusion layer is directly formed on the shaped layer.
[0013] In one embodiment, the light diffusion layer includes light diffusing fine particles, and the volume average particle size of the light diffusing fine particles is 2 μm to 30 μm or less.
[0014] In one embodiment, the light diffusion film has a haze value of 30% to 95%.
[0015] According to another aspect of the present invention, a polarizing plate can be applied. The polarizing plate includes a polarizer and the light diffusion film laminated on the polarizer via an adhesive layer.
[0016] Effects of the Invention
[0017] According to the present invention, by including a shaped layer having uneven portions and a light diffusing layer, a light diffusing film having excellent processability and optical properties and contributing to the durability (particularly moisture durability) of an optical layered body when combined with other films to constitute the optical layered body can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a schematic cross-sectional view of a light-diffusing film according to one embodiment of the present invention.
[0019] Figure 2 It is a plan view schematically showing a typical example of the plan view shape of the convex part of the concavo-convex surface in the light-diffusing film according to the embodiment of the present invention.
[0020] Figure 3 This is a schematic cross-sectional view of an optical layered body according to one embodiment of the present invention.
[0021] Figure 4 This is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. DETAILED DESCRIPTION
[0022] The embodiments of the present invention are described below with reference to the accompanying drawings, but the present invention is not limited to these embodiments. It should be noted that the accompanying drawings are schematically shown for ease of observation, and the ratio of length, width and thickness, the shape and fineness of the concave and convex, etc. are different from the actual ones.
[0023] A. Light Diffuser Film
[0024] A-1. Overall composition
[0025] Figure 1Schematic cross-sectional view of a light-diffusing film according to an embodiment of the present invention. The light-diffusing film 100 of the illustrated example has a shaped layer 10 and a light-diffusing layer 20 disposed on one side of the shaped layer 10. The shaped layer 10 has a substrate portion 11 and a concave-convex portion 12 formed on one side of the substrate portion 11. The concave-convex portion 12 has a convex portion 12a and a concave portion 12b. The light-diffusing layer 20 is disposed on the substrate portion 11 side of the shaped layer 10 (the opposite side of the concave-convex portion 12). In one embodiment, the light-diffusing film of the present invention is used by pasting the concave-convex portion 12 to other films.
[0026] Figure 2 Schematic diagram of a top view showing a representative example of the top view shape of the convex part of the concavo-convex part in the shaped layer of the light diffusing film of one embodiment of the present invention. Figure 2 As shown, the recess 12b may have a unit cell structure surrounded by the protrusion 12a (substantially the wall surface of the protrusion). By forming the recess having the unit cell structure, when the light-diffusing film is stacked on other films to form an optical laminate, it is possible to prevent moisture from invading the optical laminate. In addition, by forming the recess having the unit cell structure, it is possible to obtain a light-diffusing film that can be cut with good processability by preventing undesirable conditions such as cracks and defects at the cutting portion. It should be noted that it is not necessary to make all the recesses into unit cell structures. For example, near the end edge of the light-diffusing film, the recess may also be open on the end edge side of the light-diffusing film.
[0027] The top view shape of the convex portion 12a in the concavo-convex portion can adopt any appropriate shape. Figure 2 As shown, it can be a regular shape (for example, a lattice shape) or an irregular shape. The spacing of the convex portions (the interval between the convex portions) is preferably less than 1000 μm, more preferably less than 500 μm, and further preferably less than 100 μm. When the top view shape of the convex portion has regularity, an oblique angle of 1 to 90 degrees can be set. When the top view shape of the convex portion is an irregular shape, the spacing refers to the average spacing, and it is preferably a distribution of more than 50% relative to the case where the average value of the spacing is within ±50%. If it is such a structure, when the light diffusing film is laminated on other films, the bonding strength between the light diffusing film and other films can be ensured, and good display quality can be ensured. In addition, when the light diffusing film is laminated on other films to form an optical laminate, it is possible to prevent moisture from invading the optical laminate.
[0028] In the present invention, by providing a shaped layer with concave and convex parts, when the light diffusion film is laminated on other films to form an optical laminate, only the convex part (substantially the upper part of the convex part) of the light diffusion film can be bonded to other films. It should be noted that in this specification, for convenience, sometimes the bonding of only the convex part is referred to as "point bonding". Through such point bonding, a substantially low refractive index part generated by a concave part (air part or gap part) is specified near the point bonding part. As a result, good light diffusion performance can be achieved and the brightness viewing angle can be increased. In the past, in image display devices, other films (such as polarizers (polarizing plates)) were set separately from the light diffusion film, and as a result, an air layer was sandwiched between the polarizing plate and the light diffusion film. On the one hand, the air layer will become an obstacle to thinning, and on the other hand, the brightness viewing angle can be maintained larger by retro-reflection based on the air layer. When other films are integrated with the light diffusion film, although thinning and functional integration can be achieved, the brightness viewing angle becomes smaller due to the exclusion of the above-mentioned air layer. By forming a low refractive index portion near the point bonding portion, light is efficiently retroreflected as when there is an air layer. Therefore, according to an embodiment of the present invention, by forming point bonding, the desired light diffusion performance can be exerted and the brightness viewing angle can be maintained large (wide).
[0029] In one embodiment, the above-mentioned shaped layer does not contain light diffusive particles. The shaped layer can be manufactured by any appropriate film-making method, but the shaped layer formed in a manner without light diffusive particles is not easy to break during film-making and has excellent processability. It is one of the achievements of the present invention that the shaped layer does not contain light diffusive particles (that is, even if it has good processability) to achieve good light diffusion performance and increase the brightness viewing angle.
[0030] The thickness of the light-diffusing film of the present invention is preferably 25 μm to 250 μm, more preferably 30 μm to 100 μm.
[0031] The haze value of the light-diffusing film of the present invention is preferably 30% to 95%, more preferably 40% to 93%, and further preferably 60% to 90%. According to the present invention, a light-diffusing film that can suppress brightness reduction and achieve excellent brightness viewing angle despite high haze value can be provided.
[0032] A-2. Shaping layer
[0033] As the resin constituting the shaping layer, any appropriate resin can be used. As the specific example of the resin constituting the shaping layer, (meth) acrylic resin, polyester resin (such as polyethylene terephthalate (PET)), cycloolefin resin (such as norbornene resin), cellulose resin (such as triacetyl cellulose (TAC)), polyvinyl alcohol resin, polycarbonate resin, polyamide resin, polyimide resin, polyether sulfone resin, polysulfone resin, polystyrene resin, polyolefin resin, acetate resin can be listed. These resins can be used alone or in combination of two or more. From the viewpoint of optical properties, transparency and versatility, preferably (meth) acrylic resin, polyester resin, cycloolefin resin, more preferably (meth) acrylic resin.
[0034] In addition, in this specification, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid.
[0035] As the (meth)acrylic resin, any appropriate (meth)acrylic resin can be adopted.
[0036] It should be noted that, in order to simplify the description, (meth)acrylic resins are referred to as acrylic resins below. Acrylic resins typically contain (meth)acrylic acid alkyl esters as main components as monomer units. As (meth)acrylic acid alkyl esters constituting the main skeleton of the acrylic resin, there can be exemplified (meth)acrylic acid alkyl esters having a linear or branched alkyl group with a carbon number of 1 to 18. They can be used alone or in combination. Furthermore, any appropriate comonomer can be introduced into the acrylic resin by copolymerization. The type, amount, copolymerization ratio, etc. of such comonomers can be appropriately set according to the purpose. The constituent components (monomer units) of the main skeleton of the acrylic resin will be described later with reference to general formula (2).
[0037] The acrylic resin may preferably have at least one selected from the group consisting of a glutarimide unit, a lactone ring unit, a maleic anhydride unit, a maleimide unit and a glutaric anhydride unit. An acrylic resin having a lactone ring unit is described in, for example, Japanese Patent Application Publication No. 2008-181078, the contents of which are incorporated herein by reference. The glutarimide unit is preferably represented by the following general formula (1):
[0038]
[0039] In the general formula (1), R 1 and R 2 Each independently represents hydrogen or an alkyl group having 1 to 8 carbon atoms, and R 3 represents an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aryl group having 6 to 10 carbon atoms. In the general formula (1), preferably: R1 and R 2 are each independently hydrogen or methyl, R 3 is hydrogen, methyl, butyl or cyclohexyl. More preferably: R 1 is methyl, R 2 is hydrogen, R 3 It is methyl.
[0040] The above-mentioned alkyl (meth)acrylate is typically represented by the following general formula (2).
[0041]
[0042] In the general formula (2), R 4 represents a hydrogen atom or a methyl group, R 5 represents a hydrogen atom, or an optionally substituted aliphatic or alicyclic hydrocarbon group having 1 to 6 carbon atoms. Examples of the substituent include halogen and hydroxyl. Specific examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, chloromethyl (meth)acrylate, 2-chloroethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2,3,4,5,6-pentahydroxyhexyl (meth)acrylate, and 2,3,4,5-tetrahydroxypentyl (meth)acrylate. In the general formula (2), R 5 A hydrogen atom or a methyl group is preferred. Therefore, a particularly preferred alkyl (meth)acrylate is methyl acrylate or methyl methacrylate.
[0043] The acrylic resin may contain only a single glutarimide unit, or may contain R 1 , R 2 and R 3 Different types of glutarimide units.
[0044] The content ratio of the glutarimide unit in the acrylic resin is preferably 2 mol% to 50 mol%, more preferably 2 mol% to 45 mol%, further preferably 2 mol% to 40 mol%, particularly preferably 2 mol% to 35 mol%, and most preferably 3 mol% to 30 mol%. If the content ratio is less than 2 mol%, there is a concern that the effects derived from the glutarimide unit (e.g., high optical properties, high mechanical strength, and thinning) cannot be fully exerted. If the content ratio exceeds 50 mol%, there is a concern that, for example, heat resistance and transparency become insufficient.
[0045] The acrylic resin may contain only a single alkyl (meth)acrylate unit, or may contain R4 and R 5 Different types of alkyl (meth)acrylate units.
[0046] The content ratio of the (meth) alkyl ester unit in the acrylic resin is preferably 50 mol% to 98 mol%, more preferably 55 mol% to 98 mol%, further preferably 60 mol% to 98 mol%, particularly preferably 65 mol% to 98 mol%, and most preferably 70 mol% to 97 mol%. If the content ratio is less than 50 mol%, there is a concern that the effects (such as high heat resistance and high transparency) derived from the (meth) alkyl ester unit cannot be fully exerted. If the above content ratio is more than 98 mol%, there is a concern that the resin becomes brittle and easily cracked, and high mechanical strength cannot be fully exerted, and productivity is poor.
[0047] The acrylic resin may contain units other than the glutarimide unit and the (meth)acrylic acid alkyl ester unit.
[0048] In one embodiment, the acrylic resin may contain, for example, 0% to 10% by weight of an unsaturated carboxylic acid unit that does not participate in the intramolecular imidization reaction described below. The content of the unsaturated carboxylic acid unit is preferably 0% to 5% by weight, more preferably 0% to 1% by weight. If the content is within this range, transparency, retention stability, and moisture resistance can be maintained.
[0049] In one embodiment, acrylic resin can contain copolymerizable vinyl monomer units (other vinyl monomer units) except the above. As these other vinyl monomers, for example, acrylonitrile, methacrylonitrile, ethacrylonitrile, allyl glycidyl ether, maleic anhydride, itaconic anhydride, N-methylmaleimide, N-ethylmaleimide, N-cyclohexylmaleimide, aminoethyl acrylate, propylaminoethyl acrylate, dimethylaminoethyl methacrylate, ethylaminopropyl methacrylate, cyclohexylaminoethyl methacrylate, N-vinyl diethylamine, N-acetyl vinylamine, allylamine, methylallylamine, N-methylallylamine, 2-isopropenyl-oxazoline, 2-vinyl-oxazoline, 2-acryloyl-oxazoline, N-phenylmaleimide, phenylaminoethyl methacrylate, styrene, alpha-methylstyrene, p-glycidyl styrene, p-aminostyrene, 2-styryl-oxazoline etc. can be listed. They can be used alone or in combination. Styrene monomers such as styrene and α-methylstyrene are preferred. The content of other vinyl monomer units is preferably 0 to 1% by weight, more preferably 0 to 0.1% by weight. Within this range, the expression of undesired phase difference and the decrease in transparency can be suppressed.
[0050] The imidization rate in the above-mentioned acrylic resin is preferably 2.5% to 20.0%. If the imidization rate is within such a range, a resin having excellent heat resistance, transparency and molding processability can be obtained, and the occurrence of scorching during film forming and the reduction of mechanical strength can be prevented. In the above-mentioned acrylic resin, the imidization rate is expressed by the ratio of glutarimide units to (meth) alkyl acrylate units. This ratio can be obtained, for example, from the NMR spectrum, IR spectrum, etc. of the acrylic resin. In the present embodiment, the imidization rate can be expressed using 1 H NMR BRUKER AvanceIII (400 MHz), through the resin 1 More specifically, the peak area of O-CH3 protons derived from (meth) alkyl acrylate around 3.5 to 3.8 ppm is defined as A, and the peak area of N-CH3 protons derived from glutarimide around 3.0 to 3.3 ppm is defined as B, and the result is determined by the following formula.
[0051] Imidization rate Im (%) = {B / (A+B)} × 100
[0052] The Tg (glass transition temperature) of the acrylic resin is preferably 110°C or more, more preferably 115°C or more, further preferably 120°C or more, particularly preferably 125°C or more, and most preferably 130°C or more. If Tg is 110°C or more, a polarizing plate including a light diffusion film obtained from such a resin is likely to be a polarizing plate with excellent durability. The upper limit of Tg is preferably 300°C or less, more preferably 290°C or less, further preferably 285°C or less, particularly preferably 200°C or less, and most preferably 160°C or less. If Tg is in such a range, excellent formability can be achieved.
[0053] The acrylic resin can be produced, for example, by the following method. The method comprises: (I) copolymerizing an alkyl (meth)acrylate monomer corresponding to the alkyl (meth)acrylate unit represented by the general formula (2) with an unsaturated carboxylic acid monomer and / or a precursor monomer thereof to obtain a copolymer (a); and (II) treating the copolymer (a) with an imidizing agent to perform an intramolecular imidization reaction of the alkyl (meth)acrylate monomer unit and the unsaturated carboxylic acid monomer and / or a precursor monomer unit thereof in the copolymer (a), thereby introducing a glutarimide unit represented by the general formula (1) into the copolymer.
[0054] The details of the acrylic resin and its production method are described in, for example, Japanese Patent Application Laid-Open No. 2018-155812 and Japanese Patent Application Laid-Open No. 2018-155813. The descriptions of these publications are incorporated herein by reference.
[0055] The height H of the convex portion 12a is preferably 5% to 40% relative to the thickness of the shaped layer. If it is within such a range, good point bonding can be achieved. In addition, making the height of the convex portion within the above range is also advantageous from the viewpoint of mechanical strength, thereby ideally maintaining the shape of the concave portion, and obtaining excellent light diffusivity and brightness viewing angle.
[0056] The height H of the protrusions 12a is more preferably 10% to 30% and even more preferably 10% to 20% of the thickness of the shaping layer. Within such a range, good point bonding can be achieved.
[0057] The height H of the convex portion 12a is preferably 2.5 μm to 25 μm, and more preferably 5 μm to 20 μm. Within such a range, good point bonding can be achieved.
[0058] The average area of the concave portions having the unit cell structure is preferably 5000 μm 2 If it is within such a range, a light diffusion film can be obtained which can suppress the decrease in brightness and realize an excellent brightness viewing angle. The average area of the concave portions having a unit cell structure is more preferably 5000 μm 2 ~50000μm 2 , more preferably 7000 μm 2 ~40000μm 2 , particularly preferably 8000 μm 2 ~30000μm 2 . If it is such a range, the above-mentioned effect becomes significant, and in addition, a light-diffusing film with excellent mechanical strength can be obtained. The average area of the concave portion having a cell structure can be obtained using image analysis software (free software "ImageJ"). That is, the inside and outside of the concave portion are determined by the threshold value of the binary image of the surface of the shaped film, and the outer frame of the concave portion is determined. The area within the determined frame is calculated and the average value of the calculated area is calculated, thereby being able to be obtained.
[0059] In one embodiment, the maximum length of the concave portion of the unit cell structure when viewed from above is preferably 300 μm or more, more preferably 400 μm or more, and further preferably 500 μm or more. If it is within such a range, even when the light diffusing film is cut and used, the light diffusing film can effectively prevent water intrusion and improve the durability near the end of the optical laminate. The maximum length of the concave portion of the unit cell structure refers to the corresponding distance of the longest distance between the wall surfaces of the convex portion forming the concave portion.
[0060] The area ratio of the concave portion relative to the overall area when looking down at the concave-convex portion is preferably 50% or more, preferably 60% or more, and more preferably 70% or more. The upper limit of the area ratio of the concave portion can be, for example, 90%. If the area ratio of the concave portion is within such a range, it is possible to impart good diffusion performance to the light diffusion film while maintaining a wide brightness viewing angle, and it is possible to ensure bonding strength when the light diffusion film is laminated on other films.
[0061] In the light-diffusing film of the present invention, it is preferred that the wall surface of the protrusion 12a exists in a region within 500 μm from the end edge of the light-diffusing film. In the present invention, when the light-diffusing film is laminated on other films to form an optical laminate, the protrusion 12a can prevent moisture from invading the optical laminate. By forming the wall surface of the protrusion 12a in a region within 500 μm from the end edge of the light-diffusing film, it is possible to effectively prevent moisture from invading and improve the durability near the end of the optical laminate. It is more preferred that the wall surface of the protrusion 12a exists in a region within 400 μm from the end edge of the light-diffusing film, and it is further preferred that the wall surface of the protrusion 12a exists in a region within 300 μm from the end edge of the light-diffusing film. It is preferred that the wall surface of the protrusion 12a exists in the entire region within 500 μm (preferably within 400 μm, more preferably within 300 μm) from the end edge of the light-diffusing film.
[0062] The ratio B / A of the cross-sectional area B of the concave portion to the cross-sectional area A of the entire concave-convex portion is preferably 50% or more, more preferably greater than 50%, further preferably 60% or more, and particularly preferably 70% or more. The upper limit of the ratio B / A may be, for example, 90%. If the ratio B / A is within such a range, it is possible to impart good diffusion properties to the light-diffusing film while maintaining a wide brightness viewing angle, and it is possible to ensure bonding strength when the light-diffusing film is laminated on other films. It should be noted that the cross-sectional area A of the entire concave-convex portion is the area of the portion surrounded by the line connecting the surface of the convex portion, the line connecting the bottom of the concave portion, and the line in the up-and-down direction at both ends of the film (for reference, the outside of this portion is surrounded by a dotted line and shown in FIG. Figure 1 ), the cross-sectional area B of the recess is the sum of the cross-sectional areas of each recess 22 (the area of the portion enclosed by the line of the wall of the adjacent convex portion, the line connecting the surface of the convex portion and the line connecting the bottom of the recess).
[0063] The thickness of the shaping layer is preferably 25 μm to 250 μm, more preferably 40 μm to 100 μm.
[0064] The thickness of the substrate portion is preferably 22.5 μm to 225 μm, more preferably 30 μm to 90 μm.
[0065] The concavoconvex part (concavoconvex shape) can be formed by any appropriate method. The concavoconvex shape can be formed, for example, by a surface roughening method or by using microparticles to impart concavoconvexity. As specific examples of the surface roughening method, embossing and sandblasting can be cited. The concavoconvex part (concavoconvex shape) can be formed representatively by shaping the surface of the melt-extruded film with an embossing roller.
[0066] In one embodiment, the base material and the concavo-convex part are made of the same material. Preferably, the base material and the concavo-convex part are made of the same material and are integrally formed.
[0067] A-3. Light diffusion layer
[0068] The light diffusion layer can be composed of a light diffusion element, or it can be composed of a light diffusion adhesive or a light diffusion adhesive. The light diffusion element can be a structure having a fine concave-convex structure on the surface (a light diffusion layer of external diffusion mode), or it can be a structure comprising a matrix and light diffusing particles dispersed in the matrix (a light diffusion layer of internal diffusion mode). In addition, the light diffusion element can be a light diffusion cured layer (for example, a layer formed by coating a dispersion liquid (a coating liquid for forming a light diffusion layer) containing a matrix resin, light diffusing particles and additives as required on any appropriate substrate and curing and / or drying it), or it can be a light diffusing film (for example, a commercially available film). The matrix of the light diffusion adhesive is composed of an adhesive, and the matrix of the light diffusion adhesive is composed of an adhesive. It should be noted that when the light diffusion layer is composed of a light diffusion adhesive or a light diffusion adhesive, in order to protect the surface of the light diffusion layer, any appropriate protective film can also be arranged on the side of the light diffusion layer opposite to the excipient layer.
[0069] Details of the light diffusion element and the light diffusion adhesive are described in, for example, Japanese Patent Publication No. 2012-83741, Japanese Patent Publication No. 2012-83742, Japanese Patent Publication No. 2012-83743, Japanese Patent Publication No. 2012-83744, Japanese Patent Publication No. 2013-235259, and Japanese Patent Publication No. 2014-224964. The descriptions of these publications are incorporated herein by reference. Surface concavoconvex light diffusion elements are well known in the art.
[0070] The light diffusion layer is directly arranged on the above-mentioned excipient layer, or is laminated with the above-mentioned excipient layer by means of an adhesive layer or an adhesive layer. The directly arranged excipient layer can be formed by coating. As the light diffusion layer formed in this way, for example, there can be listed: a light diffusion layer formed by coating the above-mentioned light diffusion layer forming coating liquid; a light diffusion layer composed of a light diffusion adhesive or a light diffusion adhesive, etc. As a light diffusion layer configured by means of an adhesive layer or an adhesive layer, a light diffusion film, etc. can be listed. The adhesive layer that bonds the excipient layer to the light diffusion layer includes any appropriate adhesive. As the adhesive, for example, rubber adhesives, acrylic adhesives, silicone adhesives, epoxy adhesives, cellulose adhesives, etc. can be listed, preferably acrylic adhesives. The adhesive layer that bonds the excipient layer to the light diffusion layer includes any appropriate adhesive. As the adhesive, for example, water-based adhesives (such as vinyl alcohol adhesives), curable adhesives (such as active energy ray curing adhesives or thermosetting adhesives) and the like can be listed.
[0071] The light diffusion performance of the light diffusion layer can be represented by a haze value, for example. The haze value of the light diffusion layer is preferably 20% to 90%, more preferably 30% to 87%, and further preferably 40% to 85%. The haze value of the light diffusion layer can be controlled by adjusting the fine concavo-convex structure of the surface, the constituent material of the matrix (binder), and the constituent material, volume average particle size, and compounding amount of the light diffusing fine particles.
[0072] The total light transmittance of the light diffusion layer is preferably 75% or more, more preferably 80% or more, and even more preferably 85% or more.
[0073] The thickness of the light diffusion layer can be appropriately adjusted according to the configuration and desired light diffusion performance, etc. Specifically, the thickness of the light diffusion layer is preferably 2 μm to 100 μm, more preferably 5 μm to 30 μm.
[0074] In one embodiment, the light diffusion layer is composed of a light diffusion adhesive. The light diffusion adhesive typically includes an adhesive as a matrix and light diffusing fine particles dispersed in the adhesive.
[0075] As the adhesive (matrix), any appropriate substance can be used. As a specific example of the adhesive, rubber adhesive, acrylic adhesive, silicone adhesive, epoxy adhesive, cellulose adhesive, etc. can be listed, preferably acrylic adhesive. By using acrylic adhesive, a light diffusion layer with excellent heat resistance and transparency can be obtained. The adhesive can be used alone or in combination of two or more.
[0076] As the acrylic adhesive, any appropriate substance can be used. The glass transition temperature of the acrylic adhesive is preferably -60°C to -10°C, more preferably -55°C to -15°C. The weight average molecular weight of the acrylic adhesive is preferably 200,000 to 2,000,000, more preferably 250,000 to 1,800,000. By using an acrylic adhesive having such characteristics, appropriate adhesion can be obtained. The refractive index of the acrylic adhesive is preferably 1.40 to 1.65, more preferably 1.45 to 1.60.
[0077] The acrylic adhesive is usually obtained by polymerizing a main monomer that imparts adhesiveness, a comonomer that imparts cohesion, and a functional group-containing monomer that imparts adhesiveness and serves as a crosslinking point. The acrylic adhesive having the above characteristics can be synthesized by any appropriate method, for example, by referring to "Chemistry and Application of Adhesion / Adhesion" written by Katsuhiko Nakamae and published by Dai Nippon Book Co., Ltd.
[0078] The content of the binder in the light diffusion layer is preferably 50% by weight to 99.7% by weight, more preferably 52% by weight to 97% by weight.
[0079] As light diffusive particles, any appropriate particles can be used. As specific examples of light diffusive particles, inorganic particles, polymer particles, etc. can be listed. Light diffusive particles are preferably polymer particles. As the material of polymer particles, for example, polystyrene resin, polyurethane resin, melamine resin, silicone resin, acrylic resin, styrene-acrylic copolymer resin can be listed. These resins have a desired refractive index difference with the adhesive, and have excellent dispersibility with the adhesive, so a light diffusive layer with excellent light diffusion performance can be obtained. Preferably, it is a polystyrene resin. The shape of the light diffusive particles can be, for example, spherical, flat, or irregular. The light diffusive particles can be used alone or in combination of two or more.
[0080] The volume average particle size of the light diffusing particles is preferably greater than 1 μm and less than 30 μm, more preferably 2 μm to 30 μm, further preferably 2 μm to 25 μm, and particularly preferably 3 μm to 20 μm. By making the volume average particle size the above range, a light diffusing layer with excellent optical properties can be obtained. In particular, when light diffusing particles with a volume average particle size of more than 2 μm are used, a light diffusing layer with significantly excellent optical properties such as coloring that prevents transmitted light can be obtained. The volume average particle size can be measured using an ultracentrifugal automatic particle size distribution measuring device.
[0081] The refractive index of the light diffusing fine particles is preferably 1.50 or more, more preferably 1.55 to 1.70, and further preferably 1.58 to 1.65.
[0082] The absolute value of the difference in refractive index between the light diffusing fine particles and the binder (matrix) is preferably 0.05 or more, more preferably 0.07 to 0.15, and even more preferably 0.10 to 0.13.
[0083] The content of the light diffusing fine particles in the light diffusing layer is preferably 0.3 to 50% by weight, more preferably 3 to 48% by weight. When the amount of the light diffusing fine particles is within the above range, a light diffusing layer having excellent light diffusing performance can be obtained.
[0084] The light diffusion layer may contain any appropriate additive. Examples of the additive include an antistatic agent and an antioxidant.
[0085] In another embodiment, the light diffusion layer is composed of a light diffusion element. In this case, the light diffusion layer typically includes a matrix and light diffusing particles dispersed in the matrix. The matrix is, for example, composed of an ionizing radiation curable resin. As ionizing radiation, for example, ultraviolet rays, visible light, infrared rays, and electron beams can be listed. Ultraviolet rays are preferably ultraviolet rays, and therefore, the matrix is preferably composed of an ultraviolet curable resin. As ultraviolet curable resins, for example, acrylic resins, aliphatic (for example, polyolefin) resins, and urethane resins can be listed. Regarding light diffusing particles, the same particles as those that can be used in light diffusing adhesives can also be used. It should be noted that, in this embodiment, the above-mentioned matrix can include a resin component and an ultrafine particle component. At this time, a refractive index modulation region in which the refractive index changes substantially continuously can be formed outside the surface of the light diffusing particles. The refractive index modulation region can be formed by a substantial gradient of the dispersion concentration of the ultrafine particle component in the matrix. By adopting this structure, backscattering can be suppressed. As described above, the resin component is preferably composed of an ultraviolet curable resin (for example, an acrylic resin). Specific examples of the monomer components constituting the acrylic resin include pentaerythritol triacrylate (PETA: molecular weight 298), neopentyl glycol diacrylate (NPGDA: molecular weight 212), dipentaerythritol hexaacrylate (DPHA: molecular weight 632), dipentaerythritol pentaacrylate (DPPA: molecular weight 578), and trimethylolpropane triacrylate (TMPTA: molecular weight 296). The ultrafine particle component is preferably composed of an inorganic compound. Preferred inorganic compounds include, for example, metal oxides and metal fluorides. Specific examples of metal oxides include zirconium oxide (zirconium oxide) (refractive index: 2.19), aluminum oxide (refractive index: 1.56 to 2.62), titanium oxide (refractive index: 2.49 to 2.74), and silicon oxide (refractive index: 1.25 to 1.46). Specific examples of metal fluorides include magnesium fluoride (refractive index: 1.37) and calcium fluoride (refractive index: 1.40 to 1.43). The details of the light diffusion layer (light diffusion element) including such a matrix are described in, for example, Japanese Patent Application Laid-Open No. 2010-250295 or Japanese Patent Application Laid-Open No. 2012-088692, and these descriptions are incorporated herein by reference.
[0086] B. Optical laminate
[0087] B-1. Overall composition
[0088] Figure 3Schematic cross-sectional view of an optical laminate according to an embodiment of the present invention. The optical laminate 200 shown in the figure comprises a light diffusing film 100 and another film 110 disposed on one side of the light diffusing film 100. The light diffusing film 100 and the other film 110 are stacked in such a manner that the concavo-convex portion 12 of the shaped layer 10 of the light diffusing film 100 faces the other film 110. Typically, the light diffusing film 100 and the other film 110 are stacked with an adhesive layer 120 interposed therebetween.
[0089] As described above, in the concavoconvex portion 12 of the light diffusion film 100, the ratio B / A of the cross-sectional area B of the concave portion to the cross-sectional area A of the entire concavoconvex portion is preferably 50% or more, more preferably greater than 50%, further preferably 60% or more, and particularly preferably 70% or more. The upper limit of the ratio B / A can be, for example, 90%. The ratio B / A can correspond to the porosity. If it is within such a range, an optical laminate that can achieve good light diffusion performance and increase the brightness viewing angle and has excellent mechanical strength can be obtained.
[0090] B-2. Other films
[0091] Any appropriate film may be used as other films, such as optical films such as polarizers, wavelength conversion films, and polarized light reflection films, glass (preferably thin glass), and resin films (such as protective films).
[0092] In one embodiment, a polarizer is used as the other film. In this embodiment, the light diffusion film functions as a polarizer protective film, and the optical laminate may be a polarizing plate. The details of the polarizing plate will be described later.
[0093] B-3. Adhesive layer
[0094] The adhesive layer is composed of any appropriate adhesive or binder, and is typically formed of a water-based adhesive (eg, a vinyl alcohol-based adhesive) or a curable adhesive (eg, an active energy ray-curable adhesive or a thermosetting adhesive).
[0095] In one embodiment, the adhesive layer contains an active energy ray-curable adhesive. When the adhesive layer is formed using an active energy ray-curable adhesive, an optical layered body can be obtained without damaging the concavo-convex shape of the light-diffusing film.
[0096] As the above-mentioned active energy ray-curable adhesive, any appropriate adhesive can be used as long as it is an adhesive that can be cured by irradiation with active energy rays. As active energy ray-curable adhesives, for example, ultraviolet curable adhesives, electron beam curable adhesives, etc. can be listed. As specific examples of the curing form of active energy ray-curable adhesives, free radical curing, cation curing, anion curing, and combinations thereof (for example, a mixture of free radical curing and cation curing) can be listed.
[0097] Examples of the active energy ray-curable adhesive include an adhesive containing, as a curing component, a compound (eg, a monomer and / or an oligomer) having a radical polymerizable group such as a (meth)acrylate group or a (meth)acrylamide group.
[0098] Specific examples of the active energy ray-curable adhesive and the curing method thereof are described in, for example, Japanese Patent Application Laid-Open No. 2012-144690, which is incorporated herein by reference.
[0099] As a coating method of the above-mentioned active energy ray-curable adhesive, any appropriate method can be adopted according to the viscosity of the adhesive, the thickness of the desired adhesive layer, etc. As a coating method, for example, coating based on a reverse coater, a gravure coater (direct, reverse, offset), a rod reverse coater, a roll coater, a die coater, a rod coater, a rod coater, etc. can be cited. In addition, coating based on a dipping method can also be adopted.
[0100] Any appropriate method may be adopted as a method for curing the active energy ray-curable adhesive. Conditions such as the wavelength and irradiation amount of the active energy ray may be set to any appropriate conditions depending on the type of curable compound used.
[0101] The thickness of the adhesive layer at the maximum portion is preferably 0.5 μm to 10 μm, more preferably 0.5 μm to 5 μm. If it is within such a range, it is possible to preferably form gaps caused by the concave-convexity of the shaped film, and an optical laminate with excellent mechanical strength can be obtained. In one embodiment, the portion where the adhesive layer has the maximum thickness may correspond to the gap from the upper surface of the convex portion of the light-diffusing film (the surface opposite to the other films) to the lower surface of the other films (the surface opposite to the light-diffusing film). In another embodiment, the portion where the adhesive layer has the maximum thickness may be the position corresponding to the concave portion of the light-diffusing film ( Figure 4). For example, the adhesive layer may be formed in a manner that covers at least a portion of the wall surface of the convex portion of the light diffusion film. In this case, the adhesive layer is not formed on the concave surface of the light diffusion film, and is preferably in a so-called meniscus shape. In this embodiment, it is possible to ensure a gap and obtain an optical laminate having excellent adhesion between the light diffusion film and other films.
[0102] In one embodiment, the thickness T of the adhesive layer formed on the upper surface of the convex portion of the light diffusion film is preferably thinner than the thickness (height) H of the convex portion. The ratio T / H of the thickness T to the height H of the convex portion is preferably 50% or less, more preferably 30% or less. If the ratio T / H is in such a range, good point bonding can be achieved. The lower limit of the ratio T / H can be, for example, 10%.
[0103] The light-diffusing film has concave and convex parts, and the convex parts of the light-diffusing film are bonded (i.e., point-bonded) to other films and laminated, but the above-mentioned adhesive layer is preferably formed in the gap part on the other films in addition to the parts involved in bonding. In other words, the above-mentioned adhesive layer preferably covers at least a part (preferably all) of the surface of the other film at the concave part (void part) of the light-diffusing film. In this way, the degradation of other films can be prevented. This effect is particularly useful when the other films are degraded due to moisture, external gas, etc., for example, it is useful when the other film is a polarizer. The thickness of the adhesive layer at the gap part may be constant or not. In one embodiment, the adhesive layer in the gap part has a meniscus shape, and its thickness is not constant. As a method for providing an adhesive layer in the gap part, for example, a method of bonding the other film to the light-diffusing film after forming an adhesive precursor layer on the other film can be cited.
[0104] The storage modulus of the above-mentioned adhesive layer at 25°C is preferably 100kPa or more, more preferably 100kPa to 3GPa, and further preferably 100kPa to 1GPa. If it is such a range, the gaps caused by the concavo-convex of the light diffusion film can be ideally formed, and an optical laminate with excellent mechanical strength can be obtained. It should be noted that the storage modulus can be obtained by dynamic viscoelasticity measurement. The dynamic viscoelasticity measurement is, for example, for an adhesive sample with a thickness of 2mm×a diameter of 8mm, using the "Advanced Rheometric Expansion System (ARES)" manufactured by Rheometric Scientific, with deformation mode: torsion, measurement frequency: 1Hz, heating rate 5°C / min, and measurement temperature: -50°C to 150°C.
[0105] B-4.Polarizing plate
[0106] As described above, in one embodiment, the optical layered body is a polarizing plate. Figure 4It is a cross-sectional schematic diagram of a polarizing plate according to an embodiment of the present invention. The polarizing plate 200a shown in the figure comprises a polarizer 110a and a polarizer protective film 100a laminated on the polarizer 110a by means of an adhesive layer 120. The polarizer protective film 100a in this embodiment is equivalent to the above-mentioned light diffusion film. In addition, the polarizer 110a is equivalent to the above-mentioned other film. The polarizer protective film 100a is configured in such a way that the above-mentioned concave-convex portion side is the polarizer 110a side. The adhesive layer is as described above. In practice, another protective film 140 is configured on the opposite side of the polarizer protective film 100a. In practice, an adhesive layer 150 is further provided as the outermost layer so that the polarizing plate can be attached to the image display unit. It should be noted that an isolation film (not shown) is temporarily pasted on the surface of the adhesive layer 150 in a removable manner, so that the adhesive layer can be protected and a roll can be formed until the polarizing plate is actually used. The polarizing plate of the embodiment of the present invention can be used as a back side polarizing plate of an image display device, and can also be used as an identification side polarizing plate. According to the embodiment of the present invention, since the polarizer protective film itself has light diffusion performance and also serves as a light diffusion film, it can achieve significant thinning through the synergistic effect of the air layer exclusion effect.
[0107] Any appropriate polarizer may be adopted as the polarizer. For example, the resin film forming the polarizer may be a single-layer resin film or a laminate of two or more layers.
[0108] Specific examples of polarizers composed of a single-layer resin film include: polarizers obtained by dyeing and stretching hydrophilic polymer films such as polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films with dichroic substances such as iodine and dichroic dyes; polyene-based oriented films such as dehydrated PVA and dehydrochlorinated polyvinyl chloride films, etc. From the perspective of excellent optical properties, it is preferred to use a polarizer obtained by dyeing a PVA film with iodine and uniaxially stretching it.
[0109] The above-mentioned iodine-based dyeing is carried out, for example, by immersing the PVA film in an iodine aqueous solution. The stretching ratio of the above-mentioned uniaxial stretching is preferably 3 to 7 times. The stretching can be carried out after the dyeing treatment, or it can be carried out while dyeing. In addition, it is also possible to dye after stretching. The PVA film can be subjected to swelling treatment, cross-linking treatment, cleaning treatment, drying treatment, etc. as needed. For example, by immersing the PVA film in water for washing before dyeing, not only can the stains and anti-blocking agents on the surface of the PVA film be cleaned, but the PVA film can also be swollen to prevent uneven dyeing.
[0110] As specific examples of polarizers obtained using a laminate, there can be listed: a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a laminate of a resin substrate and a PVA-based resin layer formed by coating the resin substrate. The polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating the resin substrate can be made, for example, by the following method: a PVA-based resin solution is applied to a resin substrate, and the PVA-based resin layer is formed on the resin substrate by drying, thereby obtaining a laminate of the resin substrate and the PVA-based resin layer; the laminate is stretched and dyed to make the PVA-based resin layer into a polarizer. In the present embodiment, stretching typically includes immersing the laminate in an aqueous solution of boric acid and stretching it. Furthermore, stretching may also include stretching the laminate in the air at a high temperature (e.g., above 95°C) before stretching in an aqueous solution of boric acid, as required. The obtained laminate of resin substrate / polarizer can be used directly (that is, the resin substrate can be used as a protective layer of polarizer), or the resin substrate can be peeled off from the laminate of resin substrate / polarizer, and any appropriate protective layer corresponding to the purpose can be laminated on the peeling surface for use. The details of the manufacturing method of such a polarizer are described in, for example, Japanese Patent Publication No. 2012-73580. All the records of the publication are cited in this specification as a reference.
[0111] The thickness of the polarizer is, for example, 1 μm to 80 μm. In one embodiment, the thickness of the polarizer is preferably 1 μm to 20 μm, and more preferably 3 μm to 15 μm.
[0112] The polarizer protective film preferably has substantially optical isotropy. In this specification, "substantially optically isotropy" means that the in-plane phase difference Re(550) is 0nm to 10nm. The in-plane phase difference Re(550) is more preferably 0nm to 5nm, further preferably 0nm to 3nm, and particularly preferably 0nm to 2nm. If the Re(550) of the polarizer protective film is in such a range, it is possible to prevent the adverse effects on the display characteristics when the polarizing plate containing the polarizer protective film is applied to an image display device. It should be noted that Re(550) is the in-plane phase difference of the film measured at 23°C using light of a wavelength of 550nm. Re(550) is calculated using the formula: Re(550) = (nx-ny) × d. Here, nx is the refractive index in the direction where the refractive index in the plane is the largest (i.e., the slow axis direction), ny is the refractive index in the direction orthogonal to the slow axis in the plane (i.e., the fast axis direction), and d is the thickness of the film (nm).
[0113] The higher the transmittance at 380 nm when the thickness of the polarizer protective film is 40 μm, the more preferred. Specifically, the transmittance is preferably 75% or more, more preferably 80% or more, and further preferably 85% or more. If the transmittance is in such a range, the desired optical properties can be ensured. The transmittance can be measured, for example, by a method in accordance with ASTM-D-1003.
[0114] The haze of the polarizer protective film is preferably 50% to 99%, more preferably 70% to 95%.
[0115] The polarizer protective film preferably has the following properties: When the transmittance at 550 nm is 100%, the difference between the transmittance at 450 nm and 650 nm and the transmittance at 550 nm is preferably within ±5%, more preferably within ±2%.
[0116] Regarding the brightness viewing angle of the polarizer protective film, the brightness half-value angle (the angle at which the brightness becomes 50% of the front) is preferably 56° (28° on one side) or more, and more preferably 60° to 70° (30° to 35° on one side). Furthermore, the angle at which the brightness becomes 25% of the front is preferably 90° (45° on one side) or more, and more preferably 96° to 120° (48° to 60° on one side). According to an embodiment of the present invention, the polarizer protective film can be endowed with excellent diffusion properties, and the brightness viewing angle can be maintained wider.
[0117] The refractive index of the polarizer protective film as a whole is n F It is preferably 1.3 to 1.8, and more preferably 1.4 to 1.6. When the refractive index of the polarizer protective film is within such a range, the refractive index difference with the low refractive index portion defined by point bonding with the polarizer in the polarizing plate can be within a desired range.
[0118] The moisture permeability of the polarizer protective film is preferably 300 g / m 2 24 hr or less, more preferably 250 g / m 2 24 hr or less, more preferably 200 g / m 2 24 hr or less, particularly preferably 150 g / m 2 ·24hr or less, most preferably 100g / m 2 · 24 hr or less. When the water vapor permeability of the polarizer protective film is within such a range, a polarizing plate having excellent durability and moisture resistance can be obtained.
[0119] C. Image display device
[0120] The polarizing plate can be applied to an image display device. Therefore, the present invention also includes an image display device using such a polarizing plate. As representative examples of image display devices, liquid crystal display devices and organic electroluminescent (EL) display devices can be cited. The image display device adopts a structure known in the industry, so a detailed description is omitted.
[0121] Example
[0122] The present invention is specifically described below by way of examples, but the present invention is not limited to these examples. The measuring methods of various properties are as follows. It should be noted that, unless otherwise specified, the "parts" and "%" in the examples are by weight.
[0123] (1) Processability (tear strength)
[0124] The tear strength of the shaping layer was measured using the trouser tear method in accordance with JIS K7128-1. The test piece was cut into a specified size under constant temperature conditions (23°C, relative humidity 50%), and a 75 mm slit was cut. The tear test was performed at a speed of 200 mm / min. The tear strength of the remaining 50 mm was calculated by excluding the 20 mm at the beginning of the tear and the 5 mm before the end of the tear. The test was performed with N=5 and the average value was calculated.
[0125] When the tear strength was 0.5 N or less, there was a possibility of tearing during film formation, and thus it was recorded as NG.
[0126] (2) Optical properties
[0127] The content of the light diffusing fine particles was adjusted so that the haze of the light diffusing film was 80%, and the transmittance T(450) at a wavelength of 450 nm, the transmittance T(550) at a wavelength of 550 nm, and the transmittance T(650) at a wavelength of 650 nm were measured.
[0128] The case where the value of ((T450)-T(650)) / T(550) was within ±0.5 was evaluated as acceptable (○). Acceptable products had no coloration of transmitted light and were excellent in optical properties.
[0129] (3) Humidification durability
[0130] After the surface of the polarizer is coated with an adhesive at a thickness of 1 μm, the polarizer is bonded to the concave and convex surface of the light diffusion film (polarizer protective film) obtained in the embodiment and the comparative example, and then UV irradiation is performed to cure the adhesive to obtain a polarizing plate consisting of a shaped film (polarizer protective film) / adhesive layer / polarizer.
[0131] The polarizing plate shaping film (polarizer protective film) was laminated to a glass plate with the aid of an acrylic adhesive. The obtained laminate was placed in an environment of a temperature of 60° C. and a humidity of 90% for 500 hours. Then, the transmittance of the laminate was measured using an absorptiophotometer with an integrating sphere (“V7100” manufactured by JASCO Corporation).
[0132] The case where the transmittance after heating and humidification changed by 10% or more relative to the transmittance before heating and humidification was evaluated as unacceptable (×), and the case where the change was less than 10% was evaluated as acceptable (○).
[0133] <Example 1>
[0134] A methacrylic resin (manufactured by Kuraray Co., Ltd., product name "PARAPET HR-S") was introduced into a single screw extruder and melt-extruded at 260°C while a concavo-convex shape was given to one surface using an embossing roll to obtain a shaped layer (thickness: 50 μm, convex portion height: 10 μm, cell size: 15000 μm). 2 ).
[0135] A mixture of 10 parts of silica particles having a volume average particle size of 10 μm and acrylic ultraviolet curing resin was applied to the side of the shaped layer without the uneven shape. The coated layer was irradiated with ultraviolet rays to cure the ultraviolet curing resin to form a light diffusion layer, thereby obtaining a light diffusion film.
[0136] The obtained light-diffusing film was subjected to the above-mentioned evaluations (1) to (3). The results are shown in Table 1.
[0137] <Example 2>
[0138] A light-diffusing film was obtained in the same manner as in Example 1 except that silica particles having a volume average particle size of 6 μm were used as the silica particles of the light-diffusing layer.
[0139] The obtained light-diffusing film was subjected to the above-mentioned evaluations (1) to (3). The results are shown in Table 1.
[0140] <Example 3>
[0141] A light-diffusing film was obtained in the same manner as in Example 1 except that silica particles having a volume average particle size of 2 μm were used as the silica particles in the light-diffusing layer.
[0142] The obtained light-diffusing film was subjected to the above-mentioned evaluations (1) to (3). The results are shown in Table 1.
[0143] <Example 4>
[0144] In the same manner as in Example 1, a shaped layer was obtained.
[0145] On the side of the shaped layer without the uneven shape, the shaped layer and the acrylic film were laminated via an adhesive film (light-diffusing adhesive) in which silica particles were dispersed in an acrylic adhesive, thereby obtaining a light-diffusing film.
[0146] The obtained light-diffusing film was subjected to the above-mentioned evaluations (1) to (3). The results are shown in Table 1.
[0147] <Example 5>
[0148] In the same manner as in Example 1, a shaped layer was obtained.
[0149] The shaped layer and a light diffusing film (manufactured by Kimoto Co., Ltd., trade name "Diffusing Film MXE") were laminated on the side of the shaped layer without the uneven shape via an acrylic adhesive to obtain a light diffusing film. The light diffusing film was laminated with the surface opposite to the diffusion layer as the shaped layer side.
[0150] The obtained light-diffusing film was subjected to the above-mentioned evaluations (1) to (3). The results are shown in Table 1.
[0151] <Comparative Example 1>
[0152] 9 parts of silicone resin fine particles (volume average particle size 4.5 μm) as light diffusing fine particles were introduced into a single screw extruder with respect to 100 parts of a methacrylic resin (manufactured by Kuraray Co., Ltd., product name "PARAPET HR-S"), and melt-extruded at 260° C. while giving a concavo-convex shape to one surface with an embossing roll to obtain a light diffusing film (thickness: 50 μm, convex portion height: 10 μm, cell size: 15000 μm) 2 ).
[0153] The obtained light-diffusing film was subjected to the above-mentioned evaluations (1) to (3). The results are shown in Table 1.
[0154] <Comparative Example 2>
[0155] The prism film BEF2-T-155 manufactured by 3M Company was used for the above evaluation (3). At this time, after applying an adhesive to a thickness of 1 μm on the surface of the polarizer, the prism film was bonded to the prism side of the prism film.
[0156] [Table 1]
[0157]
[0158] Industrial Applicability
[0159] The light-diffusing film of the present invention can be used in various fields as a film capable of imparting a light-diffusing function. For example, the light-diffusing film of the present invention can be suitably used in a polarizing plate. The polarizing plate of the present invention can be suitably used in an image display device. The image display device of the present invention can be used for: mobile devices such as mobile information terminals (PDAs), smart phones, mobile phones, watches, digital cameras, and handheld game consoles; office automation equipment such as computer monitors, notebook computers, and copiers; home electrical appliances such as cameras, televisions, and microwave ovens; in-vehicle equipment such as rear-view displays, displays for car navigation systems, and car audio systems; display equipment such as digital signage and information displays for stores; security equipment such as monitoring displays; various uses such as nursing / medical equipment such as nursing displays and medical displays.
[0160] Description of Reference Numerals
[0161] 10. Forming layer
[0162] 11 Base material
[0163] 12 Concavoconvex part
[0164] 12a convex part
[0165] 12b recess
[0166] 20 Light diffusion layer
[0167] 100 Light Diffuser Film
[0168] 110 Other films
[0169] 120 Adhesive layer
[0170] 200 Optical laminate
Claims
1. A light-diffusing film comprising a shaping layer and a light-diffusing layer disposed on one side of the shaping layer, The shaping layer includes a base portion and a concave-convex portion disposed on one side of the base portion. The light diffusion layer is arranged on the substrate side of the shaping layer, The wall surface of the convex portion exists in a region within 500 μm from the edge of the light diffusion film. The ratio B / A of the cross-sectional area B of the concave portion to the cross-sectional area A of the entire concave-convex portion is 50% or more, The haze value of the light diffusion film is 30% to 95%.
2. The light diffusion film according to claim 1, in, The light diffusion layer and the shaping layer are laminated via a pressure-sensitive adhesive layer or an adhesive layer.
3. The light diffusion film according to claim 1, in, The light diffusion layer is directly formed on the shaped layer.
4. The light-diffusing film according to any one of claims 1 to 3, in, The light diffusion layer includes light diffusing fine particles, The volume average particle size of the light diffusing fine particles is 2 μm to 30 μm. 5 . A polarizing plate comprising: a polarizer; and the light-diffusing film according to claim 1 , which is laminated on the polarizer via an adhesive layer.
Citation Information
Patent Citations
Polarizer protection film, polarizing plate and image display device
JP2008181078A
Lens sheet, optical sheet for display, back light unit using it, and display device
JP2009025774A
Light diffusing element, polarizing plate with the same, liquid crystal display using both, and method for manufacturing the light diffusing element
JP2010250295A
Manufacturing method of thin polarizing film
JP2012073580A
Light-diffusing element, polarizing plate with light-diffusing element, and liquid crystal display device using the same
JP2012083741A