An in-situ preparation-testing integrated device and method for metal nanowire materials
The integrated device and method for in-situ preparation and testing of metal nanowires under a transmission electron microscope addresses the challenges of conventional TEM sample preparation by enabling real-time observation and control of growth position and state, achieving high-success-rate preparation of nanostructures with different grain boundaries and immediate in-situ testing.
Patent Information
- Application Number
- CN202210279575.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-21
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-03-21
AI Technical Summary
Conventional TEM sample preparation for metal nanowires is time-consuming, hazardous, and alters the original material characteristics, making it difficult to directly observe and control the growth position and state during preparation, and perform in-situ testing.
An integrated device and method using a transmission electron microscope, mechanical-electrical single-tilt sample rod, and CCD camera for in-situ preparation and testing of metal nanowires, enabling real-time observation and control of growth position and state, and preparation of nanostructures with different grain boundaries.
Enables high-success-rate preparation of nano-twin or polycrystalline metal nanowires with different grain boundaries, allowing immediate in-situ testing without sample oxidation or damage, suitable for various metals like gold and tungsten.
Smart Images

Figure CN114636698B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nano material preparation and testing, and in particular to an in-situ preparation-testing integrated device and method for metal nanowire materials under a transmission electron microscope. Background Art
[0002] Knoll and Ruska first mentioned the electron microscope in their paper in 1932, and realized the idea of electron lens imaging, thus turning the concept of electron lens into reality. The world's first commercial transmission electron microscope (TEM) was built in the UK four years later, in 1936. TEM uses a parallel high-energy electron beam to penetrate the sample, and focuses the image on the other side through an electromagnetic lens, and finally enlarges it step by step on the fluorescent screen. Through the objective lens behind the sample, the transmitted electron beam and the elastic scattered electron beam are focused on the image plane to obtain a TEM bright field image with diffraction contrast, and a diffraction pattern can be obtained on the back focal plane of the objective lens; by selecting a specific diffracted electron beam, a dark field image can be obtained; by using the phase interference between the diffracted electron beam and the transmitted electron beam for imaging, a high-resolution image can be obtained. With the continuous advancement of TEM-related technologies, TEM has become the most effective and most commonly used tool for material characterization, and the scale range of research includes atoms, nanometers, and micrometers or larger.
[0003] TEM has many advantages, but it is also accompanied by corresponding disadvantages. The most tedious of these is the preparation of TEM samples, but this is also one of the factors that most directly affect TEM observation results. Due to the principle of TEM imaging, enough electrons need to penetrate the sample, so the TEM sample must be thin enough (conventional experiments require the sample thickness to be around 100nm, and in more extreme cases the thickness is required to be less than 50nm, or even less than 10nm); and because TEM imaging is a high-resolution imaging technology, only a very small part of the sample can be observed each time, so the surface area of the prepared sample needs to be small enough.
[0004] The conventional TEM sample preparation and testing process, while ensuring the safety of instruments and personnel, takes a lot of time, starting from cutting thin slices from large samples, then cutting them into round slices, and finally obtaining TEM samples after drilling, pre-thinning, electrolytic polishing, ion thinning and other steps. This process will encounter dangerous chemicals, ion radiation or other risks that may cause harm to the human body, and the original morphology, structure and composition of the material will be changed and affected to a certain extent during the manufacturing process. It cannot be guaranteed that the original characteristics of the sample material can be fully reflected in the subsequent TEM observation and testing. This is especially obvious for metal nanowire materials. Therefore, a new integrated preparation-testing technology for metal nanowire materials is urgently needed. Summary of the invention
[0005] In order to solve the problems existing in the background technology, the present invention proposes an in-situ preparation-testing integrated device and method for metal nanowire materials, which can directly observe the growth position and state of the nanostructure on the metal nanowire during preparation, and the preparation method can prepare twin or polycrystalline nanostructures containing different small-angle grain boundaries, large-angle grain boundaries or twin boundaries on the nanowire with a high success rate. The problem that the growth position and state cannot be directly observed and controlled during preparation, and the in-situ test cannot be carried out in time after the preparation is completed in the prior art is solved.
[0006] The technical solution adopted by the present invention is as follows:
[0007] 1. An integrated device for in-situ preparation and testing of metal nanowire materials
[0008] The invention comprises a transmission electron microscope, a mechanical-electrical single-tilt sample rod, a sample rod control box and a CCD camera; the mechanical-electrical single-tilt sample rod comprises a non-movable platform and a movable end of a metal cap, the non-movable platform and the movable end of the metal cap are arranged opposite to each other and do not contact each other, and a nano-fracture segment and a probe are fixed on the non-movable platform and the movable end of the metal cap respectively; the sample rod control box comprises a piezoelectric ceramic drive displacement system and an electrical control system, and the non-movable platform and the movable end of the metal cap are both connected to the piezoelectric ceramic drive displacement system and the electrical control system; the mechanical-electrical single-tilt sample rod is placed in the transmission electron microscope, and the relative position and movement of the nano-fracture segment and the probe on the mechanical-electrical single-tilt sample rod are observed through the transmission electron microscope; the piezoelectric ceramic drive displacement system controls the movement of the probe through the movable end of the metal cap, and performs in-situ testing on the prepared metal nanowire sample; the CCD camera is used to record the atomic-scale structural evolution of the metal nanowire in real time during the in-situ testing process.
[0009] The nano-fracture section and the probe are made of the same metal material, specifically tungsten, gold or molybdenum.
[0010] The nano-fracture segment is prepared by a physical shearing method: the metal wire is flattened with flat-head pliers, and then the flattened part is cut transversely with wire cutters. The sheared surface at the front end is a relatively straight fracture, and a large number of nano-scale tips are formed on the straight fracture. The root of the nano-fracture segment is fixed on a non-movable platform, and the sheared surface at the front end faces the probe.
[0011] The probe is obtained by obliquely cutting off the front end of the metal wire, and a needle tip is formed at the front end after cutting; the root of the probe is fixed on the movable end of the metal cap, and the tip of the probe needle faces the nano fracture section.
[0012] 2. In-situ preparation-testing integrated method using the above device
[0013] The following steps are involved:
[0014] 1) In-situ sample cleaning: The nano-fracture section and the probe are loaded on the mechanical-electrical single-tilt sample holder, and the loaded mechanical-electrical single-tilt sample holder is placed in an Ar plasma cleaner for cleaning to remove contaminants attached to the fracture;
[0015] 2) Place the mechanical-electrical single-tilt sample rod into a transmission electron microscope, and roughly adjust the position of the probe in the sample chamber of the transmission electron microscope so that the probe and the nanofracture segment are horizontally aligned and close to each other, and the distance between the two ends is controlled within 1 mm;
[0016] 3) In-situ preparation of metal nanowires: Select two nanotips with good orientation and clear imaging on the nanofracture segment and the probe respectively, and drive the probe to gradually approach the designated nanotips on the nanofracture segment through the piezoelectric ceramic-driven displacement control system. At the same time, pre-apply voltage to both ends of the mechanical-electrical single-tilt sample rod, and fine-tune the direction of the probe so that the tip of the probe is at the same height as the designated nanotips on the nanofracture segment. Finally, make the tips of the probe and the nanofracture segment contact each other to form a closed loop, and use high-density instantaneous current to weld the sample metal nanowires;
[0017] 4) After the sample is prepared, in-situ nanomechanical testing is performed: the probe is controlled to apply a tensile / compressive load along the probe axis or a shear load perpendicular to the probe direction, or a cyclic load, to the sample metal nanowire.
[0018] 5) During the load application process, a CCD (high-resolution charge-coupled device) camera is used to record the atomic-scale structural evolution of the metal nanowires in real time. The real-time imaging information of the CCD camera is synchronously recorded using the corresponding screen recording software to complete the in-situ test.
[0019] In step 3), two nano tips with different orientation differences are selected on the probe and the nano fracture segment to prepare metal nanowires with different grain boundaries. Different orientation differences mean that the two tips have different crystal directions.
[0020] The metal nanowires obtained in step 3) are nano-twinned or polycrystalline in structure and contain different small-angle grain boundaries, large-angle grain boundaries or twin grain boundaries.
[0021] In the step 3), a voltage of -2 to 2 V is applied to both ends of the mechanical-electrical single-tilt sample rod through an electrical control system.
[0022] During the load application process of step 4), the tension / compression or shear strain rate is controlled at 10 -3 s -1 Order of magnitude, realizing quasi-static loading experiment.
[0023] In the step 4), the tensile / compressive load is applied by moving the probe along the axial direction of the probe, and the shear load is applied by moving the probe along the vertical direction of the probe. The cyclic load is the cyclic application of the tensile / compressive load or the shear load.
[0024] The beneficial effects of the present invention are:
[0025] 1. The present invention can in-situ observe and control the growth position and direction of metal nanowires.
[0026] 2. The preparation success rate of the present invention is high, and the metal nanowires are not easy to fall off or wear.
[0027] 3. The metal nanowires prepared by the present invention include nano-twin or polycrystalline structures with different small-angle grain boundaries, large-angle grain boundaries or twin boundaries.
[0028] 4. The present invention can immediately perform in-situ testing on the prepared metal nanowires, thus avoiding problems such as sample oxidation and sample damage due to improper transportation or storage during the conventional sample manufacturing and testing process.
[0029] 5. The present invention has a wide range of applications and is suitable for various metal materials such as gold, tungsten, and molybdenum. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic diagram of the device of the present invention.
[0031] Figure 2 This is a physical picture of the nanofracture section and the probe.
[0032] Figure 3 is a transmission electron microscope group of images of the metal nanowire preparation process after the probe is aligned with the designated nanotip on the nanofracture segment in Example 1;
[0033] Among them: (a) is the transmission electron microscope image of the nanofracture segment and the probe before preparation;
[0034] (b) is a transmission electron microscope image of the probe approaching the nanotip at the fixed end under the drive of the piezoelectric ceramic after pre-biasing;
[0035] (c) is a transmission electron microscope image of metal nanowires prepared by welding.
[0036] Figure 4 is a transmission electron microscope group picture of the in-situ tensile test process after the metal nanowires are prepared in Example 1;
[0037] Wherein: (a) is a transmission electron microscope image of the prepared metal nanowires;
[0038] (b) (c) are TEM images of the probe applying a tensile load along the axial displacement of the probe;
[0039] (d) is a transmission electron microscope image of the metal nanowires after in-situ tensile testing.
[0040] Figure 5 is a transmission electron microscope group picture of the in-situ shear test process after the metal nanowires are prepared in Example 2;
[0041] Wherein: (a) is a transmission electron microscope image of the prepared metal nanowires;
[0042] (b) (c) are TEM images of the probe applying shear load along the axis perpendicular to the probe axial displacement;
[0043] (d) is a transmission electron microscope image of the metal nanowires completing the in-situ shear test.
[0044] Figure 6 It is a schematic diagram of the process of preparing metal nanowires with nano twin crystal or polycrystalline structure after the nano fracture segment and the probe are fixed on the immovable platform and the movable end of the metal cap respectively, and the piezoelectric ceramic drive control system and the electrical control system are connected;
[0045] (a) is a schematic diagram of the pre-biased nanofracture segment and probe before the preparation begins;
[0046] (b) is a schematic diagram of the probe approaching the nanotip at the fixed end through the piezoelectric ceramic drive;
[0047] (c) is a schematic diagram of the completed metal nanowire preparation.
[0048] Figure 7 It is a schematic diagram of in-situ testing of the prepared metal nanowires after the nanoport end and the probe are fixed on the immovable platform and the movable end of the metal cap respectively, and the piezoelectric ceramic drive control system and the electrical control system are connected;
[0049] (a) is a schematic diagram of the prepared metal nanowires;
[0050] (b) is a schematic diagram of controlling the displacement of the probe to apply a compressive load along the axial direction of the probe;
[0051] (c) is a schematic diagram of controlling the probe displacement to apply a tensile load along the probe axis;
[0052] (d) is a schematic diagram of controlling the probe displacement to apply a shear load perpendicular to the probe axis.
[0053] In the figure: 1. Nanofracture segment; 2. Probe; 3. Immovable platform; 4. Movable end of metal cap; 5. Piezoelectric ceramic driven displacement control system; 6. Electrical control system; 7. Metal nanowire. DETAILED DESCRIPTION
[0054] The present invention is further described in detail below in conjunction with the accompanying drawings, but the present invention is not limited to the following embodiments.
[0055] like Figure 1 As shown, the instruments used for the preparation include a transmission electron microscope, a mechanical-electrical single-tilt sample rod, a sample rod control box and a CCD camera. The transmission electron microscope is used to record and observe the relative position and movement of the nanofracture segment 1 and the probe 2 on the mechanical-electrical single-tilt sample rod; the sample rod control box is mainly used to control the displacement of the probe 2 and perform in-situ testing on the prepared metal nanowire samples; the CCD camera is mainly used to record the atomic-scale structural evolution of the sample in real time during the in-situ testing process.
[0056] The mechanical-electrical single-tilt sample holder includes a non-movable platform 3 and a metal cap movable end 4. The non-movable platform 3 and the metal cap movable end 4 are arranged opposite to each other and do not touch each other. The nano-fracture segment 1 and the probe 2 are fixed on the non-movable platform 3 and the metal cap movable end 4 respectively; the nano-fracture segment 1 and the probe 2 are connected to the piezoelectric ceramic drive displacement system 5 and the electrical control system 6. In the experiment, the movable end is driven to achieve precise control in the up-down, left-right, front-back and three-dimensional directions and apply voltage. In addition, a constant bias voltage can be applied to both ends of the sample at the same time.
[0057] The integrated preparation-testing process includes the following steps:
[0058] 1) The nano-fracture segment 1 is prepared by a physical shearing method using a metal wire. A metal wire with a diameter of about 0.25 mm is flattened with a flat-head pliers, and then the flattened part is cut transversely with a wire cutter to obtain a relatively straight fracture, forming a large number of nano-scale tips at the fracture, and then the root of the nano-fracture segment 1 is fixed on a non-movable platform 3; the front tip of the probe 2 is obtained by obliquely cutting the metal wire, and the root of the probe 2 is fixed on the movable end 4 of the metal cap, and the tip of the probe 2 faces the nano-fracture segment 1;
[0059] 2) In-situ sample cleaning: Place the loaded mechanical-electrical single-tilt sample rod in an Ar plasma cleaner for about 1 minute to remove contaminants that may be attached to the nano-tips at the fracture surface;
[0060] 3) placing the mechanical-electrical sample single tilt rod into a transmission electron microscope, aligning the probe 2 and the nanofracture segment 1 horizontally in the sample chamber of the transmission electron microscope and bringing them close together, with the distance between the two ends controlled within 1 mm but not touching;
[0061] 4) In-situ preparation of metal nanowires: Select two nanotips with good orientation and clear imaging on the nanofracture segment 1 and probe 2 respectively, drive probe 2 to gradually approach the designated nanotips of nanofracture segment 1 through piezoelectric ceramics, and pre-apply -2~2V voltage to both ends of the mechanical-electrical single-tilt sample rod, fine-tune the direction of probe 2 to ensure that the nanotips on both sides are at the same height, and finally make the tips on both sides contact each other to form a closed loop, and use high-density instantaneous current to weld metal nanowires;
[0062] Regarding step 4): by selecting two nanotips with different orientation differences on the nanofracture segment 1 and the probe 2, metal nanowires containing different grain boundaries can be prepared.
[0063] 5) After the sample is prepared, in-situ nanomechanical testing can be performed. The software controls the displacement of the probe along the axial direction or perpendicular direction of the probe, thereby applying a tensile / compressive load along the axial direction of the probe or a shear load perpendicular to the probe direction, as well as a corresponding cyclic load, to the sample;
[0064] 7) During the loading process, a high-resolution CCD camera is used to record the atomic-scale structural evolution of the metal nanowires in real time. The real-time imaging information of the CCD camera is synchronously recorded using the corresponding screen recording software to complete the in-situ test.
[0065] like Figure 6 As shown, after the nano-fracture segment 1 and the probe 2 are respectively fixed on the immovable platform 3 and the movable end 4 of the metal cap, and the piezoelectric ceramic drive control system 5 and the electrical control system 6 are connected, the pre-applied -2 to 2V voltage forms a closed loop because the nano-tips are in contact with each other, and the high-density instantaneous current can weld a metal nanowire 7 with a nano-twin structure.
[0066] like Figure 7 As shown, after the nanoport end 1 and the probe 2 are respectively fixed on the immovable platform 3 and the movable end 4 of the metal cap, and the piezoelectric ceramic drive control system 5 and the electrical control system 6 are connected, the probe displacement is controlled by software to apply a compression / tensile load along the axial direction of the probe or a shear load perpendicular to the axial direction of the probe and a corresponding cyclic load.
[0067] According to the different orientation differences between the nanotips on both sides, the prepared metal nanowires can contain nanotwins or polycrystalline structures with different small-angle grain boundaries, large-angle grain boundaries or twin boundaries. Adjust the displacement step to control the tension / compression or shear strain rate to 10 -3 s -1During the loading process, a high-resolution CCD camera is used to record the atomic-scale structural evolution of metal nanowires in real time. The image acquisition frequency is one image every 3 seconds. The corresponding screen recording software is used to synchronously record the real-time imaging information of the CCD camera to achieve the effect of in-situ testing.
[0068] Embodiment 1:
[0069] like Figure 3 and Figure 4 shown.
[0070] Step 1) Sample cleaning
[0071] The purchased high-purity 0.25 mm diameter gold (Au) wire was cut into small segments with a length of about 2 cm, immersed in anhydrous ethanol, and ultrasonically cleaned for about 20 minutes to remove residual stains on the sample surface during manufacturing, transportation and storage.
[0072] Step 2) Preparation of gold wire nanofracture segments and nanotip probes
[0073] The physical shearing method was used to prepare the nano-fracture segment, that is, the end of the gold wire was flattened with flat-head pliers, and then cut off with wire cutters as the nano-fracture segment, and the nano-fracture segment was fixed on a fixed platform and the fixing screws were tightened. Care was taken to avoid bumping at the fracture during the preparation process to ensure that the obtained nano-tip was intact; another section of gold wire was taken, and a needle tip was obtained by oblique cutting, which was used as a nano-tip probe. The root of the probe was fixed on the movable end of the metal cap, and the tip of the probe was facing the nano-fracture segment. The movable needle tip was kept aligned with the nano-fracture segment, and the distance between the two ends was controlled within 1 mm as much as possible.
[0074] Step 3) In-situ sample cleaning
[0075] The loaded sample rod was placed in an Ar plasma cleaner for about 1 minute to remove contaminants that may be attached to the nanotip at the fracture end, and to ensure that there were no contaminants at the fracture end of the sample as much as possible.
[0076] Step 4) In situ preparation of gold nanowires
[0077] The electro-mechanical single-tilt sample rod containing the gold wire sample is placed in the sample chamber of the transmission electron microscope. Two nanotips with good orientation and clear atomic images are selected. The piezoelectric ceramics are used to drive the probes to approach the nanofracture segment. At the same time, a 1.2V voltage is pre-applied and the vertical position of the probe end is fine-tuned to ensure that the nanotips on both sides are at the same height. Finally, a closed loop is formed at the two tips, and the gold nanowires are welded using high-density instantaneous current.
[0078] According to the different orientation differences between the nanofracture segment and the nanotip welded with the probe, nanotwin or polycrystalline gold nanowires containing different small-angle grain boundaries, large-angle grain boundaries or twin boundaries can be prepared.
[0079] Step 5) In-situ testing of gold nanowires
[0080] After the sample is prepared, in-situ nanomechanical testing can be performed. The software controls the displacement of the probe in the axial direction to apply a tensile load to the sample. The displacement step length and tensile strain rate are controlled at 10 -3 s -1 During the loading process, a high-resolution CCD camera was used to record the atomic-scale structural evolution of the gold nanowires in real time, with an image acquisition frequency of 3 images per second. The screen recording software was used to synchronously record the real-time imaging information of the CCD camera to complete the in-situ test.
[0081] Embodiment 2:
[0082] The difference from Example 1 is that in step 5), the probe is controlled to move in the vertical direction to apply a shear load to the prepared gold nanowires. The rest of the implementation process is the same as Example 1. The atomic-scale structural evolution of the gold nanowires has changed significantly compared to when a tensile load is applied. Figure 5 and Figure 7 (d) as shown.
Claims
1. An integrated device for in-situ preparation and testing of metal nanowire materials, characterized in that: It includes a transmission electron microscope, a mechanical-electrical single-tilt sample holder, a sample holder control box and a CCD camera; The mechanical-electrical single-tilt sample rod comprises a non-movable platform (3) and a metal cap movable end (4), the non-movable platform (3) and the metal cap movable end (4) are arranged facing each other and not in contact, and the nano-fracture segment (1) and the probe (2) are fixed on the non-movable platform (3) and the metal cap movable end (4) respectively; The sample rod control box includes a piezoelectric ceramic drive displacement system (5) and an electrical control system (6), and the immovable platform (3) and the movable end of the metal cap (4) are both connected to the piezoelectric ceramic drive displacement system (5) and the electrical control system (6); The mechanical-electrical single-tilt sample rod is placed in a transmission electron microscope, and the relative position and movement of the nano-fracture segment (1) and the probe (2) on the mechanical-electrical single-tilt sample rod are observed through the transmission electron microscope; the piezoelectric ceramic driven displacement system (5) controls the movement of the probe (2) through the movable end (4) of the metal cap to perform in-situ testing on the prepared metal nanowire sample; the CCD camera is used to record the atomic-scale structural evolution of the metal nanowire in real time during the in-situ testing process; The device adopts an in-situ preparation-testing integrated method, which includes the following steps: 1) In-situ sample cleaning: The nano-fracture section (1) and the probe (2) are respectively loaded on the mechanical-electrical single-tilt sample rod, and the loaded mechanical-electrical single-tilt sample rod is placed in an Ar plasma cleaning instrument for cleaning to remove contaminants attached to the fracture; 2) placing the mechanical-electrical single-tilt sample rod into a transmission electron microscope, and roughly adjusting the position of the probe (2) in the sample chamber of the transmission electron microscope so that the probe (2) and the nanofracture segment (1) are horizontally aligned and close to each other, and the distance between the two ends is controlled within 1 mm; 3) In-situ preparation of metal nanowires: two nanotips with clear images are selected on the nanofracture segment (1) and the probe respectively, and the probe (2) is driven by a piezoelectric ceramic drive displacement control system to gradually approach the designated nanotip of the nanofracture segment (1). At the same time, voltage is pre-applied to both ends of the mechanical-electrical single-tilt sample rod, and the direction of the probe (2) is finely adjusted so that the tip of the probe (2) and the designated nanotip on the nanofracture segment (1) are at the same height. Finally, the tips of the probe (2) and the nanofracture segment (1) are brought into contact with each other to form a closed loop, and the sample metal nanowires are welded using a high-density instantaneous current; 4) After the sample is prepared, an in-situ nanomechanical test is performed: the control probe (2) applies a tensile / compressive load along the probe axis or a shear load perpendicular to the probe direction, or a cyclic load to the sample metal nanowire. 5) During the load application process, a CCD camera is used to record the atomic-scale structural evolution of metal nanowires in real time to complete in-situ testing.
2. The in-situ preparation and testing integrated device of metal nanowire material according to claim 1, characterized in that: The nano-fracture section (1) and the probe (2) are made of the same metal material, specifically tungsten, gold or molybdenum.
3. The in-situ preparation and testing integrated device of metal nanowire material according to claim 1, characterized in that: The nano-fracture segment (1) is prepared by a physical shearing method: a metal wire is flattened with flat-head pliers, and then the flattened portion is cut transversely with wire cutters, so that the front end of the sheared surface is a straight fracture surface, and a large number of nano-scale tips are formed on the straight fracture surface. The root of the nano-fracture segment (1) is fixed on a non-movable platform (3), and the front end of the sheared surface faces the probe (2).
4. The in-situ preparation and testing integrated device of metal nanowire material according to claim 1, characterized in that: The probe (2) is obtained by obliquely cutting off the front end of a metal wire, and after cutting, the front end forms a needle tip; the root of the probe (2) is fixed to the movable end (4) of the metal cap, and the tip of the probe (2) faces the nano fracture section (1).
5. The in-situ preparation and testing integrated device of metal nanowire material according to claim 1, characterized in that: In the step 3), two nanotips with different orientation differences are selected on the probe (2) and the nanofracture segment (1), so as to prepare metal nanowires with different grain boundaries.
6. The in-situ preparation and testing integrated device of metal nanowire material according to claim 1, characterized in that: The metal nanowires obtained in step 3) are nano-twinned or polycrystalline in structure and contain different small-angle grain boundaries, large-angle grain boundaries or twin grain boundaries.
7. The in-situ preparation and testing integrated device of metal nanowire material according to claim 1, characterized in that: In the step 3), a voltage of -2 to 2 V is applied to both ends of the mechanical-electrical single-tilt sample rod through an electrical control system (6).
8. The in-situ preparation and testing integrated device of metal nanowire material according to claim 1, characterized in that: During the load application process of step 4), the tension / compression or shear strain rate is controlled at 10 -3 s -1 Order of magnitude, realizing quasi-static loading experiment.
9. The in-situ preparation and testing integrated device of metal nanowire material according to claim 1, characterized in that: In the step 4), the tensile / compressive load is applied by moving the probe along the axial direction of the probe, and the shear load is applied by moving the probe along the vertical direction of the probe. The cyclic load is the cyclic application of the tensile / compressive load or the shear load.
Citation Information
Patent Citations
Method and device for preparing superfine atomic force microscope metal probe
CN110658360A
Mechanical thinning preparation device and method for substrate-free monatomic layer metal film
CN114113156A
Double-tilt in-situ mechanical sample holder for TEM based on piezoelectric ceramic drive
US20170301511A1
A double-tilt in-situ nanoindentation platform for transmission electron microscope
US20180053625A1