An injection molding method based on ultra-high molecular weight polyethylene

By controlling the pressure and temperature in the mold cavity in ultra-high molecular weight polyethylene injection molding, combined with the back pressure control system driven by high-pressure cylinder, the problem of uneven air intake and injection material density in the mold cavity is solved, and high efficiency and stability are achieved The production of finished products has improved product quality and production efficiency.

CN114619632BActive Publication Date: 2024-11-12NINGBO SHUANGMA MASCH IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210129704.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-11
Publication Date
2024-11-12
Estimated Expiration
2042-02-11

AI Technical Summary

Technical Problem

The existing ultra-high molecular weight polyethylene injection molding methods have problems such as poor quality of finished products, low production efficiency, high energy consumption and poor product consistency. They are mainly due to oxidation and finished products caused by uneven air inhalation and injection density in the mold cavity. Unstable performance.

Method used

The pressure and temperature in the mold cavity are controlled during mold heating and mold closing process, and the mold cavity is opened by the action of injection pressure, combined with the back pressure control system driven by high-pressure cylinder, to ensure the compactness and consistency of the injection material in the mold cavity and avoid air Enter and maintain appropriate pressure during cooling to stabilize the finished product quality.

Benefits of technology

It improves the quality and performance of finished products, reduces production cycle and energy consumption, ensures product consistency and stable performance, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114619632B_ABST
    Figure CN114619632B_ABST
Patent Text Reader

Abstract

The invention discloses an injection molding method based on ultra-high molecular weight polyethylene, which is characterized by comprising the following steps: closing the mold to form a closed mold cavity; heating the mold so that the temperature of the mold core reaches a predetermined temperature value; injecting injection material into the mold cavity, and when the injection material fills the mold cavity, continuing to inject injection material into the mold cavity, the mold cavity is opened under the action of the injection pressure, driving the movable template of the injection molding machine to retreat to a preset distance position, and after the movable template retreats to a position, the injection mechanism stops working and completes one injection; the mold assembly is closed for the second time to form a compression on the injection material in the mold cavity until the inner cavity thickness of the mold cavity matches the thickness of the product to be manufactured, and the mold is cooled at the same time; opening the mold to obtain the product. The advantage is that products with relatively excellent quality and performance can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an injection molding method, in particular to an injection molding method based on ultra-high molecular weight polyethylene. Background Art

[0002] Ultra-high molecular weight polyethylene is a linear thermoplastic engineering plastic with excellent comprehensive properties. It has excellent wear resistance and anti-adhesion properties, extremely high impact strength and good chemical stability, and is widely used in industrial and civil fields.

[0003] Because ultra-high molecular weight polyethylene has an ultra-high molecular weight (viscosity average molecular weight is more than 1.5 million), the melt viscosity is as high as 108Pa·s, and the melt index is almost zero, which makes it difficult to process and shape ultra-high molecular weight polyethylene. Traditionally, it is mainly formed by compression molding-sintering method, that is, after the mold is loaded and pressurized, the mold and the raw materials are placed in a heating furnace for heating and plasticization, then taken out and cooled, and finally taken out to obtain the product. This traditional molding process mainly has the following problems: first, the raw materials are heated unevenly in the mold, and there may be external melting and unmelted core, resulting in poor quality of the finished product; second, it usually takes several hours to manufacture a product using this method, the production efficiency is relatively low, and the labor intensity of workers is also relatively high; third, the energy consumption is also relatively large.

[0004] Based on this, a Chinese invention patent with publication number CN109228201A discloses an injection molding method, which mainly includes the steps of mold closing, preheating, heating, injection, film pressing cooling and mold opening. Through this method, products with good finished quality can be produced based on ultra-high molecular weight polyethylene, while having high production efficiency and low energy consumption. The above-mentioned molding method has the following disadvantages: First, in step S4, the mold clamping mechanism opens a gap in the mold cavity. In the process of opening the mold cavity, a large amount of air will be sucked in and then continue to be injected into it. At this time, the sucked air is difficult to be discharged outwards well, and there may even be air entrapment, resulting in poor quality of the finished product. At the same time, the injection material molten in a high-temperature state is easily oxidized when it comes into contact with the oxygen in the air sucked into the mold cavity, resulting in poor performance of the finished product. Secondly, this molding method completely relies on the injection position of the injection mechanism to control the filling amount of the mold cavity. Based on the high viscosity and non-flowability of the ultra-high molecular weight polyethylene in the molten state, it exists in a state close to solid elasticity in the injection barrel, with uneven density, and it is impossible to ensure that the injection weight is the same each time. At this time, the consistency of the product will be poor. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide an injection molding method based on ultra-high molecular weight polyethylene, by which products with relatively excellent quality and performance can be produced.

[0006] The technical solution adopted by the present invention to solve the above technical problems is:

[0007] An injection molding method based on ultra-high molecular weight polyethylene comprises the following steps:

[0008] (1) The mold assembly of the injection molding machine is closed for the first time to form a closed mold cavity;

[0009] (2) Heating the mold so that the temperature of the mold core reaches a predetermined temperature value;

[0010] (3) When the temperature of the mold core reaches the preset temperature value, the mold is stopped from being heated. At the same time, the injection mechanism of the injection molding machine injects the plasticized and heat-insulated injection material into the mold cavity. When the injection material fills the mold cavity, the injection mechanism continues to inject the injection material into the mold cavity. The mold cavity is opened under the action of the injection pressure, driving the movable template of the injection molding machine to retreat to a preset distance position. After the movable template retreats to the right position, the injection mechanism stops working and one injection is completed.

[0011] (4) After one injection is completed, the mold assembly is closed for the second time to compress the injection material in the mold cavity until the inner thickness of the mold cavity matches the thickness of the product to be manufactured. At the same time, the mold is cooled. After cooling to the preset temperature, the cooling stops. The injection mechanism stores the material synchronously to prepare for the next injection.

[0012] (5) Opening the mold: opening the mold cavity to obtain the product.

[0013] The predetermined temperature of the mold core in the above step (2) is 90-250° C. The above mold core temperature can effectively prevent the molten injection material from being rapidly cooled after being injected into the mold cavity, thereby effectively ensuring product quality.

[0014] In the above step (3), the mold cavity is controlled to be opened at a speed of 0.1-10 mm / s under the effect of the injection pressure, while maintaining the pressure in the mold cavity at 5-25 MPa. The speed at which the mold cavity is opened and the pressure value in the mold cavity can reduce the entry of external air into the mold cavity, while ensuring the density of the injected injection material, thereby ensuring the quality of the product.

[0015] The thickness of the mold cavity formed by the first mold closing is equal to the thickness of the product to be manufactured, and the thickness of the mold cavity after being opened under the action of the injection pressure is greater than the thickness of the mold cavity formed by the first mold closing.

[0016] The thickness of the mold cavity after being opened under the action of injection pressure is 1.1-2 times the thickness of the product to be manufactured. Based on the specific material characteristics, it is easy to produce products with stable quality and performance.

[0017] In the above step (4), the pressure in the mold cavity is always maintained at 10-30 MPa during the secondary mold closing until the mold is closed. The above pressure value is selected based on the material properties to facilitate the production of products with stable quality and performance.

[0018] The cooling rate in the above step (4) is 1-50°C / min. Based on the material properties and in combination with compression molding, the speed cannot be too fast.

[0019] In the above step (3): during the retreat of the movable template, a back pressure resistance in the opposite direction of the retreat direction is provided to the movable template, and the back pressure resistance cooperates with the injection pressure of the injection mechanism to realize that the mold cavity is opened at a speed of 0.1-10 mm / s, while maintaining the pressure in the mold cavity at 5-25 MPa. The speed at which the mold cavity is opened and the pressure value in the mold cavity can reduce the entry of external air into the mold cavity, while ensuring the density of the injected injection material, thereby ensuring the quality of the product.

[0020] The movable template is driven by a high-pressure oil cylinder, and the high-pressure oil cylinder has a back pressure control system for providing back pressure resistance to control the retreat speed of the movable template and the pressure in the mold cavity when the mold cavity opens during injection. The back pressure control system is used to control the retreat speed of the movable template and the pressure in the mold cavity, so as to achieve stable production and produce products with good consistency.

[0021] The high-pressure oil cylinder comprises a cylinder body and a tie rod with a piston, wherein the piston is movably arranged in the cylinder body to divide the inner cavity of the cylinder body into a rodless cavity and a rod cavity, and one end of the tie rod extends from the rod cavity to be connected with the movable template; when the mold is closed, the movable template is moved by the tie rod, and during injection, the mold cavity is opened under the action of the injection pressure to drive the movable template to retreat, and the movable template moves with the tie rod, and the tie rod provides back pressure resistance to the movable template under the action of the back pressure control system;

[0022] The back pressure control system includes an oil tank, an energy unit and a control unit; the energy unit includes a servo drive, a servo motor and an oil pump; the oil tank supplies oil to the oil pump, the servo motor is driven by the servo drive, and the oil pump is driven by the servo motor; the control unit includes a one-way valve, a relief valve, a first three-position four-way reversing valve, a first cartridge valve, a second two-position four-way reversing valve, a second cartridge valve, a third two-position four-way reversing valve and a proportional pressure regulating valve;

[0023] The oil inlet port of the oil pump is connected to the oil tank, the oil inlet port of the one-way valve is connected to the oil inlet port P of the first reversing valve to form a common oil circuit which is connected to the oil outlet port of the oil pump, the oil outlet port of the one-way valve is connected to the pilot oil inlet port of the first reversing valve, the pilot oil outlet port of the first reversing valve is connected to the oil tank, the oil outlet port of the overflow valve is connected to the oil return port of the first reversing valve to form a common oil circuit which is connected to the oil tank, the working oil port of the first reversing valve is connected to the main oil inlet port of the first cartridge valve, the working oil port of the first reversing valve is connected to the pilot oil inlet port of the overflow valve to form a main oil circuit which is connected to the rodless chamber, the pilot oil outlet port of the first cartridge valve is connected to the working oil port of the second reversing valve, The return oil port of the second reversing valve is connected to the pilot oil inlet port of the first cartridge valve, the pilot oil inlet port of the first cartridge valve is connected to the oil tank, the common oil circuit formed by the oil inlet port of the second reversing valve connected to the main oil outlet port of the first cartridge valve and the main oil inlet port of the second cartridge valve is connected to the rod chamber, the main oil outlet port of the second cartridge valve is connected to the oil tank, the pilot oil outlet port of the second cartridge valve is connected to the working oil port of the third reversing valve, the return oil port of the third reversing valve is connected to the pilot oil outlet port of the proportional pressure regulating valve to form a common oil circuit connected to the oil tank, and the oil inlet port of the third reversing valve is connected to the pilot oil inlet port of the proportional pressure regulating valve. Through the back pressure control system of the above structure, the high-pressure oil cylinder has the effect of returning back pressure, so that the speed of the high-pressure oil cylinder will not be too fast when the injection is passively returned, and the high-pressure oil cylinder can be returned within the adjustable speed range.

[0024] The oil inlet port of the oil pump is connected to the oil tank through an oil filter; the common oil path formed by connecting the oil outlet port of the overflow valve and the oil return port of the first reversing valve is connected to the oil tank through a cooler. The oil filter can filter out the pollutants remaining in the oil tank to protect the oil pump; the cooler is used to cool the hot oil returning to the oil tank from the oil return port. The hot oil is cooled by the cooler and becomes cold oil and enters the oil tank for recycling, thereby effectively controlling the heating of the entire system during operation and ensuring the stable and efficient operation of the entire system.

[0025] The oil inlet port of the oil pump is connected to the first port of the oil filter, and the second port of the oil filter is connected to the oil tank.

[0026] The common oil path formed by connecting the oil outlet port of the overflow valve with the oil return port T of the first reversing valve is connected to the first port of the cooler, and the second port of the cooler is connected to the oil tank.

[0027] The oil tank is provided with a liquid level gauge, which is used to conveniently observe the liquid level in the oil tank so as to replenish the oil in time, thereby ensuring the stable operation of the entire system.

[0028] The oil tank refueling port is provided with an air filter, which can maintain the balance between the pressure in the oil tank and the atmospheric pressure. When the oil tank is refilled, the oil can first pass through the air filter to remove the dirt particles in the oil, so that the oil entering the oil tank is purer, thus protecting the entire system.

[0029] The servo driver is provided with a first pressure sensor and a first pressure gauge, which cooperate with each other to effectively monitor the working pressure of the entire system.

[0030] The oil circuit connected to the main oil circuit oil outlet port of the first cartridge valve is provided with a second pressure gauge and a second pressure sensor. The second pressure sensor and the second pressure gauge cooperate to effectively monitor the working pressure of the rod chamber of the high-pressure oil cylinder.

[0031] Compared with the prior art, the advantages of the present invention are:

[0032] (1) During the entire molding process, mold heating and secondary mold compression are carried out simultaneously during the preheating process of the injection material, which effectively saves the molding cycle and reduces the manufacturing cost;

[0033] (2) This method can be completely pushed out after the injection is completed, with almost no energy consumption, which can effectively reduce the energy consumption of the entire manufacturing equipment, thereby reducing manufacturing costs;

[0034] (3) In this injection molding method, the mold clamping mechanism is opened under the action of the injection pressure generated when the injection mechanism continues to inject the injection material into the mold cavity after filling the mold cavity formed by the first mold clamping. During the entire injection process, the mold cavity is always in a filled state, and it is difficult for external air to enter the mold cavity. Therefore, it can effectively avoid the problem of air entrapment in the product and the problem of oxidation of the injection material after contacting the air, thereby effectively ensuring the quality and performance of the product;

[0035] (4) In the present injection molding method, the mold clamping mechanism is opened under the action of the injection pressure generated when the injection mechanism continues to inject the injection material into the mold cavity after filling the mold cavity formed by the first mold clamping. During the entire injection process, the mold cavity is always in a filled state. Therefore, the amount of injection material for the manufacture of each product is controllable, which can effectively avoid the situation of uneven material density, thereby ensuring the consistency of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a schematic diagram of the structure of the molding equipment used in the first embodiment of the present invention;

[0037] Figure 2 This is a schematic diagram of the structure of the molding equipment used in Example 1 of the present invention. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below with reference to the accompanying drawings.

[0039] Embodiment 1: An injection molding method based on ultra-high molecular weight polyethylene comprises the following steps:

[0040] (1) The mold assembly of the injection molding machine is closed for the first time to form a closed mold cavity;

[0041] (2) Heating the mold so that the temperature of the mold core reaches a predetermined temperature value;

[0042] (3) When the temperature of the mold core reaches the predetermined temperature value, the mold is stopped from being heated. At the same time, the injection mechanism of the injection molding machine injects the plasticized and heat-insulated injection material into the mold cavity. When the injection material fills the mold cavity, the injection mechanism continues to inject the injection material into the mold cavity. The mold cavity is opened under the action of the injection pressure, driving the movable template 3 of the injection molding machine to retreat to a preset distance position. After the movable template 3 retreats to the position, the injection mechanism stops working and one injection is completed;

[0043] (4) After one injection is completed, the mold assembly is closed for the second time to compress the injection material in the mold cavity until the inner thickness of the mold cavity matches the thickness of the product to be manufactured. At the same time, the mold is cooled. After cooling to the preset temperature, the cooling stops. The injection mechanism stores the material synchronously to prepare for the next injection.

[0044] (5) Opening the mold: opening the mold cavity to obtain the product.

[0045] In this specific embodiment, the predetermined temperature of the mold core in the above step (2) is 90-250° C. The above mold core temperature can effectively prevent the molten injection material from being rapidly cooled after being injected into the mold cavity, thereby effectively ensuring product quality.

[0046] In this specific embodiment, in the above step (3), the mold cavity is controlled to be opened at a speed of 0.1-10 mm / s under the effect of the injection pressure, while maintaining the pressure in the mold cavity at 5-25 MPa. The speed at which the mold cavity is opened and the pressure value in the mold cavity can reduce the entry of external air into the mold cavity, while ensuring the density of the injected injection material, thereby ensuring the quality of the product.

[0047] In this specific embodiment, the thickness of the mold cavity formed by the first mold closing is equal to the thickness of the desired product, and the thickness of the mold cavity after being opened under the action of the injection pressure is greater than the thickness of the mold cavity formed by the first mold closing.

[0048] In this specific embodiment, the thickness of the mold cavity after being opened under the effect of the injection pressure is 1.1-2 times the thickness of the desired product to be manufactured. Based on the specific material properties, it is convenient to manufacture products with stable quality and performance.

[0049] In this specific embodiment, in the above step (4), the pressure in the mold cavity is always maintained at 10-30 MPa during the secondary mold closing until the mold is closed. The above pressure value is selected based on the material properties to facilitate the production of products with stable quality and performance.

[0050] In this specific embodiment, the cooling rate in the above step (4) is 1-50°C / min. Based on the material properties and in combination with compression molding, the speed cannot be too fast.

[0051] In this specific embodiment, in the above step (3): during the retreat of the movable template 3, a back pressure resistance in the opposite direction of the retreat direction is provided to the movable template 3, and the back pressure resistance cooperates with the injection pressure of the injection mechanism to realize that the mold cavity is opened at a speed of 0.1-10 mm / s, while maintaining the pressure in the mold cavity at 5-25 MPa. The speed at which the mold cavity is opened and the pressure value in the mold cavity can reduce the entry of external air into the mold cavity, while ensuring the density of the injected injection material, thereby ensuring the quality of the product.

[0052] In this specific embodiment, the movable platen 3 is driven by a high-pressure oil cylinder 4, and the high-pressure oil cylinder 4 has a back pressure control system for providing back pressure resistance to control the retreat speed of the movable platen 3 and the pressure in the mold cavity during the retreat process of the movable platen 3 driven by the mold cavity opening during injection. The back pressure control system is used to control the retreat speed of the movable platen and the pressure in the mold cavity, so as to achieve stable production and produce products with good consistency.

[0053] Embodiment 2: An injection molding method based on ultra-high molecular weight polyethylene comprises the following steps:

[0054] (1) The mold assembly of the injection molding machine is closed for the first time to form a closed mold cavity;

[0055] (2) Heating the mold so that the temperature of the mold core reaches a predetermined temperature value;

[0056] (3) When the temperature of the mold core reaches the predetermined temperature value, the mold is stopped from being heated. At the same time, the injection mechanism of the injection molding machine injects the plasticized and heat-insulated injection material into the mold cavity. When the injection material fills the mold cavity, the injection mechanism continues to inject the injection material into the mold cavity. The mold cavity is opened under the action of the injection pressure, driving the movable template 3 of the injection molding machine to retreat to a preset distance position. After the movable template 3 retreats to the position, the injection mechanism stops working and one injection is completed;

[0057] (4) After one injection is completed, the mold assembly is closed for the second time to compress the injection material in the mold cavity until the inner thickness of the mold cavity matches the thickness of the product to be manufactured. At the same time, the mold is cooled. After cooling to the preset temperature, the cooling stops. The injection mechanism stores the material synchronously to prepare for the next injection.

[0058] (5) Opening the mold: opening the mold cavity to obtain the product.

[0059] In this specific embodiment, the predetermined temperature of the mold core in the above step (2) is 90-250° C. The above mold core temperature can effectively prevent the molten injection material from being rapidly cooled after being injected into the mold cavity, thereby effectively ensuring product quality.

[0060] In this specific embodiment, in the above step (3), the mold cavity is controlled to be opened at a speed of 0.1-10 mm / s under the effect of the injection pressure, while maintaining the pressure in the mold cavity at 5-25 MPa. The speed at which the mold cavity is opened and the pressure value in the mold cavity can reduce the entry of external air into the mold cavity, while ensuring the density of the injected injection material, thereby ensuring the quality of the product.

[0061] In this specific embodiment, the thickness of the mold cavity formed by the first mold closing is equal to the thickness of the desired product, and the thickness of the mold cavity after being opened under the action of the injection pressure is greater than the thickness of the mold cavity formed by the first mold closing.

[0062] In this specific embodiment, the thickness of the mold cavity after being opened under the effect of the injection pressure is 1.1-2 times the thickness of the desired product to be manufactured. Based on the specific material properties, it is convenient to manufacture products with stable quality and performance.

[0063] In this specific embodiment, in the above step (4), the pressure in the mold cavity is always maintained at 10-30 MPa during the secondary mold closing until the mold is closed. The above pressure value is selected based on the material properties to facilitate the production of products with stable quality and performance.

[0064] In this specific embodiment, the cooling rate in the above step (4) is 1-50°C / min. Based on the material properties and in combination with compression molding, the speed cannot be too fast.

[0065] In this specific embodiment, in the above step (3): during the retreat of the movable template 3, a back pressure resistance in the opposite direction of the retreat direction is provided to the movable template 3, and the back pressure resistance cooperates with the injection pressure of the injection mechanism to realize that the mold cavity is opened at a speed of 0.1-10 mm / s, while maintaining the pressure in the mold cavity at 5-25 MPa. The speed at which the mold cavity is opened and the pressure value in the mold cavity can reduce the entry of external air into the mold cavity, while ensuring the density of the injected injection material, thereby ensuring the quality of the product.

[0066] In this specific embodiment, the movable platen 3 is driven by a high-pressure oil cylinder 4, and the high-pressure oil cylinder 4 has a back pressure control system for providing back pressure resistance to control the retreat speed of the movable platen 3 and the pressure in the mold cavity during the retreat process of the movable platen 3 driven by the mold cavity opening during injection. The back pressure control system is used to control the retreat speed of the movable platen and the pressure in the mold cavity, so as to achieve stable production and produce products with good consistency.

[0067] In this specific embodiment, the high-pressure oil cylinder 4 includes a cylinder body 41 and a tie rod 43 with a piston 42. The piston 42 is movably arranged in the cylinder body 41 to divide the inner cavity of the cylinder body 41 into a rodless cavity 44 and a rod cavity 45. One end of the tie rod 43 extends from the rod cavity 45 and is connected to the movable template 3. When the mold is closed, the movable template 3 moves with the tie rod 43. When the mold cavity is opened under the action of the injection pressure during injection and the movable template 3 is driven to retreat, the movable template 3 moves with the tie rod 43. The tie rod 43 provides back pressure resistance to the movable template 3 under the action of the back pressure control system.

[0068] The back pressure control system includes an oil tank C1, an energy unit C2 and a control unit C3; the energy unit C2 includes a servo driver C201, a servo motor C203 and an oil pump C202; the oil tank C1 supplies oil to the oil pump C202, the servo motor C203 is driven by the servo driver C201, and the oil pump C202 is driven by the servo motor C203; the control unit C3 includes a one-way valve C301, a relief valve C302, a first three-position four-way reversing valve C303, a first cartridge valve C304, a second two-position four-way reversing valve C305, a second cartridge valve C306, a third two-position four-way reversing valve C307 and a proportional pressure regulating valve C308;

[0069] The oil inlet port of the oil pump C202 is connected to the oil tank C1, the oil inlet port of the one-way valve C301 is connected to the oil inlet port P of the first reversing valve C303 to form a common oil circuit connected to the oil outlet port of the oil pump C202, the oil outlet port of the one-way valve C301 is connected to the pilot oil inlet port X of the first reversing valve C303, the pilot oil outlet port Y of the first reversing valve C303 is connected to the oil tank C1, and the oil outlet port of the relief valve C302 is connected to the first reversing valve C303. The common oil circuit formed by the oil return port T of the valve C303 is connected to the oil tank C1, the working oil port B of the first reversing valve C303 is connected to the main oil inlet port of the first cartridge valve C304, the working oil port A of the first reversing valve C303 is connected to the pilot oil inlet port of the relief valve C302 to form a main oil circuit connected to the rodless chamber 44, the pilot oil outlet port of the first cartridge valve C304 is connected to the working oil port A of the second reversing valve C305, the oil return port T of the second reversing valve C305 is connected to the pilot oil inlet port Y of the first cartridge valve C304, the pilot oil inlet port Y of the first cartridge valve C304 is connected to the oil tank C1, the common oil circuit formed by the oil inlet port P of the second reversing valve C305 is connected to the main oil circuit outlet port of the first cartridge valve C304, and the common oil circuit formed by the main oil circuit inlet port of the second cartridge valve C306 is connected to the rod chamber 45 , the main oil outlet port of the second cartridge valve C306 is connected to the oil tank C1, the pilot oil outlet port of the second cartridge valve C306 is connected to the working oil port B of the third reversing valve C307, the return oil port T of the third reversing valve C307 is connected to the pilot oil outlet port of the proportional pressure regulating valve C308 to form a common oil circuit connected to the oil tank C1, and the oil inlet port P of the third reversing valve C307 is connected to the pilot oil inlet port of the proportional pressure regulating valve C308. Through the back pressure control system of the above structure, the high pressure oil cylinder 4 has the effect of returning the back pressure, so that the speed of the high pressure oil cylinder 4 will not be too fast when the injection is passively returned, and the high pressure oil cylinder 4 can be returned within the adjustable speed range.

[0070] In this specific embodiment, the oil inlet port of the oil pump C202 is connected to the oil tank C1 through an oil filter C7; the common oil path formed by connecting the oil outlet port of the overflow valve C302 and the oil return port T of the first reversing valve C303 is connected to the oil tank C1 through a cooler C6. The oil filter C7 can filter out the pollutants remaining in the oil tank C1 to protect the oil pump C202; the cooler C6 is used to cool the hot oil returning from the oil return port to the oil tank C1. The hot oil is cooled by the cooler C6 and becomes cold oil and enters the oil tank C1 for recycling, thereby effectively controlling the heating of the entire system during operation and ensuring the stable and efficient operation of the entire system.

[0071] In this specific embodiment, the oil inlet port of the oil pump C202 is connected to the first port of the oil filter C7, and the second port of the oil filter C7 is connected to the oil tank C1.

[0072] In this specific embodiment, the common oil circuit formed by connecting the oil outlet port of the overflow valve C302 and the oil return port T of the first reversing valve C303 is connected to the first port of the cooler C6, and the second port of the cooler C6 is connected to the oil tank C1.

[0073] In this specific embodiment, the oil tank C1 has a liquid level gauge C5. The liquid level gauge C5 is used to conveniently observe the liquid level in the oil tank C1, so as to replenish the oil in the oil tank C1 in time, thereby ensuring the stable operation of the entire system.

[0074] In this specific embodiment, an air filter C8 is provided on the refueling port of the fuel tank C1. The air filter C8 can maintain the balance between the pressure in the fuel tank C1 and the atmospheric pressure. At the same time, when refueling the fuel tank C1, the oil can first pass through the air filter C8 to filter out the dirt particles in the oil, so that the oil entering the fuel tank C1 is purer, thus protecting the entire system.

[0075] In this specific embodiment, the servo driver C201 is provided with a first pressure sensor C9 and a first pressure gauge C10. The first pressure sensor C9 and the first pressure gauge C10 cooperate to effectively monitor the working pressure of the entire system.

[0076] In this specific embodiment, the oil circuit connected to the main oil circuit outlet port of the first cartridge valve C304 is provided with a second pressure gauge C11 and a second pressure sensor C12. The second pressure gauge C11 and the second pressure sensor C12 cooperate to effectively monitor the working pressure of the rod chamber 45 of the high-pressure oil cylinder 4.

[0077] The specific working principle of the above-mentioned back pressure control system is: before work, the linearity of the proportional pressure regulating valve C308 (that is, the corresponding relationship between the input electrical signal and the output pressure) is set in the computer, and then through program control, the output pressure of the proportional pressure regulating valve C308 is equal to the set back pressure when the high-pressure cylinder 4 is released. At this time, the input signal value of the proportional pressure regulating valve C308 can be obtained through linear relationship conversion or manually adjusted. When high pressure starts to be generated, the high-pressure locking electromagnet of the first reversing valve C303 is energized, the second reversing valve C305 is energized, and the servo driver C201 controls the servo motor C203 to rotate. The servo motor C203 drives the oil pump C202 to rotate, and the hydraulic oil flows from the oil tank C1 through the oil filter C7 and is sucked into the oil pump C202, and provides pressure oil to the entire system. The hydraulic oil is pressed into the first reversing valve C303 through the oil outlet port of the oil pump C202 and then continues to be pressed into the first cartridge valve C304. The pilot oil port of the first cartridge valve C304 flows through the second reversing valve C305 and then flows into the oil tank C1. The pilot pressure is relieved, and the pressure oil opens the first cartridge valve C304 and flows into the rod chamber 45 of the high-pressure cylinder 4. The hydraulic oil in the rodless chamber 44 flows back to the oil tank C1 through the return oil port T of the first reversing valve C303. When the high pressure from mold closing ends, the energy unit C2 stops working, the servo motor C203 and the oil pump C202 do not run, the third reversing valve C307 is energized, the high pressure locking electromagnet of the first reversing valve C303 is still energized, the second reversing valve C305 is de-energized and returns to its position, and the injection work begins. Due to the injection pressure acting on the mold, the material in the mold expands and squeezes during the injection process, pushing the mold and the movable template 3 to move slowly backward, driving the pull rod 43 to move slowly backward, so that the hydraulic oil in the rod chamber 45 of the high-pressure oil cylinder 4 is pressed out of the rod chamber 45. At this time, the return oil of the rod chamber 45 of the high-pressure oil cylinder 4 flows to the third reversing valve C307 through the pilot control oil port of the second cartridge valve C306, and then flows into the proportional pressure regulating valve C308. When the return oil pressure slowly increases to the system set pressure of the proportional pressure regulating valve C308, the pressure oil first opens the pilot oil circuit of the proportional pressure regulating valve C308 and returns to the oil tank C1. At this time, the pilot oil pressure of the second cartridge valve C306 reaches the maximum value. As the material in the mold continues to expand, squeeze and push the mold, the main circuit pressure continues to increase, which will open the main oil circuit of the second cartridge valve C306 and flow back to the oil tank C1, thereby playing the role of the back pressure of the high-pressure cylinder 4 return. Because of the back pressure, the speed of the high-pressure cylinder 4 will not be too fast when the injection is passively returned, and the high-pressure cylinder 4 returns within the adjustable speed range.

Claims

1. An injection molding method based on ultra-high molecular weight polyethylene, characterized in that The steps include: (1) The mold assembly of the injection molding machine is closed for the first time to form a closed mold cavity; (2) heating the mold so that the temperature of the mold core reaches a predetermined temperature value; (3) When the temperature of the mold core reaches the predetermined temperature value, the mold is stopped from being heated. At the same time, the injection mechanism of the injection molding machine injects the plasticized and heat-insulated injection material into the mold cavity. When the injection material fills the mold cavity, the injection mechanism continues to inject the injection material into the mold cavity. The mold cavity is opened under the action of the injection pressure, driving the movable template of the injection molding machine to retreat to a preset distance position. After the movable template retreats to the position, the injection mechanism stops working and one injection is completed. (4) After the first injection is completed, the mold assembly is closed for the second time to compress the injection material in the mold cavity until the inner thickness of the mold cavity matches the thickness of the product to be manufactured. At the same time, the mold is cooled. After cooling to a preset temperature, the cooling is stopped. The injection mechanism stores the material synchronously to prepare for the next injection. (5) Opening the mold to open the mold cavity and obtain the product; In the above step (3), the mold cavity is controlled to be opened at a speed of 0.1-10 mm / s under the action of the injection pressure, while maintaining the pressure in the mold cavity at 5-25 MPa; In the above step (3): during the retreat of the movable template, a back pressure resistance in the opposite direction of the retreat direction is provided to the movable template, and the back pressure resistance cooperates with the injection pressure of the injection mechanism to realize that the mold cavity is opened at a speed of 0.1-10 mm / s, while maintaining the pressure in the mold cavity at 5-25 MPa; The movable template is driven by a high-pressure oil cylinder, and the high-pressure oil cylinder has a back pressure control system for providing back pressure resistance to control the retreat speed of the movable template and the pressure in the mold cavity during the process of the mold cavity opening and driving the movable template to retreat during injection; The high-pressure oil cylinder comprises a cylinder body and a pull rod with a piston, wherein the piston is movably arranged in the cylinder body to divide the inner cavity of the cylinder body into a rodless cavity and a rod cavity, and one end of the pull rod extends from the rod cavity to be connected with the movable template; The back pressure control system includes an oil tank, an energy unit and a control unit; the energy unit includes a servo drive, a servo motor and an oil pump; the oil tank supplies oil to the oil pump, the servo motor is driven by the servo drive, and the oil pump is driven by the servo motor; the control unit includes a one-way valve, a relief valve, a first three-position four-way reversing valve, a first cartridge valve, a second two-position four-way reversing valve, a second cartridge valve, a third two-position four-way reversing valve and a proportional pressure regulating valve; The oil inlet port of the oil pump is connected to the oil tank, the oil inlet port of the one-way valve is connected to the oil inlet port P of the first reversing valve to form a common oil circuit which is connected to the oil outlet port of the oil pump, the oil outlet port of the one-way valve is connected to the pilot oil inlet port of the first reversing valve, the pilot oil outlet port of the first reversing valve is connected to the oil tank, the oil outlet port of the overflow valve is connected to the oil return port of the first reversing valve to form a common oil circuit which is connected to the oil tank, the working oil port of the first reversing valve is connected to the main oil inlet port of the first cartridge valve, the working oil port of the first reversing valve is connected to the pilot oil inlet port of the overflow valve to form a main oil circuit which is connected to the rodless chamber, the pilot oil outlet port of the first cartridge valve is connected to the working oil port of the second reversing valve, The oil return port of the second reversing valve is connected to the pilot oil inlet port of the first cartridge valve, the pilot oil inlet port of the first cartridge valve is connected to the oil tank, the oil inlet port of the second reversing valve is connected to the main oil circuit oil outlet port of the first cartridge valve to form a common oil circuit connected to the main oil circuit oil inlet port of the second cartridge valve, and the common oil circuit formed is connected to the rod chamber, the main oil circuit oil outlet port of the second cartridge valve is connected to the oil tank, the pilot oil outlet port of the second cartridge valve is connected to the working oil port of the third reversing valve, the oil return port of the third reversing valve is connected to the pilot oil outlet port of the proportional pressure regulating valve to form a common oil circuit connected to the oil tank, and the oil inlet port of the third reversing valve is connected to the pilot oil inlet port of the proportional pressure regulating valve.

2. The injection molding method based on ultra-high molecular weight polyethylene according to claim 1, characterized in that The predetermined temperature of the mold core in the above step (2) is 90-250°C.

3. The injection molding method based on ultra-high molecular weight polyethylene according to claim 1, characterized in that The thickness of the mold cavity formed by the first mold closing is equal to the thickness of the product to be manufactured, and the thickness of the mold cavity after being opened under the action of the injection pressure is greater than the thickness of the mold cavity formed by the first mold closing.

4. The injection molding method based on ultra-high molecular weight polyethylene as claimed in claim 3, characterized in that The thickness of the mold cavity after being opened under the action of the injection pressure is 1.1-2 times the thickness of the product to be manufactured.

5. The injection molding method based on ultra-high molecular weight polyethylene according to claim 1, characterized in that In the above step (4), the pressure in the mold cavity is always maintained at 10-30 MPa during the secondary mold closing until the mold is in place.

6. The injection molding method based on ultra-high molecular weight polyethylene according to claim 1, characterized in that The oil inlet port of the oil pump is connected to the oil tank through an oil filter; the common oil circuit formed by connecting the oil outlet port of the overflow valve and the oil return port of the first reversing valve is connected to the oil tank through a cooler.