Positive electrode sheet, battery, and electronic device

By optimizing the morphological structure and chemical composition in the lithium cobalt oxide positive electrode material and forming an accordion stack structure, the problem of irreversible phase change of lithium cobalt oxide at high voltage is solved, and the circulation performance and compaction density of the battery are improved.

CN114613938BActive Publication Date: 2024-11-12ZHUHAI COSMX BATTERY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210302390.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-25
Publication Date
2024-11-12
Estimated Expiration
2042-03-25

AI Technical Summary

Technical Problem

The existing lithium cobalt oxide positive electrode material undergoes irreversible phase change when the charging voltage is higher than 4.55V, resulting in a difference in ionic and electronic conductivity, affecting the cycling performance and compaction density of the battery.

Method used

Using lithium cobalt oxide positive electrode active material with regular morphological structure, the cross-sectional light-section technology and SEM imaging test ensures that the number of particles of a/b≥3 N≥2, and adjusts the components under different deliquification states to form an accordion. Stacked structure to improve compaction density and conductivity.

Benefits of technology

It significantly improves the compaction density of the positive electrode sheet and the cycling performance of the battery, enhances the structural stability and discharge capacity of the positive electrode material, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114613938B_ABST
    Figure CN114613938B_ABST
Patent Text Reader

Abstract

The present invention provides a positive electrode sheet, a battery, and an electronic device. In a first aspect, the present invention provides a positive electrode sheet, the positive electrode sheet comprising a positive electrode current collector and a positive electrode active layer disposed on at least one surface of the positive electrode current collector, the positive electrode active layer comprising a positive electrode active material; in a plane formed by the length direction and the thickness direction of the positive electrode sheet, the longest distance of the particles of the positive electrode active material in the length direction of the positive electrode sheet is a, the longest distance in the thickness direction of the positive electrode sheet is b, and in an area not less than 25 μm*25 μm, the number of particles of the positive electrode active material satisfying a / b≥3 is N, and N≥2. The positive electrode active material provided by the present invention has a relatively regular morphology structure, and is easy to form an accordion stacking structure, which helps to improve the structural integrity of the positive electrode active material, thereby improving the compaction density of the positive electrode sheet and the cycle performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a positive electrode sheet, a battery and an electronic device, and relates to the technical field of electrochemistry. Background Art

[0002] With the development of thinner and lighter consumer electronic products such as mobile phones and tablets, the requirements for battery energy density are also increasing. In order to improve the energy density of the battery, increasing the battery charging cut-off voltage and the compaction density of the positive electrode sheet is an effective method. As a common positive electrode active material, the structure of lithium cobalt oxide is an irregular sphere, and the improvement of compaction density is limited. Moreover, when the charging voltage is ≥4.55V (vs. Li), lithium cobalt oxide will undergo an irreversible phase change, that is, an irreversible phase change from the O3 phase to the H1-3 phase. The ionic conductivity and electronic conductivity of the H1-3 phase are poor, which will cause the capacity of lithium cobalt oxide to decay faster, thereby accelerating the destruction of the lithium cobalt oxide structure and affecting the battery's cycle performance. How to improve the compaction density of the positive electrode sheet and the cycle performance of the battery is a technical problem that needs to be solved urgently by technicians in this field. Summary of the invention

[0003] The invention provides a positive electrode sheet, which is used for improving the compaction density of the positive electrode sheet and the cycle performance of a battery.

[0004] The present invention also provides a battery and an electronic device, comprising the positive electrode sheet.

[0005] A first aspect of the present invention provides a positive electrode sheet, the positive electrode sheet comprising a positive electrode current collector and a positive electrode active layer disposed on at least one surface of the positive electrode current collector, the positive electrode active layer comprising a positive electrode active material;

[0006] In the plane formed by the length direction and the thickness direction of the positive electrode sheet, the longest distance between the particles of the positive electrode active material in the length direction of the positive electrode sheet is a, and the longest distance between the particles of the positive electrode active material in the thickness direction of the positive electrode sheet is b, and in an area not less than 25μm*25μm, the number of particles of the positive electrode active material satisfying a / b≥3 is N, and N≥2.

[0007] The present invention provides a positive electrode sheet, which is processed by CP (cross-section) technology and then subjected to SEM imaging test. Figure 1 CP-SEM image of the positive electrode sheet provided in one embodiment of the present invention, according to Figure 1 It can be seen that the positive electrode sheet includes a positive electrode current collector 100 and a positive electrode active layer arranged on the surface of the positive electrode current collector 100, and the positive electrode active layer includes a plurality of positive electrode active materials 200. Figure 1Taking the two positive electrode active material particles circled in the figure as an example, the positive electrode active material is in the shape of long strips, the longest distance of the positive electrode active material particles in the length direction of the positive electrode sheet is a, and the longest distance of the positive electrode active material particles in the thickness direction of the positive electrode sheet is b, and the sample is taken at any position of the plane with a size of not less than 25μm*25μm, so that the number of particles of the positive electrode active material satisfying a / b≥3 is N, and within the sampling range, the number of particles of the positive electrode active material satisfying a / b≥3 is greater than or equal to 2. The positive electrode active material provided by the present invention has a relatively regular morphological structure, and is easy to form an accordion stacking structure, which helps to improve the structural integrity of the positive electrode active material, thereby improving the compaction density of the positive electrode sheet and the cycle performance of the battery.

[0008] In a specific embodiment, the positive electrode active material is lithium cobalt oxide, whose structural formula is Li n-x Na x Co 1- y Me y O2, 0.70≤n≤1, 0<x≤0.15, 0≤y≤0.15, Me is selected from one or more of Al, Mg, Ti, Zr, Ni, Mn, Y, La, Sr, W, Sc, Ce, P, Nb, V, Ta, Te. It should be noted that when the positive electrode active material is in different delithiation states, the n value is also different. Before the positive electrode sheet component is selected, the n value in the positive electrode active material (powder state) is 1. After the positive electrode sheet component is selected, when the operating voltage of the battery including the positive electrode sheet is 3.6-4.0V, the n value is reduced to 0.70-1. This is mainly because during the first charge and discharge process of the battery, a part of the lithium ions are used to form a protective layer on the surface of the positive and negative electrodes, namely the CEI film and the SEI film, causing a part of the Li + The irreversible loss of Li is reduced in the positive electrode sheet after chemical composition selection.

[0009] By performing XRD tests on the positive electrode active material, it can be known that the lithium cobalt oxide provided by the present invention has characteristic peaks that are different from conventional lithium cobalt oxide. Specifically, the X-ray diffraction spectrum of the positive electrode active material has a 002 peak corresponding to the 002 crystal plane, a 102 peak corresponding to the 102 crystal plane, and a 103 peak corresponding to the 103 crystal plane. The lithium cobalt oxide having the above-mentioned crystal phase structure has a lower platform voltage than conventional lithium cobalt oxide, and has multiple platform voltages. At the same cut-off voltage, it has a higher discharge capacity per gram and a more stable structure, which helps to improve the capacity and cycle performance of the battery.

[0010] Furthermore, the diffraction angle 2θ of the 002 crystal plane is 18.6°±0.5°, the diffraction angle 2θ corresponding to the 102 peak is 41.7°±0.5°, and the diffraction angle 2θ corresponding to the 103 peak is 47.1°±0.5°.

[0011] The X-ray diffraction spectrum of the positive electrode active material also has a 101 peak corresponding to the 101 crystal plane, a 004 peak corresponding to the 004 crystal plane, and the peak intensity ratio of the 101 peak to the 004 peak is m. When m≥1.5, it helps to further improve the structural stability of the positive electrode material, thereby being more conducive to the deintercalation of lithium ions. Otherwise, the structural stability of the positive electrode material deteriorates, and there may be incomplete reaction, poor crystallinity, and other states, resulting in poor electrochemical performance.

[0012] The particle size of the positive electrode active material is 6-18 μm, and the particle size is the size of the positive electrode active material particles, which can be obtained by testing with a Malvern laser particle size analyzer.

[0013] Based on the special structure of the positive electrode active material provided by the present invention, the positive electrode active material provided by the present invention has an electrical conductivity of ≥1E under a force of ≥4KN. -4 S / cm; under a force of ≥30KN, compaction density ≥3.75g / cm 3 The specific test method is: placing the powdered positive electrode active material in a container, compacting it under a certain external force, and then performing conductivity and compaction density tests. The powder conductivity test uses the principle of four probes, which shows that the positive electrode active material provided by the present invention has good conductivity and helps to improve the compaction density of the positive electrode sheet.

[0014] In order to increase the number of positive electrode active material particles N per unit area, the compaction density of the positive electrode sheet is ≥4.0g / cm 3 .

[0015] After testing, the gram capacity of the positive electrode material is ≥196mAh / g (3.0-4.5V, vs.Li), and at a voltage of 3.0-4.5V, when 0.1C charge and discharge is performed for the first time, the discharge gram capacity obtained is defined as C0 mAh / g, the discharge gram capacity from the beginning of discharge to 4.4V is C1 mAh / g, and the gram capacity within the voltage range of 3.8V-3.7V is C2 mAh / g, and C1 / C0≥9%, C2 / C0≥25%.

[0016] The present invention also provides a method for preparing the above-mentioned positive electrode active material, which specifically comprises: step 1, preparing a compound Na containing at least Co and Na elements x CoO2, 0.68<x<0.74; Step 2, the compound Na containing Co and Na x CoO2 and a compound containing lithium are dispersed in deionized water, and an ion exchange reaction is performed to replace part of the Na ions in the first compound with Li ions to obtain a positive electrode material.

[0017] In a specific embodiment, the preparation of the positive electrode material specifically includes the following steps:

[0018] Step 1-1, weigh the compound containing the Co element and the compound containing the sodium element according to the required stoichiometric ratio, and use a high-speed mixer, a sand mill, a ball mill, a plow mixer, or an oblique mixer to fully mix them to obtain a mixed material. During the mixing process, water, alcohol or other solvent media can be added, and the mixture can be dried after being mixed evenly.

[0019] The cobalt-containing compound may be one or more of cobalt hydroxide, cobalt trioxide, doped cobalt trioxide, cobaltous oxide, cobalt oxyhydroxide, cobalt nitrate, and cobalt sulfate; the sodium-containing compound may be one or more of sodium-containing oxide, sodium carbonate, sodium nitrate, sodium hydroxide, sodium bicarbonate, and sodium sulfate;

[0020] In addition, a compound containing a doping element Me may be added, wherein the doping element Me includes one or more of Al, Mg, Ti, Zr, Ni, Mn, Y, La, Sr, W, Sc, Ce, P, Nb, V, Ta, and Te, and may specifically be a compound containing a doping element such as basic magnesium carbonate, magnesium hydroxide, zirconium oxide, aluminum oxide, yttrium oxide, and lanthanum oxide;

[0021] Furthermore, the cobalt-containing compound, the sodium-containing compound and the Me-containing compound are mixed according to Na:Co:Me=x:(1-y):y, 0.68<x<0.74, 0≤y≤0.15 for at least 4 hours to fully mix the compounds. A technician in this field can observe the mixing state of the compounds by SEM electron microscopy.

[0022] Step 1-2: After the mixed material prepared in step 1-1 is loaded into a crucible, the mixture is placed in a high-temperature sintering device such as a muffle furnace, a tunnel furnace, a roller kiln, a tube furnace, etc., and sintered at high temperature in an air or oxygen atmosphere to obtain a first compound Na x Co 1-y Me y O2, 0.68<x<0.74, 0≤y≤0.15.

[0023] Furthermore, the sintering temperature is 700-900° C. and the sintering time is 8-50 hours.

[0024] Step 2, mixing the first compound synthesized in step 1-2 with the lithium-containing compound in a desired ratio and dispersing them in deionized water to carry out an ion exchange reaction, wherein most of the Na ions in the first compound are replaced by Li ions through the free migration and diffusion of sodium ions and lithium ions in the aqueous solution. After the reaction is completed, the reaction product is washed and dried to obtain a positive electrode material;

[0025] The compound containing lithium element can be one or more of lithium carbonate, lithium chloride, lithium bromide, lithium iodide, lithium nitrate, lithium hydroxide, and lithium fluoride. If necessary, some carbon-containing compounds or fast ion conductor compounds can be added to improve the conductivity of the positive electrode material.

[0026] The mass ratio of the lithium-containing compound to the first compound is ≥1, further 1-3; the mass ratio of the solvent to the first compound is ≥5, further 20-150.

[0027] The reaction equipment used includes a closed container equipment with a sealing function and a stirring ability, such as a wet coating reaction equipment, a coprecipitation reaction equipment, etc.; the stirring speed during the reaction is 10-200 rpm, the reaction temperature is 70-125°C, the reaction time is ≥5H, and further, the reaction time is 10-15H;

[0028] The equipment used for drying includes blast oven, vacuum drying oven, rotary kiln, disc dryer, etc. The drying temperature is 80-180℃ and the drying time is ≥10H.

[0029] On the basis of the above-mentioned positive electrode active material, a binder and a conductive agent are matched to prepare a positive electrode active layer slurry, and the slurry is coated on at least one surface of the positive electrode current collector to obtain a positive electrode active layer, and finally the positive electrode sheet is obtained by drying and rolling. The positive electrode current collector can be aluminum foil, the binder is selected from one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyacrylate lithium (PAALi), and the conductive agent is selected from one or more of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes, single-walled carbon nanotubes, multi-arm carbon nanotubes, and carbon fibers. The mass ratio of the positive electrode active material, the conductive agent, and the binder is (70-99): (0.5-15): (0.5-15), and further, the mass ratio of the positive electrode active material, the conductive agent, and the binder is (80-98): (1-10): (1-10).

[0030] A second aspect of the present invention provides a battery, comprising any of the above-mentioned positive electrode sheets.

[0031] The present invention provides a battery, specifically, the above-mentioned positive electrode sheet is assembled with a negative electrode sheet, a separator and an electrolyte to obtain a battery, wherein the negative electrode sheet includes a negative electrode current collector and a negative electrode active layer arranged on the surface of the negative electrode current collector, the negative electrode active layer includes a negative electrode active material, a conductive agent and a binder, the negative electrode active material is selected from one or more of artificial graphite, natural graphite, hard carbon, mesophase carbon microspheres, lithium titanate, silicon carbon, silicon dioxide, the types of the conductive agent and the binder are the same as those of the positive electrode active layer, the mass ratio of the negative electrode active material, the conductive agent and the binder is (70-99): (0.5-15): (0.5-15), and further, the mass ratio of the negative electrode active material, the conductive agent and the binder is (80-98): (1-10): (1-10).

[0032] In the preparation process of the negative electrode sheet, the above-mentioned negative electrode active material, conductive agent and binder are mixed in a certain proportion and dispersed in a solvent to obtain a negative electrode active layer slurry, which is then coated on the surface of the negative electrode collector to obtain a negative electrode sheet. The negative electrode collector can be copper foil.

[0033] The diaphragm is a conventional material in the art, such as a material with polypropylene as the base material, or a rubber-coated diaphragm with ceramic coated on one side or both sides thereof.

[0034] The electrolyte is a conventional material in the art, including an organic solvent, a lithium salt and an additive. The organic solvent includes ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), and fluoroethylene carbonate (FEC). The additive has a structure as shown in the following formula, and its mass is 0.1-10% of the total mass of the electrolyte.

[0035]

[0036] The positive electrode active material provided by the present invention is suitable for high voltage batteries, and the working voltage of the battery is specifically 3.0-4.5V. Under this voltage condition, since the positive electrode active material has a high gram capacity and structural stability, the battery including the positive electrode active material also has good capacity and cycle performance.

[0037] The third aspect of the present application also provides an electronic device, comprising the battery provided in the second aspect of the present invention. The battery can be used as a power source or energy storage unit of the electronic device. The electronic device can be, but is not limited to, a mobile device (such as a mobile phone, a tablet computer, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), etc.

[0038] For electronic devices such as mobile phones, tablet computers, and laptops, they are usually required to be thin and light, and lithium-ion batteries can be used as power sources.

[0039] The implementation of the present invention has at least the following advantages:

[0040] 1. The positive electrode active material provided by the present invention has a relatively regular morphology and structure, and is easy to form an accordion stacking structure, which helps to improve the compaction density of the positive electrode sheet and the cycle performance of the battery.

[0041] 2. The positive electrode active material provided by the present invention has a lower platform voltage and multiple platform voltages than conventional lithium cobalt oxide. At the same cut-off voltage, it has a higher discharge capacity and a more stable structure, which helps to improve the capacity and cycle performance of the battery.

[0042] 3. The battery provided by the present invention has good capacity and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a CP-SEM image of a positive electrode sheet provided in one embodiment of the present invention.

[0044] Description of reference numerals:

[0045] 100-positive electrode current collector;

[0046] 200-positive electrode active material. DETAILED DESCRIPTION

[0047] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.

[0049] Example 1

[0050] The method for preparing the positive electrode material provided in this embodiment comprises the following steps:

[0051] (1) 3.656 kg of sodium carbonate powder and 29.105 kg of cobalt nitrate hexahydrate powder were weighed and placed in a high-speed mixing device. After mixing at 300 rpm for 3 minutes, at 500 rpm for 5 minutes, and at 1000 rpm for 10 minutes, the mixture was taken out and confirmed to be uniform after no white sodium carbonate spots were present in the mixture.

[0052] (2) 30 g of the mixed material was placed in a ceramic crucible and sintered at high temperature using a pit-type muffle furnace with an equipment model of VBF-1200X. The sintering temperature rise curve was 5°C / min. When the temperature was raised to 750°C, the sample was sintered at a constant temperature for 10 h. After the sample was naturally cooled to room temperature after sintering, the sample was taken out to obtain the sintered cobalt- and sodium-containing compound Na 0.69 CoO2;

[0053] (3) Add 200 ml of deionized water, 10.49 g of lithium hydroxide monohydrate and 10.59 g of lithium chloride into a reaction container, stir for 5 min at 78° C. and 20 rpm, and weigh 10 g of the cobalt- and sodium-containing compound Na obtained in step 2. 0.69 CoO2, maintained at 78°C, rotation speed 20rpm, the reaction continued for 8 hours;

[0054] (4) After the reaction is completed, the reaction product is taken out, filtered and washed with deionized water three times, and then dried in a forced air drying oven at 90° C. for 8 hours to obtain a positive electrode material.

[0055] Example 2

[0056] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0057] (3) Add 200 ml of deionized water, 10.49 g of lithium hydroxide monohydrate and 21.71 g of lithium bromide into a reaction vessel, stir for 5 min at 78° C. and 20 rpm, and weigh 10 g of the cobalt- and sodium-containing compound Na obtained in step 2. 0.69 CoO2, maintain 78℃, rotation speed 20rpm, and continue the reaction for 8 hours.

[0058] Example 3

[0059] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0060] (3) Add 200 ml of deionized water, 10.49 g of lithium hydroxide monohydrate and 33.46 g of lithium iodide into a reaction container, stir for 5 min at 78° C. and 20 rpm, and weigh 10 g of the cobalt- and sodium-containing compound Na obtained in step 2. 0.69 CoO2, maintain 78℃, rotation speed 20rpm, and continue the reaction for 8 hours.

[0061] Example 4

[0062] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0063] (3) Add 200 ml of deionized water, 10.49 g of lithium hydroxide monohydrate and 6.48 g of lithium fluoride into a reaction container, stir for 5 min at 78° C. and 20 rpm, and weigh 10 g of the cobalt- and sodium-containing compound Na obtained in step 2. 0.69 CoO2, maintain 78℃, rotation speed 20rpm, and continue the reaction for 8 hours.

[0064] Example 5

[0065] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0066] (3) Add 200 ml of deionized water, 16.78 g of lithium hydroxide monohydrate and 3.69 g of lithium carbonate into a reaction container, stir for 5 min at a water temperature of 78° C. and a rotation speed of 20 rpm, and weigh 10 g of the compound Na containing cobalt and sodium obtained in step 2. 0.69 CoO2, maintain 78℃, rotation speed 20rpm, and continue the reaction for 8 hours.

[0067] Example 6

[0068] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0069] (3) Add 200 ml of deionized water, 16.78 g of lithium hydroxide monohydrate and 16.96 g of lithium chloride into a reaction vessel, stir for 5 min at a water temperature of 78° C. and a rotation speed of 20 rpm, and weigh 10 g of the compound Na containing cobalt and sodium obtained in step 2. 0.69 CoO2, maintain 78℃, rotation speed 20rpm, and continue the reaction for 8 hours.

[0070] Example 7

[0071] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0072] (3) Add 200 ml of deionized water, 16.78 g of lithium hydroxide monohydrate and 4.24 g of lithium chloride into a reaction vessel, stir for 5 min at a water temperature of 78° C. and a rotation speed of 20 rpm, and weigh 10 g of the compound Na containing cobalt and sodium obtained in step 2. 0.69 CoO2, maintain 78℃, rotation speed 20rpm, and continue the reaction for 8 hours.

[0073] Example 8

[0074] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0075] (3) Add 200 ml of deionized water, 10.49 g of lithium hydroxide monohydrate and 10.59 g of lithium chloride into a reaction container, stir for 5 min at a water temperature of 78° C. and a rotation speed of 30 rpm, and weigh 10 g of the compound Na containing cobalt and sodium obtained in step 2. 0.69 CoO2, maintain 78℃, rotation speed 30rpm, and continue the reaction for 8 hours.

[0076] Example 9

[0077] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0078] (1) Weigh 2.138 kg of sodium oxide powder and 29.105 kg of cobalt nitrate hexahydrate powder, put them into a high-speed mixing device, mix them at 300 rpm for 3 minutes, mix them at 500 rpm for 5 minutes, and mix them at 1000 rpm for 10 minutes. Then take out the mixture and confirm that there are no white spots of sodium oxide in the mixture. The mixture is considered to be uniform.

[0079] Example 10

[0080] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0081] (1) Weigh 3.656 kg of sodium carbonate powder and 7.493 kg of cobaltous oxide powder, put them into a high-speed mixing device, mix them at 300 rpm for 3 minutes, mix them at 500 rpm for 5 minutes, and mix them at 1000 rpm for 10 minutes. Then take out the mixture and confirm that there are no white spots of sodium oxide in the mixture. The mixture is considered to be uniform.

[0082] Embodiment 11

[0083] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0084] (1) Weigh 3.656 kg of sodium carbonate powder and 9.293 kg of cobalt hydroxide powder, put them into a high-speed mixing device, mix them at 300 rpm for 3 minutes, mix them at 500 rpm for 5 minutes, and mix them at 1000 rpm for 10 minutes. Then take out the mixture and confirm that there are no white spots of sodium carbonate in the mixture. The mixture is considered to be uniform.

[0085] Example 12

[0086] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0087] (1) Weigh 3.656 kg of sodium carbonate powder and 8.026 kg of cobalt tetroxide powder, put them into a high-speed mixing device, mix them at 300 rpm for 3 minutes, mix them at 500 rpm for 5 minutes, and mix them at 1000 rpm for 10 minutes. Then take out the mixture and confirm that there are no white spots of sodium carbonate in the mixture. The mixture is considered to be uniform.

[0088] Embodiment 13

[0089] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0090] (1) Weigh 3.656 kg of sodium carbonate powder, 9.200 kg of cobalt hydroxide powder and 50.98 g of nano alumina powder, put them into a high-speed mixing device, mix them at 300 rpm for 3 minutes, mix them at 500 rpm for 5 minutes, and mix them at 1000 rpm for 10 minutes. Then take out the mixture and confirm that there are no white spots of sodium carbonate in the mixture. The mixture is considered to be uniform.

[0091] Embodiment 14

[0092] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0093] (1) Weigh 3.656 kg of sodium carbonate powder, 9.014 kg of cobalt hydroxide powder and 152.94 g of nano-alumina powder, put them into a high-speed mixing device, mix them at 300 rpm for 3 minutes, mix them at 500 rpm for 5 minutes, and mix them at 1000 rpm for 10 minutes. Then take out the mixture and confirm that there are no white spots of sodium carbonate in the mixture. The mixture is considered to be uniform.

[0094] Embodiment 15

[0095] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0096] (1) Weigh 3.656 kg of sodium carbonate powder, 8.828 kg of cobalt hydroxide powder and 254.9 g of nano-alumina powder, put them into a high-speed mixing device, mix them at 300 rpm for 3 minutes, mix them at 500 rpm for 5 minutes, and mix them at 1000 rpm for 10 minutes. Then take out the mixture and confirm that there are no white spots of sodium carbonate in the mixture. The mixture is considered to be uniform.

[0097] Example 16

[0098] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0099] (1) 3.656 kg of sodium carbonate powder, 9.200 kg of cobalt hydroxide powder and 40.30 g of nano magnesium oxide powder were weighed and placed in a high-speed mixing device. After mixing at 300 rpm for 3 minutes, at 500 rpm for 5 minutes and at 1000 rpm for 10 minutes, the mixture was taken out and confirmed to be uniform after no white sodium carbonate spots were present in the mixture.

[0100] Embodiment 17

[0101] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0102] (1) Weigh 3.656 kg of sodium carbonate powder, 9.014 kg of cobalt hydroxide powder and 120.91 g of nano magnesium oxide powder, put them into a high-speed mixing device, mix them at 300 rpm for 3 minutes, mix them at 500 rpm for 5 minutes, and mix them at 1000 rpm for 10 minutes. Then take out the mixture and confirm that there are no white spots of sodium carbonate in the mixture. The mixture is considered to be uniform.

[0103] Embodiment 18

[0104] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0105] (1) Weigh 3.656 kg of sodium carbonate powder, 8.828 kg of cobalt hydroxide powder and 201.52 g of nano magnesium oxide powder, put them into a high-speed mixing device, mix them at 300 rpm for 3 minutes, mix them at 500 rpm for 5 minutes, and mix them at 1000 rpm for 10 minutes. Then take out the mixture and confirm that there are no white spots of sodium carbonate in the mixture. The mixture is considered to be uniform.

[0106] Embodiment 19

[0107] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0108] (1) Weigh 2.138 kg of sodium oxide powder and 9.293 kg of cobalt hydroxide powder, put them into a high-speed mixing device, mix them at 300 rpm for 3 minutes, mix them at 500 rpm for 5 minutes, and mix them at 1000 rpm for 10 minutes. Then take out the mixture and confirm that there are no white spots of sodium oxide in the mixture. The mixture is considered to be uniform.

[0109] Embodiment 20

[0110] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0111] (1) Weigh 2.138 kg of sodium oxide powder, 9.200 kg of cobalt hydroxide powder and 50.98 g of nano-alumina powder, put them into a high-speed mixing device, mix them at 300 rpm for 3 minutes, mix them at 500 rpm for 5 minutes, and mix them at 1000 rpm for 10 minutes. Then take out the mixture and confirm that there are no white spots of sodium oxide in the mixture. The mixture is considered to be uniform.

[0112] Embodiment 21

[0113] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0114] (1) Weigh 2.138 kg of sodium oxide powder, 9.014 kg of cobalt hydroxide powder and 152.94 g of nano-alumina powder, put them into a high-speed mixing device, mix them at 300 rpm for 3 minutes, mix them at 500 rpm for 5 minutes, and mix them at 1000 rpm for 10 minutes. Then take out the mixture and confirm that there are no white spots of sodium carbonate in the mixture. The mixture is considered to be uniform.

[0115] Embodiment 22

[0116] The preparation method of the positive electrode material provided in this embodiment can refer to Example 1, except that:

[0117] (1) Weigh 2.138 kg of sodium oxide, 8.828 kg of cobalt hydroxide powder and 254.9 g of nano-alumina powder, put them into a high-speed mixing device, mix them at 300 rpm for 3 minutes, mix them at 500 rpm for 5 minutes, and mix them at 1000 rpm for 10 minutes. Then take out the mixture and confirm that there are no white spots of sodium oxide in the mixture. The mixture is considered to be uniform.

[0118] Comparative Example 1

[0119] The positive electrode material provided in this comparative example is conventional undoped lithium cobalt oxide, and its chemical composition is Li 1.003 CoO2, the preparation method comprises the following steps:

[0120] (1) Lithium carbonate and conventional non-doped spherical Co3O4 particles purchased on the market were weighed at a molar ratio of Li:Co=100.3:100, and the two substances were mixed using the same stirring equipment as in the experimental example at 300 rpm for 3 minutes, 500 rpm for 5 minutes, and 1000 rpm for 10 minutes. The mixture was taken out and it was confirmed that there were no white lithium carbonate spots in the mixture, and the mixture was considered to be uniform;

[0121] (2) 30 g of the mixed material was placed in a ceramic crucible and sintered at high temperature using a pit-type muffle furnace with an equipment model of VBF-1200X. The sintering temperature rise curve was 5°C / min. When the temperature was raised to 1050°C, the sample was sintered at a constant temperature for 10 h. After the sample was naturally cooled to room temperature after sintering, the sample was taken out to obtain the sintered cobalt- and lithium-containing compound Li 1.003 CoO2;

[0122] (3) After the sintered lithium cobalt oxide was crushed and ground, the powder was placed in a muffle furnace again at 950°C for 8 hours, and then the sintered product was crushed to obtain Li2O3 with a D50 of 15.2 μm without any doping or coating. 1.003 CoO2.

[0123] Comparative Example 2

[0124] The positive electrode material provided in this comparative example is high voltage doped coated lithium cobalt oxide, and its chemical composition is Li 1.0028 Co 0.982 Al 0.014 Mg 0.002 La 0.002 O2;

[0125] The preparation method of the positive electrode material comprises the following steps:

[0126] (1) Lithium carbonate and conventional spherical Co3O4 particles doped with Al and La purchased on the market and magnesium oxide particles were weighed in a molar ratio of Li:Co:Mg=100.28:98.2:0.2. The stoichiometric ratio of the Co3O4 particles was Co:Al:La=98.2:1.4:0.2. The two substances were mixed using the same stirring equipment as in the experimental example at 300 rpm for 3 minutes, 500 rpm for 5 minutes, and 1000 rpm for 10 minutes. The mixture was taken out and it was confirmed that there were no white spots of lithium carbonate in the mixture. The mixture was considered to be uniform.

[0127] (2) 30 g of the mixture was placed in a ceramic crucible and sintered at high temperature using a pit-type muffle furnace with a model of VBF-1200X. The sintering temperature was increased by 5°C / min. When the temperature was increased to 1030°C, the mixture was sintered at a constant temperature for 10 h. After the mixture was naturally cooled to room temperature, the sample was taken out to obtain the sintered cobalt- and lithium-containing compound Li 1.0028 Co 0.982 Al 0.014 Mg 0.002 La 0.002 O2;

[0128] (3) The sintered lithium cobalt oxide was crushed and ground, and then weighed with titanium dioxide at a molar ratio of Co:Ti=98.2:0.2. The two materials were then placed in a high-speed mixing device, and the mixing program was set. After mixing at 300 rpm for 3 minutes, at 500 rpm for 5 minutes, and at 1000 rpm for 10 minutes, the mixture was taken out and the powder was placed in a muffle furnace again at 950°C for 8 hours. The sintered product was then crushed to obtain a doped and coated high-voltage lithium cobalt oxide material Li with a D50 of 14.8 μm. 1.0028 Co 0.982 Al 0.014 Mg 0.002 La 0.002 Ti 0.002 O2.

[0129] Comparative Example 3

[0130] The preparation method of the positive electrode material provided in this comparative example can refer to Example 1, except that:

[0131] (3) Weigh 10.49 g of lithium hydroxide monohydrate, 10.59 g of lithium chloride and 10 g of the compound containing cobalt and sodium obtained in step 2. 0.69 CoO2 is added into the mixer, mixed evenly and then sintered at 300℃ for 5 hours.

[0132] Comparative Example 4

[0133] The preparation method of the positive electrode material provided in this comparative example can refer to Example 1, except that:

[0134] (3) Weigh 10.49 g of lithium hydroxide monohydrate, 10.59 g of lithium chloride and 10 g of the cobalt- and sodium-containing compound Na obtained in step 2. 0.69 CoO2 is added into the mixer, mixed evenly and then sintered at 250°C for 5 hours.

[0135] The positive electrode materials provided in Examples 1-22 and Comparative Examples 1-4 were subjected to XRD test, conductivity test and compaction density test. The crystal plane diffraction angle, peak intensity ratio, conductivity and compaction density test results obtained by XRD test are shown in Table 1:

[0136] Table 1 Test results of positive electrode active materials provided by Examples 1-22 and Comparative Examples 1-4

[0137]

[0138] It can be found from the data in Table 1 that compared with Comparative Examples 1-2, the positive electrode active materials provided by the present invention all have characteristic peaks corresponding to the 002 crystal plane, the 102 crystal plane, and the 103 crystal plane, and under the force of 8KN, the conductivity is ≥1E-4 S / cm, under the force of 30KN, compaction density ≥3.75g / cm 3 , indicating that the positive electrode active material provided by the present invention has better discharge gram capacity, structural stability, and conductive performance. At the same time, the positive electrode active material provided by the present invention is easy to be compacted, which helps to improve the compaction density of the positive electrode sheet.

[0139] According to the XRD data provided in Examples 1-12 in Table 1, different preparation raw materials and proportions have a certain influence on the phase peak position and peak intensity of the positive electrode material; according to the XRD data provided in Examples 13-22, it can be seen that with the increase of the content of the doping element, the peak intensity ratio of the 101 and 004 crystal planes in the positive electrode material is significantly improved; according to Comparative Examples 3-4, compared with the ion exchange reaction using sintering, the peak intensity ratio m of the 101 crystal plane / 004 crystal plane in the positive electrode material prepared by the solution method provided by the present invention is significantly improved.

[0140] The positive electrode active materials provided in Examples 1-22 and Comparative Examples 1-4 were subjected to a button capacity test. The preparation method of the button battery is as follows: the positive electrode active material is mixed with conductive carbon black (SP) and PVDF in a weight ratio of 8:1:1, and dispersed in a solvent to obtain a positive electrode active layer slurry. The slurry is coated on an aluminum foil current collector, and the positive electrode sheet is prepared by roller pressing. The positive electrode sheet is then punched into a small disc with a diameter of 12 mm using a film mold. After drying and weighing, a button battery is assembled in a glove box under Ar protective atmosphere using a 2025 button battery shell, a Li metal disc as the negative electrode, and a conventional high-voltage lithium cobalt oxide electrolyte. After the button cell was manufactured, it was left to stand for 4 hours under normal conditions and then the first charge and discharge capacity test was carried out. The test conditions were as follows: 0.1C charging to 4.5V, constant voltage charging to 0.025C cutoff, and then left to stand for 3 minutes, and then 0.1C discharging to 3.0V. The first discharge capacity C0 mAh / g was recorded, and the discharge capacity in grams C1 mAh / g from the start of discharge to the voltage cutoff of 4.4V was defined. The capacity in grams released within the discharge voltage range of 3.8V-3.7V in the discharge capacity was C2 mAh / g. C1 / C0 and C2 / C0 were calculated. The results are shown in Table 2.

[0141] The positive electrode active materials provided in Examples 1-22 and Comparative Examples 1-2 were amplified to a certain amount, mixed with conductive carbon black and PVDF in a weight ratio of 96:2:2, dispersed in a solvent to prepare a positive electrode active layer slurry, and coated on the surface of the positive electrode aluminum current collector, and rolled according to the compaction density shown in Table 2 to prepare a positive electrode sheet, and the positive electrode sheet was treated with CP and then subjected to SEM imaging test. Under the condition of a magnification of 5000 (i.e., the sampling area is 25μm*25μm), the number of particles N of the positive electrode active material with a / b≥3 was counted, and the statistical results are shown in Table 2.

[0142] The positive electrode sheet is assembled with the negative electrode sheet, the separator and the electrolyte to obtain a lithium-ion battery, wherein the preparation method of the negative electrode sheet comprises: mixing artificial graphite, styrene diene rubber (SBR), sodium carboxymethyl cellulose and conductive carbon black in a weight ratio of 94:3:2:1, dispersing the mixture in water and mixing it by double planetary mixing to obtain a negative electrode active layer slurry, and coating the mixture on a negative electrode copper current collector to obtain a negative electrode sheet;

[0143] The electrolyte includes an organic solvent and an additive, the organic solvent includes ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC) and fluoroethylene carbonate (FEC), and the additive has a structure as shown below:

[0144]

[0145] Then the lithium ion battery cycle performance test was conducted. The cycle performance test process was as follows: at 25°C, the battery was charged to 4.50V at a constant current with a charge rate of 1C, then charged to 4.50V at a constant voltage with a charge rate of 0.05C, and then discharged to 3.0V at a discharge rate of 1C. This charge and discharge cycle was repeated 500 times. The discharge capacity at the first cycle and the discharge capacity at the 500th cycle were measured, and the capacity retention rate after the cycle was calculated: the capacity retention rate after the cycle = (discharge capacity at the 500th cycle) / (discharge capacity at the first cycle)*100%. The results are shown in Table 2:

[0146] Table 2 Performance test results of positive electrode sheets and lithium-ion batteries assembled from Examples 1-22 and Comparative Examples 1-2

[0147]

[0148] According to Table 2, the positive electrode sheet prepared from the positive electrode active material provided by the present invention is suitable for a higher compaction density. Thanks to the accordion stacking structure in the positive electrode sheet, within the same area, the number of particles N satisfying a / b≥3 is also significantly increased, indicating that the regularity of the particles of the positive electrode active material is improved, and with the increase of the doping element content, the number of particles satisfying this condition is significantly increased. According to Examples 13-22, with the increase of the doping element content in the positive electrode active material, the number of particles N also increases, indicating that the regularity of the particles is significantly increased, which is helpful to improve the cycle performance of the lithium-ion battery.

[0149] According to Table 2, the gram capacity of the positive electrode active material provided by the present invention is significantly improved. Specifically, C1 / C0≥9%, C2 / C0≥25%, indicating that the positive electrode active material with a special structure provided by the present invention has more charge and discharge platforms and higher gram capacity. In addition, based on the lower platform voltage and good structural stability of the positive electrode active material, the capacity retention rate of the lithium-ion battery after 500 cycles is above 80%, and it has good cycle performance under high voltage.

[0150] In summary, the positive electrode active material provided by the present invention can enable the lithium-ion battery to have a higher discharge capacity and excellent cycle performance at a high voltage, and can meet people's demand for thinner lithium-ion batteries.

[0151] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A positive electrode sheet, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active layer comprises a positive electrode active material; In the plane formed by the length direction and thickness direction of the positive electrode sheet, the longest distance of the particles of the positive electrode active material in the length direction of the positive electrode sheet is a, and the longest distance in the thickness direction of the positive electrode sheet is b, and in any area not less than 25 μm*25 μm, the number of particles of the positive electrode active material satisfying a / b≥3 is N, and N≥2; The compaction density of the positive electrode sheet is ≥4.0g / cm 3 ; The positive electrode active material is Li n-x Na x Co 1-y Me y O2, 0.70≤n≤1, 0<x≤0.15, 0≤y≤0.15, Me is selected from one or more of Al, Mg, Ti, Zr, Ni, Mn, Y, La, Sr, W, Sc, Ce, P, Nb, V, Ta, Te; The X-ray diffraction spectrum of the positive electrode active material has a 002 peak corresponding to the 002 crystal plane, a 102 peak corresponding to the 102 crystal plane, and a 103 peak corresponding to the 103 crystal plane; The diffraction angle 2θ of the 002 crystal plane is 18.6°±0.5°, the diffraction angle 2θ corresponding to the 102 peak is 41.7°±0.5°, and the diffraction angle 2θ corresponding to the 103 peak is 47.1°±0.5°; The X-ray diffraction spectrum of the positive electrode active material has a 101 peak corresponding to the 101 crystal plane and a 004 peak corresponding to the 004 crystal plane, and the peak intensity ratio of the 101 peak to the 004 peak is m, and m≥1.

5.

2. The positive electrode sheet according to claim 1, characterized in that: The particle size of the positive electrode active material is 6-18 μm.

3. The positive electrode sheet according to claim 1, characterized in that: The positive electrode active material has an electrical conductivity of ≥1E under a force of ≥4KN -4 S / cm; under a force of ≥30KN, compaction density ≥3.75g / cm 3 .

4. A battery, characterized in that: A positive electrode sheet comprising any one of claims 1 to 3.

5. An electronic device, characterized in that: The electronic device comprises the battery according to claim 4.