A hot extrusion method for profiles without core and shrinkage and a hot extrusion die thereof

By designing a single crescent-shaped feed inlet and curved motion path on the aluminum alloy hot extrusion die, the problems of sandwiching, shrinking and welding lines in aluminum alloy hot extrusion are solved, and uniform extrusion and welding of aluminum alloy profiles are achieved. High quality processing.

CN114602986BActive Publication Date: 2024-10-15CHUANGARC TECH INNOVATION (FOSHAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210286390.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-23
Publication Date
2024-10-15
Estimated Expiration
2042-03-23

AI Technical Summary

Technical Problem

In the hot extrusion processing of aluminum alloys, the peripheral density, center looseness, sandwiching and shrinkage problems caused by traditional solid aluminum profile molds, as well as welding line defects caused by multiple feed inlets, affect the profile quality.

Method used

A profile-free, no-shrink hot extrusion method and mold design are adopted. A single feed inlet is provided on the hot extrusion mold to form a curved crescent-shaped feed inlet and a curved movement path, so that the blank is evenly distributed in the mold. Squeeze to avoid straight movement and weld lines.

Benefits of technology

It achieves sandwich-free and shrink-free profile processing, improves the quality and uniformity of profiles, avoids the appearance of welding lines, and ensures higher processing quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114602986B_ABST
    Figure CN114602986B_ABST
Patent Text Reader

Abstract

The present invention provides a hot extrusion method for a profile without a core and a shrinkage tail and a hot extrusion die thereof; wherein the method comprises: feeding a processed bar into the hot extrusion die from a single feed port of an upper die of the hot extrusion die, wherein a blank formed by the processed bar is blocked inside the hot extrusion die and moves in a curve so that all the blanks are fully extruded, and then outputted from a profile forming port of a lower die of the hot extrusion die to complete the hot extrusion process. The method can avoid turbulence of the blank in the die, and the processed profile has no core and no shrinkage tail, and can also avoid welding lines in the profile, thereby improving the process quality of the profile.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hot extrusion, and more particularly to a hot extrusion method for a profile without a core and without a shrink tail and a hot extrusion die thereof. Background Art

[0002] In aluminum alloy extrusion processing, aluminum bars are usually placed in the internal cavity of the bladder, and the extruder pushes the extrusion gasket to extrude the aluminum bars into the die to form solid aluminum profiles. At present, this type of hot extrusion processing method has the following shortcomings:

[0003] (1) The inlet and outlet of the traditional solid aluminum profile mold are on the center line of the hot extrusion process; the center billet is not extruded or is slightly extruded, and there is a large pressure difference between the center of the extruded material and the two sides of the material. The solid aluminum profile formed by extrusion will have a very dense molecular spacing on the periphery and a relatively loose molecular structure in the center; the produced profile is prone to sandwiching at the front and shrinking at the tail.

[0004] (ii) Some new molds have several feed ports on the upper mold. The blanks are fed from each feed port and then merged in the welding chamber, and then formed and output from the profile forming port. However, in this type of mold, due to the spacing between the feed ports, the produced profiles will have welding line defects, affecting the quality of the profiles. Summary of the invention

[0005] In order to overcome the shortcomings and deficiencies in the prior art, the purpose of the present invention is to provide a hot extrusion method for a profile without a core and without a shrinkage tail and a hot extrusion die thereof; this method can avoid turbulence of the blank in the die, and the processed profile has no core and no shrinkage tail, and can also avoid the appearance of welding lines in the profile, thereby improving the process quality of the profile.

[0006] In order to achieve the above-mentioned object, the present invention is implemented by the following technical scheme: a method for hot extrusion of profiles without core and tail shrinkage, characterized in that: the processed rod is fed into the hot extrusion die from a single feeding port of the upper die of the hot extrusion die, and the blank formed by the processed rod is hindered inside the hot extrusion die and moves in a curve so that all the blanks are fully extruded, and then output from the profile forming port of the lower die of the hot extrusion die to complete the hot extrusion process.

[0007] The present invention can prevent part of the blank from moving straightly from the feed port to the profile forming port without hindrance, thereby causing part of the blank to be not extruded or insufficiently extruded and causing turbulence. The profile processed by the present invention has no sandwich and no shrinkage tail. In addition, a single feed port can prevent the problem of welding lines in the profile caused by multiple feed ports, thereby improving the processing quality of the profile.

[0008] A hot extrusion die for a profile without a sandwich and a shrink tail, characterized in that it comprises an upper die and a lower die; the upper die is provided with a feed inlet and a welding cavity 1 which are interconnected; the feed inlet is one and is in a crescent shape bending around the center line of the hot extrusion process; the lower die is provided with a welding cavity 2 and a profile forming port which are interconnected; the welding cavity 1 and the welding cavity 2 together form a welding chamber; the top wall of the welding cavity 1 is provided with a choke protruding downward; the center of the profile forming port is located on the center line of the hot extrusion process, and the profile forming port is completely located in the shadow area projected by the choke head onto the lower die, so that a curved path for the movement of the processed rod is formed between the feed inlet and the profile forming port.

[0009] The present invention can avoid that part of the blank moves straightly from the feed inlet to the profile forming port without hindrance, thereby causing part of the blank to be not extruded or insufficiently extruded and causing turbulence. The profile processed by the present invention has no sandwich and no shrinkage tail. The hot extrusion die of the present invention is only provided with a single feed inlet, which can avoid the problem of welding lines on the profile caused by multiple feed inlets, and improve the process quality of the profile; the feed inlet is in a crescent shape bent around the center line of the hot extrusion process, which can make the blank formed by the processed rod material evenly distributed before reaching the lower mold material forming port, so that the profile can be output under uniform extrusion, further improving the quality of the profile.

[0010] Preferably, on the upper end surface of the upper die, the middle of the feed port is located on one side of the upper die section BB, and both ends of the feed port are located on the other side of the upper die section BB; the upper die section BB refers to the upper die section where the center line of the hot extrusion process is located.

[0011] Preferably, the feed port gradually tilts away from the hot extrusion processing center line on the surface extending from the second welding cavity to the second welding cavity, forming an inclined surface. This design can increase the feeding area of ​​the feed port on the one hand, and on the other hand, it can play a blocking role, so that the blank can be better extruded.

[0012] Preferably, the upper die is a symmetrical structure with the upper die section AA as the symmetry plane; the upper die section AA and the upper die section BB intersect vertically, and the vertical intersection is the hot extrusion processing center line;

[0013] The outer arc of the top of the feed port is on the circumference of a circle with a point on the center line of the hot extrusion process as the center; in the side area of ​​the upper die section BB close to the center of the feed port, the inner arc of the bottom of the feed port is on the circumference of a circle with a point on the center line of the hot extrusion process as the center.

[0014] Preferably, the ratio of the diameter of the circumference of the circle to the diameter of the processed rod is: (0.85-0.95):1.

[0015] Preferably, the center of the bottom surface of the choke and the middle of the feed inlet are both located on the same side of the upper die section BB. The choke is biased toward the feed inlet, and the blank can easily reach the area of ​​the choke away from the feed inlet.

[0016] Preferably, the baffle head is provided with reinforcing ribs on the side away from the feed inlet; the reinforcing ribs are respectively fixed to the top wall of the welded cavity and one side wall of the welded cavity; a spacing is left between the bottom of the reinforcing ribs and the bottom of the baffle head.

[0017] Preferably, a gap of 2 is left between the bottom of the choke and the bottom of the upper die. The blank enters from the crescent-shaped inlet, passes through the circumference of the choke and reaches the welding area with a circular cross section, and is evenly distributed before reaching the profile forming port.

[0018] Preferably, the ratio of the feed port area to the cross-sectional area of ​​the processed rod is: 1:(2-4); the ratio of the cross-sectional area of ​​the profile forming port to the maximum cross-sectional area of ​​the welding chamber is: 1:(7-30).

[0019] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0020] 1. The present invention can prevent part of the blank from moving straightly from the feed port to the profile forming port without obstruction, thereby causing part of the blank to be not extruded or insufficiently extruded and causing turbulence, and the processed profile has no sandwich and no shrinkage;

[0021] 2. The present invention has only a single feed inlet, which can avoid the problem of welding lines on the profile caused by multiple feed inlets, and improve the process quality of the profile;

[0022] 3. The present invention can make the blank formed by processing the bar material evenly distributed before reaching the lower mold material forming port, so that the profile can be output under uniform extrusion, further improving the quality of the profile;

[0023] 4. The feed port of the present invention forms an inclined surface, which can not only increase the feeding area of ​​the feed port, but also play a blocking role, so that the blank can be better extruded. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a cross-sectional schematic diagram of a hot extrusion die of the present invention;

[0025] Figure 2 This is one of the schematic diagrams of the upper die structure of the hot extrusion die of the present invention;

[0026] Figure 3 This is the second schematic diagram of the upper die structure of the hot extrusion die of the present invention;

[0027] Figure 4 1 is a schematic diagram corresponding to the internal structure and cross section of the hot extrusion die of the present invention;

[0028] Figure 5 is a cross-sectional schematic diagram of the hot extrusion die of Example 2;

[0029] Figure 6 is a cross-sectional schematic diagram of the hot extrusion die of Example 3;

[0030] Among them, 1 is the upper mold, 2 is the lower mold, 3 is the feed port, 4 is the welding cavity one, 5 is the welding cavity two, 6 is the profile forming port, 7 is the baffle head, 8 is the inclined surface, 9 is the reinforcing rib, 10 is the outer arc, 11 is the inner arc, and 12 is the stop port. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0032] Embodiment 1

[0033] The present embodiment provides a method for hot extrusion of profiles without core and tail shrinkage, wherein a processed rod is fed into the hot extrusion die from a single feed port of an upper die of the hot extrusion die, and a blank formed by the processed rod is obstructed inside the hot extrusion die and moves in a curve so that all the blanks are fully extruded, and then output from a profile forming port of a lower die of the hot extrusion die to complete the hot extrusion process.

[0034] The present invention can prevent part of the blank from moving straightly from the feed port to the profile forming port without hindrance, thereby causing part of the blank to be not extruded or insufficiently extruded and causing turbulence. The profile processed by the present invention has no sandwich and no shrinkage tail. In addition, a single feed port can prevent the problem of welding lines in the profile caused by multiple feed ports, thereby improving the processing quality of the profile.

[0035] like Figures 1 to 4 As shown, this embodiment is a hot extrusion die for a profile without a sandwich and a shrinkage tail, comprising an upper die 1 and a lower die 2; the upper die 1 is provided with a feed port 3 and a welding cavity 4 which are interconnected; the lower die 2 is provided with a welding cavity 2 5 and a profile forming port 6 which are interconnected; the welding cavity 1 4 and the welding cavity 2 5 together form a welding chamber.

[0036] The upper die 1 is preferably a symmetrical structure with the section AA of the upper die 1 as the symmetry plane. There is one feed port 3, which is crescent-shaped and curved around the center line of the hot extrusion process. On the upper end surface of the upper die 1, the middle of the feed port 3 is located on one side of the section BB of the upper die 1, and both ends of the feed port 3 are located on the other side of the section BB of the upper die 1. The section AA of the upper die 1 intersects the section BB of the upper die 1 perpendicularly, and the perpendicular intersection is the center line of the hot extrusion process.

[0037] The crescent shape of the feed port 3 means that: the outer arc 10 of the top of the feed port 3 is on the circumference of a circle with a point on the hot extrusion processing center line as the center; in the area on the side of the cross section BB of the upper die 1 close to the center of the feed port 3, the inner arc 11 of the bottom of the feed port 3 is on the circumference of a circle with a point on the hot extrusion processing center line as the center; the ratio of the diameter of the circumference of the circle to the diameter of the processed rod is preferably: (0.85-0.95): 1. The ratio of the area of ​​the feed port 3 to the cross-sectional area of ​​the processed rod is preferably: 1: (2-4).

[0038] The feed port 3 gradually tilts away from the hot extrusion processing center line on the surface extending from the welding cavity 2 5 to the welding cavity 2 5, forming an inclined surface 8. This design can increase the feeding area of ​​the feed port 3 on the one hand, and can also play a blocking role on the other hand, so that the billet can be better extruded.

[0039] The top wall of the welding cavity 4 is provided with a choke 7 protruding downward; the center of the profile forming port 6 is located on the center line of the hot extrusion process, and the profile forming port 6 is completely located in the shadow area of ​​the choke 7 projected onto the lower die 2, so that a curved path for the processing rod to move is formed between the feed port 3 and the profile forming port 6. The ratio of the cross-sectional area of ​​the profile forming port 6 to the maximum cross-sectional area of ​​the welding chamber is preferably: 1: (7-30).

[0040] The center of the bottom surface of the choke head 7 and the middle of the feed inlet 3 are both located on the same side of the cross section BB of the upper die 1. The blank can easily reach the area of ​​the choke head 7 away from the feed inlet 3.

[0041] The baffle head 7 is provided with a reinforcing rib 9 on the side away from the feed inlet 3; the reinforcing rib 9 is respectively fixed to the top wall of the welding cavity 4 and the side wall of the welding cavity 4; a spacing of 1 is left between the bottom of the reinforcing rib 9 and the bottom of the baffle head 7. A spacing of 2 is left between the bottom of the baffle head 7 and the bottom of the upper mold 1. The blank enters from the crescent-shaped feed inlet 3, passes through the periphery of the baffle head 7, and reaches the welding area with a circular cross section, and is evenly distributed before reaching the profile forming port 6.

[0042] The welding cavity 1 4 extends from a side close to the feed port 3 to a side close to the welding cavity 2 5 and gradually increases in size.

[0043] The present invention can prevent part of the blank from moving straightly without hindrance from the feed port 3 to the profile forming port 6, thereby causing part of the blank to be not extruded or insufficiently extruded and causing turbulence; therefore, the profile obtained by the processing of the present invention has no sandwich and no shrinkage tail. The hot extrusion die of the present invention is only provided with a single feed port 3, which can avoid the problem of welding lines in the profile caused by multiple feed ports 3, thereby improving the process quality of the profile. The feed port 3 is in a crescent shape bent around the center line of the hot extrusion process, and combined with the flow control head offset toward the feed port, the blank formed by the processed rod can be evenly distributed before reaching the lower mold material forming port, so that the profile can be output under uniform extrusion, further improving the quality of the profile.

[0044] The hot extrusion die of the invention can be used for the production and processing of solid profiles such as cylindrical and square columns.

[0045] Embodiment 2

[0046] The present embodiment is a hot extrusion die for profiles without core and shrinkage tail, which is different from the first embodiment in that: in the present embodiment, the second welding cavity of the lower die is a stepped cavity, such as Figure 5 As shown; the rest of the structure of this embodiment is the same as that of the first embodiment.

[0047] Embodiment 3

[0048] The present embodiment is a hot extrusion die for profiles without core and shrinkage tail, which is different from the first and second embodiments in that: in the present embodiment, the upper die 1 and the lower die 2 are positioned with each other by means of a stopper 12, such as Figure 6 The rest of the structure of this embodiment is the same as that of the first or second embodiment.

[0049] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A hot extrusion die for profiles without core and shrinkage, characterized in that: The invention comprises an upper die and a lower die; the upper die is provided with a feed inlet and a welding cavity 1 which are interconnected; the feed inlet is one and is crescent-shaped and bends around the center line of the hot extrusion process; the lower die is provided with a welding cavity 2 and a profile forming port which are interconnected; the welding cavity 1 and the welding cavity 2 together form a welding chamber; the top wall of the welding cavity 1 is provided with a flow blocker protruding downward; the center of the profile forming port is located on the center line of the hot extrusion process, and the profile forming port is completely located in the shadow area projected by the flow blocker to the lower die, so that a curved path for the movement of the processed rod is formed between the feed inlet and the profile forming port; On the upper end surface of the upper die, the middle of the feed port is located on one side of the upper die section BB, and both ends of the feed port are located on the other side of the upper die section BB; the upper die section BB refers to the upper die section where the center line of the hot extrusion process is located; The upper die is a symmetrical structure with the upper die section AA as the symmetry plane; the upper die section AA and the upper die section BB intersect vertically, and the vertical intersection is the hot extrusion processing center line; The outer arc of the top of the feed port is on the circumference of a circle with a point on the center line of the hot extrusion process as the center; in the area on one side of the upper die section BB close to the center of the feed port, the inner arc of the bottom of the feed port is on the circumference of a circle with a point on the center line of the hot extrusion process as the center; The ratio of the diameter of the circle to the diameter of the processed rod is: (0.85-0.95):1; The ratio of the area of ​​the feed port to the cross-sectional area of ​​the processed rod is: 1:(2-4); the ratio of the cross-sectional area of ​​the profile forming port to the maximum cross-sectional area of ​​the welding chamber is: 1:(7-30).

2. The profile non-sandwich and non-shrinkage hot extrusion die according to claim 1, characterized in that: The feed port is gradually inclined away from the hot extrusion processing center line on a surface extending from the second welding cavity to the second welding cavity, forming an inclined surface.

3. The profile non-sandwich and non-shrinkage hot extrusion die according to claim 1, characterized in that: The center of the bottom surface of the baffle head and the middle of the feed opening are both located on the same side of the upper die section BB.

4. The profile non-sandwich and non-shrinkage hot extrusion die according to claim 1, characterized in that: The baffle head is provided with reinforcing ribs on the side away from the feed inlet; the reinforcing ribs are respectively fixed to the top wall of the welded cavity and one side wall of the welded cavity; a spacing is left between the bottom of the reinforcing ribs and the bottom of the baffle head.

5. The profile non-sandwich and non-shrinkage hot extrusion die according to claim 1, characterized in that: A gap of two is left between the bottom of the baffle head and the bottom of the upper mold.