A chemically pre-lithiated micron-sized silicon, its preparation method and application

Through the chemical prelithiation of micron silicon method, active lithium is embedded to solve the problem of volume changes in micron silicon and repeated growth of SEI films in lithium-ion batteries, improving the first Coulomb efficiency and battery performance of lithium-ion batteries.

CN114649507BActive Publication Date: 2024-11-26SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210238451.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-10
Publication Date
2024-11-26
Estimated Expiration
2042-03-10

AI Technical Summary

Technical Problem

The process of intercalation of lithium and deliquefaction in the negative electrode of a micron silicon in the lithium-ion battery leads to volume changes, crushing and repeated growth of SEI films, resulting in low Coulomb efficiency, especially the first time Coulomb efficiency is poor.

Method used

Using chemical prelithiated micron silicon method, by soaking the micron silicon electrode sheet in 4,4'-dimethylbiphenyl lithium solution, embedded in active lithium to form LixSi, thereby compensating for the loss of lithium ions during charging and discharging. Avoid volume changes and SEI membrane growth.

Benefits of technology

It improves the first Coulomb efficiency of the silicon negative electrode, reduces the charge and discharge loss capacity, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114649507B_ABST
    Figure CN114649507B_ABST
Patent Text Reader

Abstract

The present invention relates to a chemical pre-lithiation micron silicon and a preparation method and application thereof. The method comprises: 1) coating a slurry on a copper foil, and vacuum drying the coated copper foil to obtain a micron silicon pole piece; the slurry comprises micron silicon, a binder, and carbon black; 2) adding the dried micron silicon pole piece to a pre-lithiation solution for immersion, and then rinsing to obtain a chemical pre-lithiation micron silicon lithium ion battery negative electrode; the pre-lithiation solution is a 4,4'-dimethylbiphenyl lithium solution. Pre-lithiation can be used to compensate for the loss of active lithium during the charge and discharge process. The first coulomb efficiency of the silicon negative electrode is improved; and the loss capacity of the silicon negative electrode during the first charge and discharge is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion battery negative electrodes, and in particular relates to chemical pre-lithiation micron silicon and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Micron silicon is considered to be the lithium-ion battery negative electrode with the most commercial potential. However, the lithium insertion and delithiation process of the micron silicon negative electrode will produce huge volume changes, which will break the active material. The SEI film between the silicon-based negative electrode and the electrolyte will grow repeatedly, consuming a large amount of electrolyte and active lithium ions. Therefore, the coulombic efficiency of the silicon-based negative electrode, especially the first coulombic efficiency, is low. Summary of the invention

[0004] In view of the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a chemical pre-lithiation micron silicon and a preparation method and application thereof.

[0005] In order to solve the above technical problems, the technical solution of the present invention is:

[0006] A method for chemical pre-lithiation of micron silicon, the method comprising:

[0007] 1) coating a slurry on a copper foil, and vacuum drying the coated copper foil to obtain a micron silicon pole piece; the slurry includes micron silicon, a binder, and carbon black;

[0008] 2) The dried micron silicon pole piece is added to a pre-lithiation solution for immersion, and then rinsed to obtain a chemically pre-lithiation micron silicon lithium-ion battery negative electrode; the pre-lithiation solution is a 4,4'-dimethylbiphenyl lithium solution.

[0009] The present invention provides a method for chemical pre-lithiation of micron silicon, firstly, a micron silicon pole piece is made, and carbon black is used as a conductive agent; then the pole piece is vacuum dried; the dried micron silicon pole piece is immersed in a pre-lithiation solution for loading, and during the immersion process, the active lithium in 4,4'-dimethylbiphenyl lithium is embedded in the micron silicon, and the pre-lithiation of the micron silicon is completed. The obtained micron silicon pole piece can be used to compensate for the loss of active lithium during the charge and discharge process through pre-lithiation. The first coulomb efficiency of the silicon negative electrode is improved; and the loss capacity of the silicon negative electrode during the first charge and discharge is reduced.

[0010] The binder in the present invention can be any binder commonly used in lithium batteries without any particular limitation. In some embodiments of the present invention, the binder is one or more of carboxycellulose, styrene-butadiene rubber, and polyacrylic acid.

[0011] In some embodiments of the present invention, micron silicon is one or more of micron silicon particles, micron two-dimensional silicon, and micron porous silicon. In some embodiments of the present invention, the particle size of micron silicon is 1 to 10 um. In the present invention, micron silicon within a certain micron particle size range is selected.

[0012] In some embodiments of the present invention, the mass ratio of micron silicon, binder and carbon black is 3-8:1:1; preferably 6:2:2 or 8:1:1.

[0013] In some embodiments of the present invention, in step 1), the slurry is mixed with micron silicon, a binder and carbon black by stirring, and the stirring time is 6h-30h; further, 10h-24h.

[0014] In some embodiments of the present invention, the vacuum drying temperature is 50-100° C., and the vacuum drying time is 10 h to 28 h; further, the vacuum drying temperature is 80° C., and the vacuum drying time is 12 h to 24 h.

[0015] In some embodiments of the present invention, 4,4'-dimethylbiphenyl lithium is a complex formed by dissolving a metal lithium sheet in a 4,4'-dimethylbiphenyl solution, and the solvent of the 4,4'-dimethylbiphenyl solution is ethylene glycol dimethyl ether (DME). Further, the concentration of 4,4'-dimethylbiphenyl lithium in the solution is 0.2-1.0 mol / L.

[0016] In some embodiments of the present invention, the pre-lithiation time is 5 minutes to 30 minutes. The pre-lithiation time can ensure that the active lithium in 4,4'-dimethylbiphenyl lithium can be embedded in micron silicon, which can greatly improve the first coulombic efficiency of the silicon negative electrode. The principle of using biphenyl lithium in the present invention is to use the principle of active lithium embedding, which is different from the principle of biphenyl pre-lithiation silicon. Biphenyl pre-lithiation silicon forms an SEI film, which is a passivation film in lithium-ion batteries.

[0017] In some embodiments of the present invention, in step 2), a flushing agent is used for flushing, and the flushing agent is an organic solvent that can dissolve 4,4'-dimethylbiphenyl, and further can be ethylene glycol dimethyl ether, ethylene glycol methyl ether, and the like.

[0018] In a second aspect, the chemical pre-lithiated micron silicon obtained by the above method is a composite micron silicon material, and active lithium (forming Li x The micron silicon negative electrode of the present invention can make up for the loss of active lithium in the initial charge and discharge process, and improve the initial coulomb efficiency of the silicon negative electrode.

[0019] The third aspect is the application of the above-mentioned chemical pre-lithiation micron silicon in the negative electrode of lithium-ion batteries.

[0020] One or more technical solutions of the present invention have the following beneficial effects:

[0021] The chemical pre-lithiated micron silicon and the preparation method thereof of the present invention, wherein active lithium is pre-embedded in the chemical pre-lithiated micron silicon during the preparation process, avoids huge volume changes during the lithium insertion and delithiation processes, avoids repeated growth of the SEI film between the silicon-based negative electrode and the electrolyte, and improves the coulombic efficiency of the silicon-based negative electrode, especially the first coulombic efficiency; and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present application. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0023] Figure 1 This is the XRD pattern of the micron silicon used in Example 1.

[0024] Figure 2 This is a SEM image of the micron silicon used in Example 1.

[0025] Figure 3 This is the first charge and discharge curve of the unlithiated micro-silicon lithium-ion battery negative electrode.

[0026] Figure 4 This is the first charge and discharge curve of the pre-lithiated micron silicon lithium ion battery negative electrode prepared in Example 1. DETAILED DESCRIPTION

[0027] It should be noted that the following detailed descriptions are all illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0028] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, they indicate the presence of features, steps, operations, devices, components and / or combinations thereof. The present invention is further described below in conjunction with the embodiments

[0029] Example 1

[0030] A method for chemical pre-lithiation of micron silicon is as follows:

[0031] (1) 1 μm silicon, polyacrylic acid and carbon black were mixed in a mass ratio of 6:2:2 and stirred at room temperature for 24 h;

[0032] (2) The prepared slurry was evenly applied on the copper foil and dried under vacuum conditions for 12 hours;

[0033] (3) The cut micron silicon electrode is added to a 0.5 mol / L 4,4'-dimethylbiphenyl lithium glycol dimethyl ether solution and soaked for 10 min, and then rinsed with glycol dimethyl ether to obtain pre-lithiated micron silicon.

[0034] Example 2

[0035] A method for chemical pre-lithiation of micron silicon is as follows:

[0036] (1) 10 μm silicon, polyacrylic acid and carbon black were mixed in a mass ratio of 6:2:2 and stirred at room temperature for 24 h;

[0037] (2) Apply the prepared slurry evenly on the copper foil and dry it under vacuum for 24 hours;

[0038] (3) The cut micron silicon electrode is added into a 0.2 mol / L 4,4'-dimethylbiphenyl lithium glycol dimethyl ether solution and soaked for 10 min, and then rinsed with glycol dimethyl ether to obtain pre-lithiated micron silicon.

[0039] Example 3

[0040] A method for chemical pre-lithiation of micron silicon is as follows:

[0041] (1) mixing micron two-dimensional silicon, polyacrylic acid, and carbon black in a mass ratio of 6:2:2 and stirring at room temperature for 24 hours;

[0042] (2) The prepared slurry was evenly applied on the copper foil and dried under vacuum conditions for 18 hours;

[0043] (3) The cut micron silicon electrode is added to a 1.0 mol / L 4,4'-dimethylbiphenyl lithium glycol dimethyl ether solution and soaked for 10 min, and then rinsed with glycol dimethyl ether to obtain pre-lithiated micron silicon.

[0044] Example 4

[0045] A method for chemical pre-lithiation of micron silicon is as follows:

[0046] (1) mixing microporous silicon, carboxycellulose and carbon black in a mass ratio of 6:2:2 and stirring at room temperature for 24 hours;

[0047] (2) The prepared slurry was evenly applied on the copper foil and dried under vacuum conditions for 12 hours;

[0048] (3) The cut micron silicon electrode is added to a 0.5 mol / L 4,4'-dimethylbiphenyl lithium glycol dimethyl ether solution and soaked for 20 min, and then rinsed with glycol dimethyl ether to obtain pre-lithiated micron silicon.

[0049] Example 5

[0050] A method for chemical pre-lithiation of micron silicon is as follows:

[0051] (1) 1 μm silicon, styrene-butadiene rubber and carbon black were mixed in a mass ratio of 8:1:1 and stirred at room temperature for 24 h;

[0052] (2) The prepared slurry was evenly applied on the copper foil and dried under vacuum conditions for 12 hours;

[0053] (3) The cut micron silicon electrode is added into a 0.5 mol / L 4,4'-dimethylbiphenyl lithium glycol dimethyl ether solution and soaked for 5 min, and then rinsed with glycol dimethyl ether to obtain pre-lithiated micron silicon.

[0054] Figure 1 This is the XRD diagram of the micron silicon used in step 1) of Example 1. It can be seen from the diagram that it contains silicon element.

[0055] Figure 2 This is a SEM image of the micron-sized silicon particles used in step 1) of Example 1. From the image, it can be seen that the particle size of the micron silicon is 1-10 um.

[0056] The pre-lithiated micron silicon prepared in Example 3 and the unlithiated micron silicon used in Example 3 were subjected to charge and discharge experiments. The experimental process was to use an electrochemical workstation to perform constant current charge and discharge on a half-cell assembled with the pre-lithiated micron silicon negative electrode material and a lithium sheet at a current density of 200 mA / g.

[0057] The first charge and discharge curve of unlithiated micro-silicon is as follows: Figure 3 As shown in Figure 1, it can be seen that during the first charge and discharge process, the capacity loss reaches 216 mAh / g. The first charge and discharge curve of pre-lithiated micron silicon is shown in Figure 1. Figure 4 As shown, it can be seen that during the first charge and discharge process, the capacity loss reaches 24 mAh / g, which indicates that the pre-lithiated micron silicon of the present invention can improve the first coulombic efficiency when used as the negative electrode of the lithium-ion battery.

[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for chemical pre-lithiation of micron silicon, characterized in that: The method is: 1) coating a slurry on a copper foil, and vacuum drying the coated copper foil to obtain a micron silicon pole piece; the slurry includes micron silicon, a binder, and carbon black; 2) The dried micron silicon pole piece is added to a pre-lithiation solution and soaked, and then rinsed to obtain a chemical pre-lithiation micron silicon lithium-ion battery negative electrode; the pre-lithiation solution is a 4,4'-dimethylbiphenyl lithium solution; The vacuum drying temperature is 50-100°C, and the vacuum drying time is 10h to 28h; The mass ratio of micron silicon, binder and carbon black is 3-8:1:1; 4,4'-dimethylbiphenyl lithium is a complex formed when a metal lithium sheet is dissolved in a 4,4'-dimethylbiphenyl solution, and the solvent of the 4,4'-dimethylbiphenyl solution is ethylene glycol dimethyl ether; The mass ratio of the micron silicon, the binder and the carbon black is 6:2:2 or 8:1:1; Micron silicon is one or more of micron silicon particles, micron two-dimensional silicon, and micron porous silicon; the particle size of micron silicon is 1 to 10 um.

2. The method for chemical pre-lithiation of micron silicon according to claim 1, characterized in that: The binder is one or more of carboxyl cellulose, styrene-butadiene rubber and polyacrylic acid.

3. The method for chemical pre-lithiation of micron silicon according to claim 1, characterized in that: In step 1), the slurry is made of micron silicon, a binder and carbon black and is mixed by stirring for 6 hours to 30 hours.

4. The method for chemical pre-lithiation of micron silicon according to claim 1, characterized in that: The vacuum drying temperature is 80°C, and the vacuum drying time is 12h to 24h.

5. The method for chemical pre-lithiation of micron silicon according to claim 1, characterized in that: The concentration of 4,4'-dimethylbiphenyl lithium in the complex is 0.2-1.0 mol / L.

6. The method for chemical pre-lithiation of micron silicon according to claim 1, characterized in that: The pre-lithiation time is 5 min to 30 min.

7. Chemically pre-lithiated micron silicon obtained by the method described in any one of claims 1 to 6.

8. Use of the chemically pre-lithiated micron silicon according to claim 7 in the negative electrode of a lithium-ion battery.