Rotor core, rotor and rotating electrical machine
By using electromagnetic steel plates with specific chemical composition in the rotor core, optimizing the rolling direction and magnetic properties, the problem of insufficient improvement in the magnetic properties of the rotor core in the existing technology is solved, and higher magnetic flux density and uniformity of magnetic properties are achieved. Reduces iron loss and copper loss.
Patent Information
- Application Number
- CN202080078201.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-15
- Filing Date
- 2020-11-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-11-13
AI Technical Summary
The existing rotor core's magnetic properties in reluctance motors and reluctance generators are insufficiently improved, especially the research on electromagnetic steel plates has not been fully explored, resulting in room for improvement in the magnetic properties of reluctance motors and reluctance generators.
Electromagnetic steel plates with specific chemical composition are used, containing elements such as C, Si, sol.Al, S, N, etc., and are optimized through specific rolling directions and magnetic properties to meet specific magnetic flux density and X-ray random intensity ratio conditions to achieve Improve the magnetic properties of the rotor core.
By optimizing the chemical composition and structure of the electromagnetic steel plate, the magnetic properties of the rotor core of the reluctance motor or reluctance generator are significantly improved, the magnetic flux density and magnetic properties uniformity are enhanced, and the iron loss and copper loss are reduced.
Smart Images

Figure CN114667662B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a rotor core, a rotor and a rotating electric machine, and is particularly applicable to a reluctance motor and a reluctance generator.
[0002] This application claims priority based on Japanese Patent Application No. 2019-206676 filed in Japan on November 15, 2019, and the contents of which are incorporated herein by reference. Background Art
[0003] Generally, the rotor of a reluctance motor does not use a magnet. Therefore, it is not necessary to use high-cost rare earth in the reluctance motor. From this point of view, the reluctance motor has attracted much attention in recent years.
[0004] The reluctance motor configures the rotor and stator in such a way that the magnetic poles of the rotor and the stator are opposite to each other, and by sequentially changing the excitation current flowing through multiple excitation coils wound on the stator, a magnetic attraction in the rotational direction (circumferential direction) is generated on the rotor, thereby rotating the rotor.
[0005] As reluctance motors, there are switched reluctance motors and synchronous reluctance motors (for example, refer to Patent Documents 1 and 2). As described in Patent Documents 1 and 2, in a reluctance motor, rotor magnetic poles are formed by providing salient poles (convex portions) spaced apart in the circumferential direction or by forming slits in the rotor core.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2012-114975
[0009] Patent Document 2: Japanese Patent Application Publication No. 2017-135878 Summary of the invention
[0010] Technical problem to be solved by the invention
[0011] However, the techniques described in Patent Documents 1 and 2 do not study the electromagnetic steel sheets used in the rotor core. Therefore, there is room for improvement in the magnetic properties of the conventional rotor core. This applies not only to reluctance motors but also to reluctance generators.
[0012] The present invention has been made in view of the above-mentioned problems, and aims to improve the magnetic characteristics of a rotor core used in a reluctance motor or a reluctance generator.
[0013] Technical means for solving technical problems
[0014] In order to solve the above-mentioned problems, the present invention adopts the following configuration.
[0015] (1) A rotor core of the present invention is a rotor core of a reluctance motor or a reluctance generator, and has a plurality of electromagnetic steel sheets, characterized in that the electromagnetic steel sheets have the following chemical composition: in terms of mass %, containing: C: less than 0.0100%, Si: 1.50% to 4.00%, sol.Al: 0.0001% to 1.0%, S: less than 0.0100%, N: less than 0.0100%, Mn, Ni, Co, Pt, Pb, Cu, A u: 2.50% to 5.00% in total, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, Cd: 0.0000% to 0.0100% in total; Mn content (mass %) is recorded as [Mn], Ni content is recorded as [Mn], When (mass %) is recorded as [Ni], Co content (mass %) is recorded as [Co], Pt content (mass %) is recorded as [Pt], Pb content (mass %) is recorded as [Pb], Cu content (mass %) is recorded as [Cu], Au content (mass %) is recorded as [Au], Si content (mass %) is recorded as [Si], and sol.Al content (mass %) is recorded as [sol.Al], the following formula (A) is satisfied; the remainder is composed of Fe and impurities; the rolling direction is When B50 is denoted as B50L, B50 in the direction of 90° with the rolling direction is denoted as B50C, B50 in two directions of which the smaller angle is 45° with the rolling direction and B50 in one direction and the other direction are denoted as B50D1 and B50D2 respectively, the following equations (B) and (C) are satisfied; the X-ray random intensity ratio of {100}<011> is greater than 5 and less than 30, and the plate thickness is less than 0.50 mm.
[0016] ([Mn]+[Ni]+[Co]+[Pt]+[Pb]+[Cu]+[Au])-([Si]+[sol.Al])>0%…(A)
[0017] (B50D1+B50D2) / 2>1.7T…(B)
[0018] (B50D1+B50D2) / 2>(B50L+B50C) / 2…(C)
[0019] Here, the magnetic flux density B50 is the magnetic flux density when the magnetic field is excited at an intensity of 5000 A / m.
[0020] (2) The rotor core described in (1) above may satisfy the following formula (D).
[0021] (B50D1+B50D2) / 2>1.1×(B50L+B50C) / 2…(D)
[0022] (3) The rotor core described in (1) above may have a feature satisfying the following formula (E).
[0023] (B50D1+B50D2) / 2>1.2×(B50L+B50C) / 2…(E)
[0024] (4) The rotor core described in (1) above may have a feature satisfying the following formula (F).
[0025] (B50D1+B50D2) / 2>1.8T…(F)
[0026] (5) The rotor of the present invention is a rotor of a reluctance motor or a reluctance generator having a rotor core described in any one of (1) to (4), and has the following characteristics: the center line of at least one magnetic pole of the rotor in the circumferential direction is consistent with the direction in which the magnetic properties of at least one electromagnetic steel sheet are best; the direction in which the magnetic properties are best is at least one of the two directions in which the smaller angle formed with the rolling direction is 45°.
[0027] (6) The rotor described in (5) may also have the following characteristics: the number of magnetic poles is a multiple of 4; in the first direction of the two directions in which the magnetic properties of at least one of the electromagnetic steel sheets are the best, the two magnetic poles are located at positions opposite to each other with the axis separated therefrom; in the second direction of the two directions in which the magnetic properties of at least one of the electromagnetic steel sheets are the best, the two magnetic poles are located at positions opposite to each other with the axis separated therefrom; the circumferential center line of the two magnetic poles located at positions opposite to each other with the axis separated therefrom in the first direction is consistent with the first direction of at least one of the electromagnetic steel sheets; the circumferential center line of the two magnetic poles located at positions opposite to each other with the axis separated therefrom in the second direction is consistent with the second direction of at least one of the electromagnetic steel sheets.
[0028] (7) The rotor described in (6) may also have the following characteristics: the number of magnetic poles is 4; the center lines in the circumferential direction of two of the magnetic poles located at positions opposite to each other across the axis in the first direction are consistent with the first direction of the plurality of electromagnetic steel sheets; the center lines in the circumferential direction of two of the magnetic poles located at positions opposite to each other across the axis in the second direction are consistent with the second direction of the plurality of electromagnetic steel sheets.
[0029] (8) The plurality of electromagnetic steel sheets in the rotor according to any one of (5) to (7) may be stacked in a state where two directions with the best magnetic properties are shifted from each other.
[0030] (9) The plurality of electromagnetic steel sheets in the rotor according to any one of (5) to (8) may be stacked in a state where two directions with the best magnetic properties are periodically shifted in the stacking direction of the electromagnetic steel sheets.
[0031] (10) The rotor described in any one of (5) to (9) may also have the following feature: among all the magnetic poles whose center line in the circumferential direction coincides with the direction in which the magnetic properties of at least one of the electromagnetic steel sheets are best, the number of the electromagnetic steel sheets whose direction in which the magnetic properties of the electromagnetic steel sheets are best coincides with the center line in the circumferential direction of the magnetic pole is the same.
[0032] (11) The rotor described in any one of (5) to (10) may also have the following characteristics: it includes at least one electromagnetic steel plate, in which the direction in which the magnetic characteristics are best among all the magnetic poles coincides with the center line of the circumferential direction of the magnetic pole.
[0033] (12) The rotor described in any one of (5) to (11) may also have the following feature: in each of the plurality of electromagnetic steel sheets, at least one direction having the best magnetic properties coincides with the center line of the magnetic pole in the circumferential direction.
[0034] (13) The rotor described in any one of (5) to (12) may also have the following feature: in each of the plurality of electromagnetic steel sheets, the regions constituting the respective magnetic poles of the electromagnetic steel sheet have the same positional relationship relative to the rolling direction. (14) The rotating electrical machine of the present invention may also have the following feature: it has the rotor core described in any one of (1) to (13) and is a reluctance motor or a reluctance generator.
[0035] Effects of the Invention
[0036] According to the above aspect of the present invention, it is possible to improve the magnetic characteristics of a rotor core used in a reluctance motor or a reluctance generator. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a diagram showing a first example of the structure of a rotating electrical machine.
[0038] Figure 2 This is a diagram showing a first example of a rotor structure.
[0039] Figure 3 It is a diagram showing a first example of the positional relationship with respect to the rolling direction of electromagnetic steel sheets constituting the rotor core.
[0040] Figure 4 It is a diagram showing a second example of the structure of the rotating electrical machine.
[0041] Figure 5 It is a diagram showing a second example of the rotor structure.
[0042] Figure 6 This is a diagram showing an example of a cross section of a rotor core.
[0043] Figure 7 It is a diagram showing a second example of the positional relationship with respect to the rolling direction of the electromagnetic steel sheets constituting the rotor core.
[0044] Figure 8 It is a diagram showing a first example of the structure of a rotating electrical machine.
[0045] Fig. 9 It is a diagram showing a third example of the rotor structure.
[0046] Fig. 10A It is a diagram showing a third example of the positional relationship with respect to the rolling direction of the electromagnetic steel sheets constituting the rotor core.
[0047] Fig. 10B This is a diagram showing an example of the rolling direction and easy magnetization direction of an electromagnetic steel sheet.
[0048] Fig.11 It is a diagram showing an example of the positional relationship of electromagnetic steel sheets in the height direction. DETAILED DESCRIPTION
[0049] (Electromagnetic steel sheet for rotor core)
[0050] First, an electromagnetic steel sheet used for a rotor core of an embodiment described later will be described.
[0051] First, the chemical composition of the steel used in an example of the non-oriented electrical steel sheet for the rotor core and its manufacturing method will be described. In the following description, the unit "%" of the content of each element contained in the non-oriented electrical steel sheet or the steel represents "mass%" unless otherwise specified. In addition, in the numerical limit range described with "~", the lower limit value and the upper limit value are included. The numerical values expressed as "less than" or "more than" are not included in the numerical range. The non-oriented electrical steel sheet and the steel, which are an example of the non-oriented electrical steel sheet for the rotor core, have a chemical composition capable of undergoing a ferrite-austenite phase transformation (hereinafter referred to as α-γ phase transformation), and contain: C: 0.0100% or less, Si: 1.50% to 4.00%, sol.Al: 0.0001% to 1.0%, S: 0.0100% or less, N: 0.0100% or less, and one or more selected from the group consisting of Mn, Ni, Co, Pt, Pb, Cu, Au: a total of 2.50% to 5.00%, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and one or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: a total of 0.0000% to 0.0100%, and the balance is composed of Fe and impurities. Further, the contents of Mn, Ni, Co, Pt, Pb, Cu, Au, Si, and sol.Al satisfy the predetermined conditions described later. Examples of the impurities include impurities contained in raw materials such as ores or scraps, and impurities contained in the manufacturing process.
[0052] <<C: 0.0100% or less>>
[0053] C increases iron loss or causes magnetic aging. Therefore, the lower the C content, the better. This phenomenon is significant when the C content exceeds 0.0100%. Thus, the C content is made 0.0100% or less. The reduction of the C content is also beneficial to the uniform improvement of the magnetic properties in all directions within the sheet surface. It should be noted that although the lower limit of the C content is not particularly limited, considering the cost of decarburization treatment during refining, it is preferably 0.0005% or more.
[0054] <<Si: 1.50% to 4.00%>>
[0055] Si increases the resistance, reduces the eddy current loss, and reduces the iron loss, or increases the yield ratio and improves the blanking processability of the iron core. When the Si content is less than 1.50%, these effects cannot be fully obtained. Therefore, the Si content is made 1.50% or more. On the other hand, when the Si content exceeds 4.00%, the magnetic flux density decreases, or the hardness rises excessively, resulting in a reduction in blanking processability, or cold rolling becomes difficult. Therefore, the Si content is made 4.00% or less.
[0056] <<sol.Al: 0.0001% - 1.0%>>
[0057] sol.Al increases the resistance and reduces the eddy current loss, and also reduces the iron loss. sol.Al is beneficial to increasing the magnitude of the magnetic flux density B50 relative to the saturation magnetic flux density. Here, the magnetic flux density B50 is the magnetic flux density when excited in a magnetic field with a magnetic field strength of 5000 A / m. When the content of sol.Al is less than 0.0001%, these effects cannot be fully obtained. In addition, Al also has the effect of promoting desulfurization during steelmaking. Thus, the content of sol.Al is made to be 0.0001% or more. On the other hand, when the content of sol.Al exceeds 1.0%, the magnetic flux density decreases, or the yield ratio decreases, resulting in a reduction in blanking processability. Thus, the content of sol.Al is made to be 1.0% or less.
[0058] <<S: 0.0100% or less>>
[0059] S is not an essential element and is contained as an impurity in steel, for example. S hinders recrystallization and grain growth during annealing through the precipitation of fine MnS. Thus, the lower the S content, the better. The increase in iron loss and the reduction in magnetic flux density due to the hindrance of recrystallization and grain growth are significant when the S content exceeds 0.0100%. Therefore, the S content is made to be 0.0100% or less. It should be noted that although the lower limit of the S content is not specifically limited, considering the cost of desulfurization treatment during refining, it is preferably 0.0003% or more.
[0060] <<N: 0.0100% or less>>
[0061] Similar to C, N deteriorates the magnetic properties, so the lower the N content, the better. Thus, the N content is made to be 0.0100% or less. It should be noted that although the lower limit of the N content is not specifically limited, considering the cost of denitrification treatment during refining, it is preferably 0.0010% or more.
[0062] <<Select one or more from the group consisting of Mn, Ni, Co, Pt, Pb, Cu, Au: Total 2.50% - 5.00%>>
[0063] These elements are necessary elements for the occurrence of α-γ phase transformation, so at least a total of 2.50% or more of these elements are contained. On the other hand, if the total exceeds 5.00%, the cost will increase and the magnetic flux density will decrease. Thus, the total of these elements is made to be 5.00% or less.
[0064] In addition, as a condition for the occurrence of α-γ phase transformation, the following conditions must be further satisfied. That is, when the Mn content (mass %) is recorded as [Mn], the Ni content (mass %) is recorded as [Ni], the Co content (mass %) is recorded as [Co], the Pt content (mass %) is recorded as [Pt], the Pb content (mass %) is recorded as [Pb], the Cu content (mass %) is recorded as [Cu], the Au content (mass %) is recorded as [Au], the Si content (mass %) is recorded as [Si], and the sol.Al content (mass %) is recorded as [sol.Al], it is preferred that the following formula (1) is satisfied in terms of mass %.
[0065] ([Mn]+[Ni]+[Co]+[Pt]+[Pb]+[Cu]+[Au])-([Si]+[sol.Al])>0%…(1)
[0066] When the above-mentioned formula (1) is not satisfied, the magnetic flux density becomes low because the α-γ phase transition does not occur.
[0067] <<Sn:0.000%~0.400%、Sb:0.000%~0.400%、P:0.000%~0.400%> >
[0068] Sn or Sb improves the texture after cold rolling and recrystallization and increases its magnetic flux density. Therefore, these elements can be contained as needed, but excessive inclusion will cause embrittlement of the steel. Therefore, either the Sn content or the Sb content is less than 0.400%. In addition, in order to ensure the hardness of the steel plate after recrystallization, P can be contained, but excessive inclusion will cause embrittlement of the steel. Therefore, the P content is less than 0.400%. When further effects such as magnetic properties are imparted as described above, it is preferred to contain one or more selected from the group consisting of 0.020% to 0.400% Sn, 0.020% to 0.400% Sb, and 0.020% to 0.400% P.
[0069] <<One or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total>>
[0070] Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn and Cd react with S in the molten steel during casting to form sulfide or oxysulfide or precipitates of both. Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn and Cd are sometimes collectively referred to as "coarse precipitate forming elements" below. The particle size of the precipitates of the coarse precipitate forming elements is about 1μm to 2μm, which is much larger than the particle size of fine precipitates such as MnS, TiN, AlN (about 100nm). Therefore, these fine precipitates adhere to the precipitates of the coarse precipitate forming elements, making it difficult to hinder the recrystallization and grain growth during annealing such as intermediate annealing. In order to fully obtain such an effect, it is preferred that the total amount of coarse precipitate forming elements is 0.0005% or more. However, if the total amount of these elements exceeds 0.0100%, the total amount of sulfides or oxysulfides or both will be excessive, thereby inhibiting recrystallization and grain growth during intermediate annealing. Therefore, the total content of the coarse precipitate-forming elements is set to 0.0100% or less.
[0071] <<Texture>>
[0072] Next, the texture of a non-oriented electromagnetic steel sheet as an example of an electromagnetic steel sheet for a rotor core is described. The details of the manufacturing method will be described later. A non-oriented electromagnetic steel sheet as an example of an electromagnetic steel sheet for a rotor core has a chemical composition that can undergo an α-γ phase transformation. The structure is refined by direct quenching after the finish rolling during hot rolling, so that the {100} crystal grains become a growing structure. As a result, the clustering strength of the non-oriented electromagnetic steel sheet as an example of an electromagnetic steel sheet for a rotor core becomes 5 to 30 in the {100}<011> orientation, and the magnetic flux density B50 in the direction of 45° relative to the rolling direction becomes particularly high. In this way, the magnetic flux density becomes high in a specific direction, but a high magnetic flux density can be obtained in the overall average in all directions. If the clustering strength of the {100}<011> orientation is less than 5, the clustering strength of the {111}<112> orientation that reduces the magnetic flux density will become high, so that the magnetic flux density decreases overall. In addition, the production method in which the cluster strength of the {100}<011> orientation exceeds 30 requires thickening the hot-rolled sheet, which causes a problem of difficulty in production.
[0073] The clustering intensity of the {100}<011> orientation can be measured by X-ray diffraction or electron backscatter diffraction (EBSD). Since the reflection angle of the sample from the X-ray and electron beam varies depending on the crystal orientation, the crystal orientation intensity can be obtained based on the reflection intensity of the randomly oriented sample. As an example of an electromagnetic steel sheet for a rotor core, the clustering intensity of the {100}<011> orientation of a suitable non-oriented electromagnetic steel sheet is an X-ray random intensity ratio of 5 to 30. At this time, the crystal orientation is measured by EBSD, and the value converted to the X-ray random intensity ratio can also be used.
[0074] <<Thickness>>
[0075] Next, the thickness of a non-oriented electromagnetic steel sheet as an example of an electromagnetic steel sheet used for a rotor core is described. The thickness of a non-oriented electromagnetic steel sheet as an example of an electromagnetic steel sheet used for a rotor core is 0.50 mm or less. If the thickness exceeds 0.50 mm, good high-frequency iron loss cannot be obtained. Therefore, the thickness is set to 0.50 mm or less.
[0076] <<Magnetic properties>>
[0077] Next, the magnetic properties of a non-oriented electromagnetic steel sheet as an example of an electromagnetic steel sheet for a rotor core are investigated. When investigating the magnetic properties, the value of the magnetic flux density B50 of a non-oriented electromagnetic steel sheet as an example of an electromagnetic steel sheet for a rotor core is measured. In the manufactured non-oriented electromagnetic steel sheet, one direction and the other direction of the rolling direction cannot be distinguished. Therefore, in the present embodiment, the rolling direction refers to two directions, one direction and the other direction. If the value of B50 (T) in the rolling direction is B50L, the value of B50 (T) in the direction inclined at 45° from the rolling direction is B50D1, the value of B50 (T) in the direction inclined at 90° from the rolling direction is B50C, and the value of B50 (T) in the direction inclined at 135° from the rolling direction is B50D2, it can be found that the anisotropy of the magnetic flux density is the highest in B50D1 and B50D2, and the lowest in B50L and B50C. It should be noted that (T) refers to the unit of magnetic flux density (Tesla).
[0078] At this time, considering the distribution of all orientations (0° to 360°) of the magnetic flux density with the clockwise (or counterclockwise) direction as the positive direction, if the rolling direction is 0° (one direction) and 180° (the other direction), B50D1 is the B50 value of 45° and 225°, and B50D2 is the B50 value of 135° and 315°. Similarly, B50L is the B50 value of 0° and 180°, and B50C is the B50 value of 90° and 270°. The B50 value of 45° is strictly consistent with the B50 value of 225°, and the B50 value of 135° is strictly consistent with the B50 value of 315°. However, it is difficult to make the magnetic properties of B50D1 and B50D2 the same during actual manufacturing, so there is a case where they are not strictly consistent. Similarly, the B50 value at 0° is strictly consistent with the B50 value at 180°, and the B50 value at 90° is strictly consistent with the B50 value at 270°, but on the other hand, there is a case where B50L and B50C are not strictly consistent. In a non-oriented electromagnetic steel sheet, which is an example of an electromagnetic steel sheet for a rotor core, the average values of B50D1 and B50D2, and the average values of B50L and B50C satisfy the following equations (2) and (3).
[0079] (B50D1+B50D2) / 2>1.7T…(2)
[0080] (B50D1+B50D2) / 2>(B50L+B50C) / 2…(3)
[0081] Thus, when the magnetic flux density is measured, as shown in formula (2), when the average value of B50D1 and B50D2 is greater than 1.7 T, high anisotropy of the magnetic flux density is confirmed as shown in formula (3).
[0082] Furthermore, in addition to satisfying the formula (1), it is preferred that the anisotropy of the magnetic flux density be higher than that of the formula (3), as shown in the following formula (4).
[0083] (B50D1+B50D2) / 2>1.1×(B50L+B50C) / 2…(4)
[0084] Furthermore, it is preferred that the anisotropy of the magnetic flux density be higher as shown in the following formula (5).
[0085] (B50D1+B50D2) / 2>1.2×(B50L+B50C) / 2…(5)
[0086] Furthermore, as shown in the following formula (6), the average value of B50D1 and B50D2 is preferably 1.8T or more.
[0087] (B50D1+B50D2) / 2>1.8T…(6)
[0088] It should be noted that the above 45° is a theoretical value. In actual manufacturing, it is difficult to achieve the same value as 45°, so it also includes the case where the angle is not strictly consistent with 45°. In this regard, the same applies to the cases of 0°, 90°, 135°, 180°, 225°, 270°, and 315°.
[0089] The magnetic flux density was measured by cutting out 55 mm square samples from directions such as 45° and 0° relative to the rolling direction and measuring them using a single plate magnetic measuring device.
[0090] <<Manufacturing method>>
[0091] Next, a method for manufacturing an example of a non-oriented electromagnetic steel sheet as an example of an electromagnetic steel sheet for a rotor core is described. When manufacturing the non-oriented electromagnetic steel sheet as an example of an electromagnetic steel sheet for a rotor core, for example, hot rolling, cold rolling (first cold rolling), intermediate annealing (first annealing), skin pass rolling (second cold rolling), final annealing (third annealing), stress relief annealing (second annealing), etc. are performed.
[0092] First, the steel is heated and hot rolled. The steel is, for example, a steel billet produced by general continuous casting. Rough rolling and finish rolling of hot rolling are performed at a temperature in the γ region (above the Ar1 temperature). That is, the final temperature of the finish rolling is above the Ar1 temperature, and hot rolling is performed in a manner such that the coiling temperature is greater than 250° and less than 600°. Thus, by cooling thereafter, the austenite phase changes to ferrite, thereby refining the structure. If cold rolling is subsequently performed in a refined state, stretching recrystallization (hereinafter referred to as "expansion") becomes easier to occur, thereby making it easier for {100} grains, which are usually difficult to grow, to grow.
[0093] In addition, when manufacturing a non-oriented electromagnetic steel sheet as an example of an electromagnetic steel sheet for a rotor core, the temperature (final temperature) at the final pass of finish rolling is further set to be above the Ar1 temperature, and the coiling temperature is set to be above 250° and below 600°. The crystal structure is refined by transformation from austenite to ferrite. By refining the crystal structure in this way, expansion can be easily caused by intermediate annealing in the subsequent cold rolling.
[0094] After that, the hot-rolled sheet is directly coiled without annealing, and after pickling, the hot-rolled steel sheet is cold rolled. It is preferred to set the reduction rate to 80% to 95% during cold rolling. If the reduction rate is less than 80%, expansion is difficult to occur. If the reduction rate exceeds 95%, the {100} grains will grow more easily through the subsequent expansion, but the hot-rolled steel sheet needs to be thickened, and hot rolling becomes difficult, and the operation is also likely to become difficult. The reduction rate of cold rolling is more preferably above 86%. When the reduction rate of cold rolling is above 86%, expansion becomes more likely to occur.
[0095] After the cold rolling is completed, intermediate annealing is continued. When manufacturing a non-oriented electromagnetic steel sheet, which is an example of an electromagnetic steel sheet for a rotor core, intermediate annealing is performed at a temperature that does not transform into austenite. That is, the temperature of the intermediate annealing is preferably less than the Ac1 temperature. By performing intermediate annealing in this way, expansion occurs, and {100} grains become easier to grow. In addition, the time of intermediate annealing is preferably 5 seconds to 60 seconds.
[0096] After the intermediate annealing is completed, skin-pass rolling is then performed. If skin-pass rolling and annealing are performed in the state where expansion occurs in the manner described above, the {100} grains will further grow starting from the portion where expansion occurs. This is because through skin-pass rolling, the {100}<011> grains have the property of being difficult to accumulate strain, while the {111}<112> grains have the property of being easy to accumulate strain. In the subsequent annealing, the {100}<011> grains with less strain use the strain difference as the driving force to erode the {111}<112> grains. This erosion phenomenon caused by the strain difference as the driving force is called strain-induced grain boundary migration (hereinafter referred to as SIBM). The reduction rate of skin-pass rolling is preferably 5% to 25%. Since the amount of strain is too small when the reduction rate is less than 5%, SIBM does not occur in the subsequent annealing, and the {100}<011> grains cannot become larger. On the other hand, when the reduction rate exceeds 25%, the strain amount is too large, and recrystallization nuclei (hereinafter referred to as nucleation) will occur, in which new crystal grains are generated from {111}<112> crystal grains. Almost all the crystal grains generated in this nucleation are {111}<112> crystal grains, so the magnetic properties will deteriorate.
[0097] After skin smooth rolling, the strain is released and final annealing is performed to improve the workability. The final annealing is also performed at a temperature that does not transform into austenite, and the temperature of the final annealing is lower than the Ac1 temperature. By performing the final annealing in this way, the {100}<011> grains can erode the {111}<112> grains and improve the magnetic properties. In addition, the time at 600°C ~ Ac1 temperature is kept within 1200 seconds during the final annealing. If the annealing time is too short, the strain generated during skin smooth rolling will almost completely remain, and warping will occur when punching into complex shapes. On the other hand, if the annealing time is too long, the grains become too large, the collapsed edge expands during punching, and the required punching accuracy cannot be achieved.
[0098] After the final annealing is completed, the non-oriented electromagnetic steel sheet is subjected to forming processing, etc., to be processed into the desired steel parts. Then, in order to remove the strain caused by forming processing (such as punching) in the steel parts composed of the non-oriented electromagnetic steel sheet, stress relief annealing is performed on the steel parts. In this embodiment, in order to allow SIBM to occur and to make the grain size coarse even at a temperature lower than Ac1, the temperature of stress relief annealing is set to, for example, about 800°C, and the time of stress relief annealing is set to about 2 hours. The magnetic properties can be improved by stress relief annealing.
[0099] In the non-oriented electromagnetic steel sheet (iron steel part) as an example of an electromagnetic steel sheet for a rotor core, in the manufacturing method, high B50 of the above formula (1) and good anisotropy of the above formula (2) are obtained by mainly performing finish rolling at a temperature of Ar1 or higher in the hot rolling process. Furthermore, by setting the reduction rate to about 10% in the skin pass rolling process, even better anisotropy of the above formula (4) is obtained.
[0100] It should be noted that in this embodiment, the Ar1 temperature is obtained from the thermal expansion change of the steel material (steel plate) during cooling at an average cooling rate of 1°C / sec. In addition, in this embodiment, the Ac1 temperature is obtained from the thermal expansion change of the steel material (steel plate) during heating at an average heating rate of 1°C / sec.
[0101] The electromagnetic steel sheet for a rotor core as described above as one example can be used to manufacture an iron and steel component composed of a non-oriented electromagnetic steel sheet.
[0102] Next, an embodiment will be shown and a non-oriented electromagnetic steel sheet as an example of an electromagnetic steel sheet used for a rotor core will be specifically described. The embodiment shown below is only an example of a non-oriented electromagnetic steel sheet, and the non-oriented electromagnetic steel sheet is not limited to the following example.
[0103] <<First Embodiment>>
[0104] By casting molten steel, ingots with the compositions shown in the following Tables 1 to 2 are produced. The left side of the formula here represents the value on the left side of the formula (1). Thereafter, the produced ingot is heated to 1150°C for hot rolling and rolled to a plate thickness of 2.5 mm. Then, after the finish rolling is completed, the hot-rolled steel plate is water-cooled and coiled. At this time, the temperature at the final pass stage of the finish rolling (final temperature) is 830°C, which is higher than all Ar1 temperatures. It should be noted that the final temperature of No. 108, which did not undergo γ-α phase transformation, was set to 850°C. In addition, the coiling temperature was carried out under the conditions shown in Table 1.
[0105] Next, the hot rolled steel sheet was pickled to remove the oxide film, and then rolled at the reduction ratio after cold rolling shown in Table 1. Then, intermediate annealing was performed at 700°C for 30 seconds in an oxygen-free atmosphere. Subsequently, rolling was performed at the second cold rolling (skin pass rolling) reduction ratio shown in Table 1.
[0106] Next, to investigate the magnetic properties, after the second cold rolling (skin-pass rolling), a final annealing was performed at 800°C for 30 seconds, and a 55 mm square sample was made by shearing. After stress relief annealing was performed at 800°C for 2 hours, the magnetic flux density B50 was measured. The measured samples were 55 mm square samples taken from the two directions of 0° and 45° in the rolling direction. Then, the magnetic flux density B50 of these two samples at 0°, 45°, 90°, and 135° relative to the rolling direction was measured as B50L, B50D1, B50C, and B50D2, respectively.
[0107] Table 1
[0108]
[0109] Table 2
[0110]
[0111] The underlines in Tables 1 and 2 indicate conditions that are outside the scope of the present invention. Inventive Examples No. 101 to No. 107, No. 109 to No. 111, and No. 114 to No. 130 all have good values of magnetic flux density B50 in the 45° direction and on average over the entire circumference. However, No. 116 and No. 127 exceed the appropriate coiling temperature, so the magnetic flux density B50 is slightly low. No. 129 and No. 130 have a low cold rolling reduction rate, so the magnetic flux density B50 is slightly lower than that of No. 118 with the same composition and coiling temperature. On the other hand, since the Si concentration of Comparative Example No. 108 is high and the value on the left side of the formula is below 0, it is a composition in which α-γ phase transformation does not occur, so the magnetic flux density B50 is very low. Since the skin smooth rolling rate of Comparative Example No. 112 is set low and the {100} <011> strength is less than 5, the magnetic flux density B50 is very low. The {100}<011> strength of Comparative Example No. 113 is greater than 30, which is outside the scope of the present invention. Since the thickness of the hot-rolled sheet No. 113 is 7 mm, there is a problem of difficulty in handling.
[0112] <<Second Embodiment>>
[0113] By casting molten steel, an ingot having the composition shown in Table 3 below is produced. Thereafter, the produced ingot is heated to 1150°C and hot rolled to a plate thickness of 2.5 mm. After the finish rolling is completed, the hot rolled steel plate is water cooled and coiled. At this time, the final temperature of the final pass of the finish rolling is 830°C, which is a temperature greater than the Ar1 temperature.
[0114] Next, the hot rolled steel sheet is pickled to remove the oxide film, and then cold rolled to a thickness of 0.385 mm. Then, intermediate annealing is performed in an oxygen-free environment, and the temperature of the intermediate annealing is controlled to achieve a recrystallization rate of 85%. Then, a second cold rolling (skin pass rolling) is performed to a thickness of 0.35 mm.
[0115] Next, in order to investigate the magnetic properties, a final annealing was performed at 800°C for 30 seconds after the second cold rolling (skin smooth rolling). After a 55 mm square sample was made by shearing, a stress relief annealing was performed at 800°C for 2 hours, and the magnetic flux density B50 and iron loss W10 / 400 were measured. The magnetic flux density B50 was measured in the same order as in the first embodiment. On the other hand, the iron loss W10 / 400 was measured as the energy loss (W / kg) generated by the sample when an AC magnetic field of 400 Hz was applied to make the maximum magnetic flux density reach 1.0 T. The iron loss is the average value of the measurement results at 0°, 45°, 90°, and 135° relative to the rolling direction.
[0116] Table 3
[0117]
[0118] Table 4
[0119]
[0120] No. 201 to No. 214 are all invention examples, and all have good magnetic properties. In particular, No. 202 to No. 204 have higher magnetic flux density B50 than No. 201 and No. 205 to No. 214, and No. 205 to No. 214 have lower iron loss W10 / 400 than No. 201 to No. 204.
[0121] The inventors have found that in order to effectively utilize the properties of the non-oriented electromagnetic steel sheet, it is important to simultaneously achieve both the uniform magnetic properties in the circumferential direction of the rotor core and the best uniform magnetic properties in order to construct the rotor core of a reluctance motor or a reluctance generator. The rotor core of the embodiment described below is a product based on this concept.
[0122] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. It should be noted that in the following description, in the description of (electromagnetic steel sheet for rotor core), as required, the direction inclined at 45° from the rolling direction and the direction inclined at 135° from the rolling direction are collectively referred to as two directions with a smaller angle of 45° with the rolling direction. It should be noted that the 45° is an angle expressed by assuming that the angles of any of the clockwise and counterclockwise directions have positive values. When the clockwise direction is the negative direction and the counterclockwise direction is the positive direction, the two directions with a smaller angle of 45° with the rolling direction become two directions with a smaller angle of 45° and -45° with the rolling direction. In addition, as required, the direction inclined at θ° from the rolling direction is referred to as the direction with an angle of θ° with the rolling direction. In this way, the direction inclined at θ° from the rolling direction and the direction with an angle of θ° with the rolling direction have the same meaning. In the following description, unless otherwise specified, the electromagnetic steel sheet is the non-oriented electromagnetic steel sheet described in the item (electromagnetic steel sheet for rotor core). In the following description, in addition to the case where the length, direction, position, etc. are strictly consistent, the case where the length, direction, position, etc. are consistent within the scope that does not deviate from the gist of the invention (for example, within the scope of the error generated in the manufacturing process) is also included.
[0123] (First embodiment)
[0124] First, the first embodiment will be described.
[0125] Figure 1 Schematic diagram of the structure of an exemplary rotating electrical machine. It should be noted that, in the present embodiment, an example is given of a case where the rotating electrical machine is a switched reluctance motor. It should be noted that the rotating electrical machine may also be a generator instead of a motor. In addition, in each figure, the XYZ coordinates represent the directional relationship in each figure. A ● mark in ○ represents the direction from the inner side of the paper toward the near front side. A × mark in ○ represents the direction from the near front side of the paper toward the inner side.
[0126] Figure 1 An example of a diagram (plan view) of a rotating electrical machine as viewed from above is shown.
[0127] exist Figure 1 In the figure, the rotating electric machine 100 includes a rotor 110, a stator 120, and a rotating shaft 130. In addition, the rotating electric machine 100 includes a known structure of the rotating electric machine 100, such as a case to which the stator 120 is fixed.
[0128] The stator 120 is relatively arranged on the outside of the rotating electric machine 100. The outer peripheral surface of the rotor 110 is relatively arranged on the inside of the rotating electric machine 100 in a manner that it is spaced from the inner peripheral surface of the stator 120. The outer peripheral surface of the rotating shaft 130 is opposite to the inner peripheral surface of the rotor 110, and is arranged at the center of the rotating electric machine 100 in a state of being directly or indirectly connected to the rotor 110. The axis O of the rotor 110 and the stator 120 coincides with the axis O of the rotating shaft 130. It should be noted that in the following description, the direction in which the rotor 110 of the rotating electric machine 100 rotates is referred to as the circumferential direction as needed. The height direction of the rotating electric machine 100 (equal to the stacking direction of the electromagnetic steel sheets) is referred to as the height direction as needed. The direction perpendicular to the height direction, that is, the direction in which the axis O passes, is referred to as the radial direction as needed.
[0129] The stator 120 has a stator core and a winding. The stator core has a yoke extending in the circumferential direction and a plurality of teeth extending from the inner circumference of the yoke toward the axial direction. The plurality of teeth are arranged at equal intervals in the circumferential direction. Figure 1 In the example, there are six teeth and the stator 120 has six poles. A winding is wound on the stator core. The winding method of the winding wound on the stator core is concentrated winding. The stator 120 can be implemented with a known structure.
[0130] Figure 2 FIG. 1 is a schematic diagram showing an example of the structure of the rotor 110 . Figure 2 (a) is an example of a view (plan view) of the rotor 110 viewed from above. Figure 2 (a) is to pull out Figure 1 The part of the rotor 110 is obtained. Figure 2 (b) Figure 2 (a) Section II.
[0131] The rotor 110 has a rotor core 111. The rotor core 111 is formed by punching Figure 2 (a) A plurality of electromagnetic steel sheets of the shape shown in FIG. Figure 2 (a) and Figure 2 As shown in (b), the plurality of electromagnetic steel sheets are stacked to match the outer edges of the plurality of electromagnetic steel sheets. The surface of the plurality of electromagnetic steel sheets is subjected to insulation treatment. The plurality of electromagnetic steel sheets are fixed, for example, by riveting or using an adhesive. It should be noted that, for example, the electromagnetic steel sheets can also be processed into Figure 2 (a) is used instead of punching. It should be noted that the rotor core 111 is not divided in the circumferential direction.
[0132] The rotor core 111 has a yoke extending in the circumferential direction and a plurality of salient poles extending (radially) from the outer circumferential side of the yoke in a direction opposite to the axial direction (toward the stator 120 ). The plurality of salient poles are arranged at equal intervals in the circumferential direction. The plurality of salient poles are magnetic poles of the rotor core 111 . Figure 2 (a) has four salient poles. In this embodiment, a case where the rotor 110 has four poles is described as an example.
[0133] Figure 3 FIG. 1 is a schematic diagram showing an example of the positional relationship of electromagnetic steel sheets constituting rotor core 111 with respect to the rolling direction.
[0134] Figure 3 FIG. 1 shows one of the plurality of electromagnetic steel sheets constituting the rotor core 111. The electromagnetic steel sheet 300 is formed by punching a hoop (parent material) into Figure 2 At this time, among all the electromagnetic steel sheets 300 constituting the rotor core 111, each salient pole ( Figure 2 The positional relationship of the regions of the four salient poles in the example shown in (a) relative to the rolling direction is the same.
[0135] The positional relationship of the regions constituting the magnetic poles (salient poles) of the electromagnetic steel sheet 300 with respect to the rolling direction is represented by, for example, the angle between the rolling direction and the center line of the regions constituting the magnetic poles of the electromagnetic steel sheet 300 .
[0136] exist Figure 3 In FIG. 1 , the virtual line 310 represented by a single-dot chain line is the rolling direction of the electromagnetic steel sheet 300. The virtual lines 320a to 320b represented by a dotted line are the center lines of the magnetic pole (salient pole) region constituting the electromagnetic steel sheet 300. Here, an example is given to illustrate the case where the magnetic characteristics of the electromagnetic steel sheet 300 coincide with the best direction. The center lines 320a to 320b of the region constituting the magnetic pole of the electromagnetic steel sheet 300 are straight lines extending in a direction parallel to the plate surface of the electromagnetic steel sheet 300 (a direction perpendicular to the height direction (Z-axis direction)), and are imaginary straight lines passing through the axis O of the electromagnetic steel sheet 300 (rotor core 111) and the center of the circumferential direction of the region constituting the magnetic pole. In this way, in the present embodiment, an example is given to illustrate the case where the center lines 320a to 320b of all the regions constituting the magnetic pole of the electromagnetic steel sheet 300 coincide with any direction of the direction in which the magnetic characteristics of the electromagnetic steel sheet 300 are best. In the following description, the direction with the best magnetic characteristics is referred to as the easy magnetization direction as needed.
[0137] exist Figure 3In the example shown, when punching any hoop (parent material), the angle between the rolling direction 310 and the center line 320a-320b is the same. In this way, for example, the position of the die for the hoop (parent material) can be set to a certain level for punching. By punching the hoop (parent material) in this way, a plurality of electromagnetic steel sheets 300 constituting the rotor core 111 can be obtained. That is, the electromagnetic steel sheets constituting the rotor core 111 are all aligned with the center line 320a-320b. Figure 3 The electromagnetic steel sheets 300 shown are the same. In any of the electromagnetic steel sheets 300, the center lines 320a and 320b of the regions constituting the magnetic poles of the electromagnetic steel sheets 300 coincide with one of the two easy magnetization directions ED1 and ED2.
[0138] As described above, the two directions that form an angle of 45° with the rolling direction 310 are the easy magnetization directions ED1 to ED2. It should be noted that, as described above, the angles in the direction from the X-axis toward the Y-axis (counterclockwise toward the paper) and the direction from the Y-axis toward the X-axis are both positive angles. In addition, the angles formed by the two directions are both the smaller angles.
[0139] Figure 2 In the example shown in (a), four magnetic poles (salient poles) are arranged at equal intervals in the circumferential direction. Therefore, the angle (center angle) formed by the center lines of two magnetic poles that are spaced apart and located adjacent to each other in the circumferential direction is 90° (=360÷4). It should be noted that the easy magnetization directions ED1~ED2 are the easy magnetization directions passing through the axis O among the easy magnetization directions existing in the electromagnetic steel sheet 300. In addition, the center line of the magnetic pole is the center line of the magnetic pole in the circumferential direction, which is a radial extension axis and is the same as the center line 320a~320b of the magnetic pole region constituting the electromagnetic steel sheet 300. In addition, the angle formed by the easy magnetization directions ED1 and ED2 is 90°.
[0140] Therefore, for example, by stacking a plurality of electromagnetic steel sheets 300 so that the easy magnetization directions ED1 and ED2 are aligned, it is possible to make one of the two easy magnetization directions ED1 and ED2 coincide with the center lines of all the magnetic poles (salient poles) of the rotor core 111 at all positions in the height direction where the electromagnetic steel sheets 300 are arranged. In the present embodiment, for example, the easy magnetization directions ED1 and ED2 correspond to the first direction and the second direction.
[0141] As described above, in this embodiment, by aligning all easy magnetization directions with the center line of the magnetic pole (salient pole), the magnetic properties of the rotor core 111 can be improved (the easy magnetization direction of the area located at the magnetic pole and the center line of the area are represented by dotted lines 320a to 320b (= ED1 to ED2)). Therefore, the magnetic properties of the rotor core 111 become optimal.
[0142] In addition, in the present embodiment, the number of electromagnetic steel sheets 300 whose easy magnetization direction ED1 or ED2 coincides with the center line of the magnetic pole is the same in all magnetic poles (salient poles) of the rotor core 111. Thus, the magnetic characteristics of the rotor core 111 in the circumferential direction can be made uniform. As described above, in the present embodiment, at all positions in the height direction of the electromagnetic steel sheets 300, one of the two easy magnetization directions ED1 and ED2 is made to coincide with the center line of all magnetic poles of the rotor core 111. Thus, the number of electromagnetic steel sheets 300 whose easy magnetization direction ED1 or ED2 coincides with the center line of each magnetic pole is the same as the number of electromagnetic steel sheets 300 constituting the rotor core 111. For example, the number of electromagnetic steel sheets 300 constituting the rotor core 111 is 100. In this case, the number of electromagnetic steel sheets 300 whose easy magnetization direction ED1 or ED2 coincides with the center line of the magnetic pole is the same and is 100 in all magnetic poles of the rotor core 111. That is, the number of electromagnetic steel sheets 300 whose easy magnetization direction coincides with the center line of the magnetic pole is counted for each magnetic pole, and the counted number is the same as 100 for each magnetic pole.
[0143] In addition, as described in the item (Electromagnetic Steel Sheet for Rotor Core), the rotor core 111 is subjected to final annealing and stress relief annealing.
[0144] Calculation Example
[0145] Next, a calculation example will be described.
[0146] In this calculation example, the rotating electrical machine to be calculated is a switched reluctance motor. The number of poles of the rotor is 4 and the number of poles of the stator is 6. The outer diameter of the rotor core is 90 mm and the height (thickness) is 75 mm. The outer diameter of the stator core is 160 mm, the inner diameter is 90.6 mm, and the height (thickness) is 75 mm. A DC voltage of 150 V is applied to each phase of the stator, and at the same time, the rotor rotates at a speed of 600 rpm.
[0147] As the electromagnetic steel sheet for the rotor core of the rotating electric machine, the electromagnetic steel sheet described in the item (Electromagnetic steel sheet for the rotor core) and the known non-oriented electrical steel sheet are used. The thickness of any electromagnetic steel sheet is 0.25 mm. As the known non-oriented electromagnetic steel sheet, a non-oriented electromagnetic steel sheet with W10 / 400 of 12.8 W / kg is used. W10 / 400 is the iron loss when the magnetic flux density is 1.0 T and the frequency is 400 Hz. In addition, the known non-oriented electromagnetic steel sheet has good magnetic properties only in the rolling direction.
[0148] The electromagnetic steel sheet described in the item (electromagnetic steel sheet for rotor core) is referred to as Figure 2 (a) The method described is punched.
[0149] The stator core formed by stacking the punched electromagnetic steel sheets described in the section (Electromagnetic Steel Sheets for Rotor Core) with their easy magnetization directions aligned is the stator core to be analyzed for the first time.
[0150] In addition, the known non-oriented electrical steel sheet is punched out in the following manner: That is, the positional relationship of each region of the rotor core with respect to the rolling direction is the same as that of the electromagnetic steel sheet described in the item (Electromagnetic steel sheet for rotor core).
[0151] A rotor core formed by stacking known non-oriented electrical steel sheets punched out in this manner with the rolling directions aligned is used as a stator core for the second analysis object.
[0152] The rotors of the first and second analysis objects are used as the rotating electric machines of the size and shape as the calculation objects. Furthermore, numerical analysis (computer simulation) is performed by the finite element method to derive the average torque of the rotor core of the first and second analysis objects when each rotating electric machine is operated under the above conditions. It should be noted that the numerical analysis uses the finite element method electromagnetic field analysis software JMAG manufactured by JSOL Co., Ltd. The results are shown in Table 5.
[0153] Table 5
[0154] Average torque Development Materials 1.010 Existing Materials 1.000
[0155] In Table 5, the developed material shows the results of the first analysis object with respect to the starter movement. The existing material shows the results of the second analysis object with respect to the starter movement. The values shown in Table 5 are relative values when the values of the existing material are 1.000.
[0156] As shown in Table 5, the average torque increased by 1.0% when the electromagnetic steel sheet (developed material) described in the item (electromagnetic steel sheet for rotor core) was used compared to the case where the known non-oriented electrical steel sheet (existing material) was used. In this way, by stacking the electromagnetic steel sheets described in the item (electromagnetic steel sheet for rotor core), the torque of the rotor core can be increased.
[0157] Summarize
[0158] In the present embodiment as described above, the electromagnetic steel sheet 300 is formed in such a manner that the center lines of the four magnetic poles (salient poles) of the rotor core 111 coincide with the easy magnetization direction ED1 or ED2. Furthermore, the electromagnetic steel sheets 300 are stacked in such a manner that the easy magnetization directions ED1 and ED2 are aligned. Thus, the electromagnetic steel sheets can be stacked so that the magnetic characteristics in the circumferential direction of the rotor core 111 are as uniform as possible and the uniformized magnetic characteristics are as good as possible. Thus, even if the magnitude of the current flowing through the stator coil is reduced, it is possible to generate the required torque and reduce the copper loss of the rotating electric machine (stator).
[0159] Modifications
[0160] <Variation 1>
[0161] In this embodiment, the case where a plurality of electromagnetic steel sheets 300 are stacked while aligning (the two directions of) the easy magnetization directions ED1 and ED2 is described as an example. However, since the magnetic properties of the two easy magnetization directions ED1 and ED2 are theoretically the same, this is not necessary if the rolling direction 310 is aligned. In this case, the plurality of electromagnetic steel sheets 300 are stacked while aligning the easy magnetization directions ED1 or ED2 without distinguishing between the easy magnetization directions ED1 and ED2.
[0162] <Variation 2>
[0163] In this embodiment, an inner rotor type rotating electrical machine is described as an example. However, an outer rotor type rotating electrical machine may also be used. It should be noted that the rotating electrical machine may also be a motor (engine) or a generator.
[0164] (Second embodiment)
[0165] Next, the second embodiment will be described. In the first embodiment, an example was given in which the rotating electrical machine is a switched reluctance motor. In contrast, in the present embodiment, an example is given in which the rotating electrical machine is a synchronous reluctance motor. As described above, the main difference between the present embodiment and the first embodiment is that the rotor core to which the electromagnetic steel sheet described in the item (electromagnetic steel sheet for rotor core) is applicable is different. Therefore, in the description of the present embodiment, the same part as the first embodiment is appended with the same Figure 1 to Figure 3 The same symbols etc. are used and detailed description thereof is omitted.
[0166] Figure 4 Schematic diagram of the structure of an exemplary rotating electrical machine. As described above, in this embodiment, the rotating electrical machine is described as a synchronous reluctance motor. It should be noted that the rotating electrical machine may be a generator instead of a motor.
[0167] Figure 4 An example of a diagram (plan view) of a rotating electrical machine as viewed from above is shown.
[0168] exist Figure 4 In the figure, the rotating electric machine 400 includes a rotor 410, a stator 420, and a rotating shaft 430. In addition, the rotating electric machine 400 includes a known structure of the rotating electric machine 400, such as a housing to which the stator 420 is fixed.
[0169] The stator 420 is relatively arranged on the outside of the rotating electric machine 400. The outer peripheral surface of the rotor 410 is relatively arranged on the inside of the rotating electric machine 400 in a manner that it is spaced from the inner peripheral surface of the stator 420. The outer peripheral surface of the rotating shaft 430 is opposite to the inner peripheral surface of the rotor 410, and is arranged at the center of the rotating electric machine 400 in a state of being directly or indirectly connected to the rotor 410. The axis O of the rotor 410 and the stator 420 is consistent with the axis O of the rotating shaft 430.
[0170] The stator 420 has a stator core and a winding. The stator core has a yoke extending in the circumferential direction and a plurality of teeth extending from the inner circumference of the yoke toward the axial direction. The plurality of teeth are arranged at equal intervals in the circumferential direction. Figure 4 In the example, there are 6 teeth and the stator 420 has 6 poles. The stator core is wound with windings. The winding method of the winding wound on the stator core is distributed winding. The stator 420 can be implemented by known materials.
[0171] Figure 5 FIG. 4 is a schematic diagram showing an example of the structure of the rotor 410 . Figure 5 An example of a view (plan view) of the rotor 410 viewed from above is shown. It should be noted that: Figure 5 To pull out Figure 4 portion of the rotor 410 . Figure 6 A schematic cross-sectional view of a rotor core. Figure 6 (a) Figure 5 (a) Section II, Figure 6 (b) Figure 5 (b) II-II cross-section.
[0172] The rotor 410 has a rotor core 411. The rotor core 411 is formed by punching Figure 5 A plurality of electromagnetic steel sheets of the shape shown in Figure 5 , Figure 6 (a) and Figure 6 As shown in (b), the plurality of electromagnetic steel sheets are stacked so that the outer edges of the plurality of electromagnetic steel sheets are aligned with the slits 510a to 510f. The surface of the plurality of electromagnetic steel sheets is subjected to insulation treatment. It should be noted that laser processing may be used instead of punching to process the electromagnetic steel sheets into Figure 5 It should be noted that the rotor core 411 is not divided in the circumferential direction.
[0173] The rotor core 411 has a substantially hollow cylindrical shape with a plurality of slits 510a to 510l extending therethrough in the height direction (Z-axis direction). As described in Patent Document 2, the plurality of slits 510a to 510l may be provided with metal, insulating resin, or conductive rods.
[0174] The slits 510a, 510d, 510g, and 510j have the same shape and size. The slits 510b, 510e, 510h, and 510k have the same shape and size. The slits 510c, 510f, 510i, and 510l have the same shape and size.
[0175] The slits 510a, 510d, 510g, and 510j are arranged at positions closer to the outer peripheral surface of the rotor core 411 than the other slits 510b, 510c, 510e, 510f, 510h, 510i, 510k, and 510l. The slits 510c, 510f, 510i, and 510l are arranged at positions closer to the axis O of the rotor core 411 than the other slits 510a, 510b, 510d, 510e, 510g, 510h, 510j, and 510k. The slits 510b, 510e, 510h, and 510k are arranged between the slits 510a and 510c, between the slits 510d and 510f, between the slits 510g and 510i, and between the slits 510j and 510l, respectively.
[0176] The planar shape of the slits 510a to 510l has a curved shape from the center in the length direction toward both ends and close to the outer peripheral surface of the rotor core 411 when viewed from the height direction (Z-axis direction). The center in the length direction of the slits 510a to 510l is closest to the axis O of the rotor core 411, and the two ends in the length direction are closest to the outer peripheral surface of the rotor core 411.
[0177] If slits 510a~510c are the first slit group, slits 510d~510f are the second slit group, slits 510g~510i are the third slit group, and slits 510j~510l are the fourth slit group, then the first slit group, the second slit group, the third slit group, and the fourth slit group are arranged at equal intervals of 90° in the circumferential direction, that is, they are configured in a four-fold symmetrical relationship with the axis O of the rotor core 411 as the rotation axis.
[0178] The position of the outer circumference of the rotor core 411, i.e., the middle position 520a between the slits 510c and 510f, the position of the outer circumference of the rotor core 411, i.e., the middle position 520b between the slits 510f and 510l, the position of the outer circumference of the rotor core 411, i.e., the middle position 520c between the slits 510i and 510l, and the position of the outer circumference of the rotor core 411, i.e., the middle position 520d between the slits 510c and 510i are the circumferential center positions of the magnetic poles. Figure 5 In the example shown, the direction along the line connecting the positions 520a to 520d and the axis O is the longitudinal direction of the magnetic pole. As described above, in this embodiment, the case where the rotor 410 has four poles is described as an example.
[0179] It should be noted that the number or shape of the slits is not limited to Figure 5 , Figure 6 (a) Figure 6 (b) The situation shown.
[0180] Figure 7 FIG. 4 is a schematic diagram showing an example of the positional relationship of electromagnetic steel sheets constituting the rotor core 411 with respect to the rolling direction.
[0181] Figure 7 FIG. 4 shows one of the plurality of electromagnetic steel sheets constituting the rotor core 411. The electromagnetic steel sheet 700 is formed by punching a hoop (parent material) into Figure 5 At this time, in all the electromagnetic steel sheets 700 constituting the rotor core 411, the regions constituting the magnetic poles (the circumferential center positions 520a to 520d) of the electromagnetic steel sheets 700 are made to have the same positional relationship with respect to the rolling direction.
[0182] The positional relationship of the regions constituting the magnetic poles of the electromagnetic steel sheet 700 with respect to the rolling direction is expressed, for example, by the angle formed by the rolling direction and the center line of the regions constituting the magnetic poles of the electromagnetic steel sheet 700 .
[0183] exist Figure 7 , the virtual line 710 indicated by a single-dot chain line is the rolling direction of the electromagnetic steel sheet 700. The virtual lines 720a to 720b indicated by dotted lines are the center lines of the magnetic pole regions constituting the electromagnetic steel sheet 700, and an example is given here of a case where the center lines 720a to 720b of the regions constituting the magnetic poles of the electromagnetic steel sheet 700 are virtual straight lines extending in a direction parallel to the plate surface of the electromagnetic steel sheet 700 (a direction perpendicular to the height direction (Z-axis direction)), and are virtual straight lines passing through the axis O of the electromagnetic steel sheet 700 (rotor core 411) and the center positions 520a to 520d of the circumferential direction of the regions. Thus, in this embodiment, an example is given of a case where the center lines 720a to 720b of all the regions constituting the magnetic poles of the electromagnetic steel sheet 700 are consistent with one of the easy magnetization directions of the electromagnetic steel sheet 700.
[0184] exist Figure 7 In the example shown, when punching any hoop (parent material), the angle between the rolling direction 710 and the center line 720a-720b is made the same. In this way, for example, the punching process can be performed by setting the positional relationship of the die to the hoop (parent material) to be constant. By punching the hoop (parent material) in this way, a plurality of electromagnetic steel sheets 700 constituting the rotor core 411 can be obtained. That is, the electromagnetic steel sheets constituting the rotor core 411 are all Figure 7The electromagnetic steel sheets 700 shown are the same. In any of the electromagnetic steel sheets 700, the center lines 720a and 720b of the regions constituting the magnetic poles of the electromagnetic steel sheets 700 coincide with one of the two easy magnetization directions ED1 and ED2.
[0185] As described above, the two directions that form an angle of 45° with the rolling direction 710 are the easy magnetization directions ED1 to ED2. It should be noted that, as described above, the angles in the direction from the X-axis toward the Y-axis (counterclockwise toward the paper surface) and the direction from the Y-axis toward the X-axis are both positive angles. In addition, the angles formed by the two directions are both the smaller angles.
[0186] exist Figure 5 In the example shown, four magnetic poles are arranged at equal intervals in the circumferential direction. Therefore, the angle (center angle) formed by the center lines of two magnetic poles that are spaced apart and located adjacent to each other in the circumferential direction is 90° (=360÷4). It should be noted that the easy magnetization directions ED1~ED2 are the easy magnetization directions passing through the axis O among the easy magnetization directions existing in the electromagnetic steel sheet 700. In addition, the center line of the magnetic pole is the center line of the magnetic pole in the circumferential direction, which is the radial extension axis and is the same as the center line 720a~720b of the magnetic pole area constituting the electromagnetic steel sheet 700. In addition, the angle formed by the easy magnetization directions ED1 and ED2 is 90°.
[0187] Therefore, for example, by stacking a plurality of electromagnetic steel sheets 700 with the easy magnetization directions ED1 and ED2 aligned, it is possible to make any one of the two easy magnetization directions ED1 and ED2 coincide with the center lines of the magnetic poles of all rotor cores 411 at all positions in the height direction where the electromagnetic steel sheets 700 are arranged. In the present embodiment, for example, the easy magnetization directions ED1 and ED2 correspond to the first direction and the second direction.
[0188] As described above, in this embodiment, similar to the first embodiment, all easy magnetization directions are aligned with the center line of the magnetic pole, thereby making the magnetic properties of the rotor core 411 excellent (the easy magnetization directions in the magnetic pole region and the center line of the region are indicated by dotted lines 720a to 720b). Therefore, the magnetic properties of the rotor core 411 are optimized.
[0189] In addition, in the present embodiment, the number of electromagnetic steel sheets 700 whose easy magnetization direction ED1 or ED2 is aligned with the center line of the magnetic pole is the same in all the magnetic poles of the rotor core 411. Therefore, the magnetic characteristics in the circumferential direction of the rotor core 411 can be made uniform. As described above, in the present embodiment, one of the two easy magnetization directions ED1 and ED2 is aligned with the center line of all the magnetic poles of the rotor core 411 at all positions in the height direction where the electromagnetic steel sheets 700 are arranged. Therefore, the number of electromagnetic steel sheets 700 whose easy magnetization direction ED1 or ED2 is aligned with the center line of each magnetic pole is the same as the number of electromagnetic steel sheets 700 constituting the rotor core 411. For example, the number of electromagnetic steel sheets 700 constituting the rotor core 411 is 100. In this case, the number of electromagnetic steel sheets 700 whose easy magnetization direction ED1 or ED2 is aligned with the center line of the magnetic pole is the same as 100 in all the magnetic poles of the rotor core 411.
[0190] In addition, as described in the item (Electromagnetic steel sheet for rotor core), the rotor core 411 is subjected to final annealing and stress relief annealing.
[0191] Summarize
[0192] As described above, the rotor core of the synchronous reluctance motor is also the same as the rotor core of the switched reluctance motor described in the first embodiment, and can be applied to the electromagnetic steel sheets described in the section (Electromagnetic steel sheets used for rotor core) and achieve the same effects as described in the first embodiment.
[0193] Modifications
[0194] It should be noted that the form of the rotor core is not limited to that described in the present embodiment, and a known rotor core used in a synchronous reluctance motor may be used.
[0195] In addition, in this embodiment, various modifications described in the first embodiment can be adopted.
[0196] (Third embodiment)
[0197] Next, the third embodiment is described. In the first embodiment, the case where the rotor core 111 has four magnetic poles is described as an example. In contrast, in this embodiment, the case where the rotor core has more than four magnetic poles is described. Thus, the main difference between this embodiment and the first embodiment is that the structure is different due to the different number of poles of the rotating electrical machine. Therefore, in the description of this embodiment, the same parts as the first embodiment are attached with the same Figure 1 to Figure 3 The same symbols are used and their detailed description is omitted.
[0198] Figure 8 A schematic diagram of the structure of an exemplary rotating electrical machine. Figure 8An example of a diagram (plan view) of a rotating electrical machine as viewed from above is shown.
[0199] exist Figure 8 In the figure, the rotating electric machine 800 includes a rotor 810, a stator 820, and a rotating shaft 830. In addition, the rotating electric machine 800 includes a known structure of the rotating electric machine 800, such as a housing to which the stator 820 is fixed.
[0200] The stator 820 is relatively arranged on the outside of the rotating electric machine 800. The outer peripheral surface of the rotor 810 is relatively arranged on the inside of the rotating electric machine 800 in a manner that it is spaced from the inner peripheral surface of the stator 820. The outer peripheral surface of the rotating shaft 830 is opposite to the inner peripheral surface of the rotor 810, and is arranged at the center of the rotating electric machine 800 in a state of being directly or indirectly connected to the rotor 810. The axis O of the rotor 810 and the stator 820 is consistent with the axis O of the rotating shaft 830.
[0201] The stator 820 has a stator core and a winding. The stator core has a yoke extending in the circumferential direction and a plurality of teeth extending from the inner circumference of the yoke toward the axial direction. The plurality of teeth are arranged at equal intervals in the circumferential direction. Figure 8 In the example, a case where there are 8 teeth and the stator 820 has 8 poles is described. A winding is wound on the stator core. The winding method of the winding wound on the stator core is concentrated winding. The stator 820 can be realized by a known material.
[0202] Fig. 9 FIG. 8 is a schematic diagram showing an example of the structure of the rotor 810 . Fig. 9 (a) is an example of a view (plan view) of the rotor 810 viewed from above. Fig. 9 (a) is to pull out Figure 8 The rotor 810 part is obtained. Fig. 9 (b) Fig. 9 (a) Section II.
[0203] The rotor 810 has a rotor core 811. The rotor core 811 is formed by punching Fig. 9 (a) A plurality of electromagnetic steel sheets of the shape shown in FIG. Fig. 9 (a) and Fig. 9 As shown in (b), the plurality of electromagnetic steel sheets are stacked in such a manner that the outer edges thereof are aligned. The surface of the plurality of electromagnetic steel sheets is subjected to insulation treatment. It should be noted that, for example, the electromagnetic steel sheets may be processed into Fig. 9 (a) is used instead of punching. It should be noted that the rotor core 811 is not divided in the circumferential direction.
[0204] The rotor core 811 has a yoke extending in the circumferential direction and a plurality of salient poles extending radially from the outer circumferential side of the yoke in the opposite direction of the axial direction (stator 820 side). The plurality of salient poles are arranged at equal intervals in the circumferential direction. The plurality of salient poles constitute the magnetic pole portion of the rotor core 811. Fig. 9 (a) has six salient poles. Thus, in this embodiment, the case where the rotor 810 has six poles is described as an example.
[0205] Fig. 10A FIG. 8 is a schematic diagram showing an example of the positional relationship of the electromagnetic steel sheets constituting the rotor core 811 with respect to the rolling direction.
[0206] Fig. 10A FIG. 8 is a diagram showing one of the plurality of electromagnetic steel sheets constituting the rotor core 811. As described above, the electromagnetic steel sheet 1000 is formed by punching a hoop (parent material) into Fig. 9 At this time, among all the electromagnetic steel sheets 1000 constituting the rotor core 811, each salient pole ( Fig. 9 The positional relationship of the regions of the six salient poles in the example shown in (a) relative to the rolling direction is the same.
[0207] The positional relationship of the regions constituting each magnetic pole (salient pole) of the electromagnetic steel sheet 1000 with respect to the rolling direction is represented by, for example, the angle formed by the rolling direction and the center line of the region constituting each magnetic pole of the electromagnetic steel sheet 1000 .
[0208] exist Fig. 10A , the virtual line 1010 represented by a single-point chain line is the rolling direction of the electromagnetic steel sheet 1000. The virtual lines 1020a~1020c represented by dotted lines are the center lines of the area constituting the magnetic poles (salient poles) of the electromagnetic steel sheet 1000. The center lines 1020a~1020c of the magnetic pole area constituting the electromagnetic steel sheet 1000 are determined in the manner described in the first embodiment. In the first embodiment, since the magnetic poles of the rotor core 111 are 4 poles, the center lines 320a~320b of the area constituting the magnetic poles of the electromagnetic steel sheet 300 are 2, but in this embodiment, since the magnetic poles of the rotor core 811 are 6 poles, the center lines 1020a~1020c of the magnetic pole area constituting the electromagnetic steel sheet 1000 are 3.
[0209] exist Fig. 10A In the example shown, when punching any hoop (parent material), the angle between the rolling direction 1010 and the center line 1020a to 1020c is the same. For example, the punching process can be performed by setting the positional relationship of the die to the hoop (parent material) to be constant. By punching the hoop (parent material) in this way, a plurality of electromagnetic steel sheets 1000 constituting the rotor core 811 can be obtained. That is, the electromagnetic steel sheets constituting the rotor core 811 are all at the same angle as the center line 1020a to 1020c. Fig. 10A The electromagnetic steel sheets 1000 shown are the same.
[0210] Fig. 10B Schematic diagram showing an example of a rolling direction 1010 of an electromagnetic steel sheet 1000 and a direction with the best magnetic properties (easy magnetization direction).
[0211] exist Fig. 10B In the figure, the imaginary lines ED1 to ED2 of the dotted lines are the easy magnetization directions of the electromagnetic steel sheet 1000. As described above, the two directions at an angle of 45° formed by the rolling direction 1010 are easy magnetization directions. It should be noted that, as described above, the angles in either the direction from the X-axis toward the Y-axis (counterclockwise toward the paper) and the direction from the Y-axis toward the X-axis are all positive angles. In addition, the angles formed by the two directions are both smaller angles.
[0212] exist Fig. 10B In the example shown, the easy magnetization directions ED1 and ED2 are two directions with the best magnetic properties. It should be noted that the easy magnetization directions ED1 and ED2 are easy magnetization directions existing in the easy magnetization directions of the electromagnetic steel sheet 1000 and passing through the axis O. Figure 8 In the example shown, six magnetic poles (salient poles) are arranged at equal intervals in the circumferential direction. Thus, the angle (center angle) formed by the center lines of two magnetic poles that are spaced apart and located adjacent to each other in the circumferential direction is 60° (=360÷6). It should be noted that the center line of the magnetic pole is the same as the center lines 1020a~1020c of the magnetic pole region constituting the electromagnetic steel sheet 1000. On the other hand, the angle formed by the easy magnetization directions ED1 and ED2 is 90°. Thus, it is impossible to make the two easy magnetization directions ED1 and ED2 consistent with the center lines 1020a~1020c of the magnetic pole region constituting the electromagnetic steel sheet 1000. Thus, of the two easy magnetization directions ED1 and ED2, one easy magnetization direction ED1 is made consistent with the center line of the magnetic pole, but it is impossible to make the region of the remaining one easy magnetization direction ED2 consistent with the center line of the magnetic pole.
[0213] exist Fig. 10B In the example shown, magnetic poles (salient poles) exist at positions facing each other across the axis O of the electromagnetic steel sheet 1000 (rotor core 811). Therefore, in one electromagnetic steel sheet 1000, the easy magnetization direction ED1 coincides with the center line of the two magnetic poles.
[0214] On the other hand, for example, when the number of magnetic poles is 5, there is no magnetic pole at positions facing each other across the axis of the electromagnetic steel plate (rotor core). In this case, the easy magnetization direction coincides with the center line of only one magnetic pole.
[0215] In addition, Fig. 10BIn the example shown, the easy magnetization direction ED1 coincides with the center lines of two magnetic poles in one electromagnetic steel sheet 1000. In contrast, when the number of magnetic poles is greater than 4 and is a multiple of 4 (e.g., 8), the easy magnetization directions ED1 and ED2 coincide with the center lines of the four magnetic poles.
[0216] In the present embodiment as described above, as many easy magnetization directions as possible are made to coincide with the center lines of as many magnetic poles as possible, thereby making the magnetic characteristics of the rotor core 811 as good as possible.
[0217] In this embodiment, as in the first embodiment, at all positions in the height direction of the configuration of the electromagnetic steel sheet 1000, one of the two easy magnetization directions ED1-ED2 cannot be made consistent with the center line of all the magnetic poles (salient poles) of the rotor core 811. Therefore, as in the first embodiment, if the electromagnetic steel sheets 1000 are stacked while aligning the easy magnetization directions ED1-ED2, the magnetic properties of the two magnetic poles (salient poles) regions whose center lines coincide with the easy magnetization directions ED1-ED2 are particularly good compared to the magnetic properties of the other magnetic pole regions. Therefore, the magnetic properties will be greatly uneven in the circumferential direction of a specific rotor core 811. Therefore, in order to make the magnetic properties as uniform as possible in the circumferential direction of the rotor core 811, the electromagnetic steel sheets 1000 are rotated and stacked.
[0218] Rotation stacking is to stack electromagnetic steel sheets while rotating them at a predetermined angle, with the axis O of the rotor core (electromagnetic steel sheet) as the rotation axis in a certain direction, with one electromagnetic steel sheet or multiple electromagnetic steel sheets aligned in a reference direction as a unit. The predetermined angle is generally fixed, but it may not be fixed. By performing rotation stacking, multiple electromagnetic steel sheets are stacked in a state where the easy magnetization directions are offset.
[0219] If the number of magnetic poles (salient poles) whose center lines coincide with the easy magnetization direction ED1 or ED2 of at least one electromagnetic steel sheet 1000 in the rotor core 811 is greater than the number of magnetic poles (salient poles) whose center lines coincide with the easy magnetization direction ED1 or ED2 in one electromagnetic steel sheet 1000, the method of rotating the stacking is not limited. Fig. 10B In the example shown, in one electromagnetic steel sheet 1000, the number of magnetic poles (salient poles) whose center lines coincide with the easy magnetization direction ED1 or ED2 is 2 (see Fig. 10B In this case, the number of magnetic poles (salient poles) whose center lines coincide with the easy magnetization direction ED1 or ED2 of at least one electromagnetic steel sheet 1000 may be 3 or more.
[0220] However, it is preferred that there is at least one electromagnetic steel sheet 1000 whose easy magnetization direction ED1 or ED2 coincides with the center line of the magnetic pole in all the magnetic poles (salient poles) of the rotor core 811. That is, when counting the number of electromagnetic steel sheets 1000 whose easy magnetization direction ED1 or ED2 coincides with the center line of the magnetic pole for each magnetic pole of the rotor core 811, it is preferred that the counted number is 1 or more in any magnetic pole. This is because the magnetic characteristics in the circumferential direction of the rotor core 811 can be made uniform. In addition, it is preferred that the number of electromagnetic steel sheets 1000 whose easy magnetization direction ED1 or ED2 coincides with the center line of the magnetic pole in all the magnetic poles (salient poles) whose center lines coincide with the easy magnetization direction ED1 or ED2 of at least one electromagnetic steel sheet 1000 is the same. That is, when counting the number of electromagnetic steel sheets 1000 whose easy magnetization direction ED1 or ED2 coincides with the center line of the magnetic pole for each magnetic pole of the rotor core 811, it is preferred that the counted numbers are the same. This is because the magnetic characteristics of the rotor core 811 in the circumferential direction can be made uniform. It should be noted that in this case, when the number of electromagnetic steel sheets 1000 whose easy magnetization direction ED1 or ED2 is consistent with the center line of the magnetic pole for each magnetic pole of the rotor core 811 is counted, there may be a magnetic pole whose counted number is 0. Furthermore, it is more preferred to satisfy these conditions at the same time. That is, in all the magnetic poles (salient poles) of the rotor core 811, it is preferred that the number of electromagnetic steel sheets 1000 whose easy magnetization direction ED1 or ED2 is consistent with the center line of the magnetic pole is the same. That is, for each magnetic pole of the rotor core 811, when the number of electromagnetic steel sheets 1000 whose easy magnetization direction ED1 or ED2 is consistent with the center line of the magnetic pole is counted, it is preferred that the counted number is the same number greater than 1 in any magnetic pole. Thereby, the magnetic characteristics of the rotor core 811 in the circumferential direction can be made more uniform.
[0221] Fig.11 FIG. 1 is a schematic diagram showing an example of the positional relationship of electromagnetic steel sheets 1000 in the height direction (Z-axis direction) in a rotor core 811 formed by rotational stacking.
[0222] Here, for example, the axis O of the rotor core 811 (electromagnetic steel sheet 1000) is used as the rotation axis and the rotation direction is counterclockwise toward the paper. Fig. 10A The electromagnetic steel sheets 1000 shown are stacked while rotating the reference direction of the electromagnetic steel sheets 1000 by 360°÷the number of magnetic poles of the rotor core, with one electromagnetic steel sheet 1000 as a unit. The number of magnetic poles of the rotor core 811 is 6, so the rotational stacking angle during rotational stacking is 60 (=360÷6)°.
[0223] The magnetic pole (salient pole) whose center line is aligned with the easy magnetization direction ED1 of the electromagnetic steel sheet 1000 arranged at the top (most positive direction side of the Z axis) is (A), the magnetic pole (salient pole) whose center line is aligned with the easy magnetization direction ED1 of the electromagnetic steel sheet 1000 arranged at the second position from top to bottom is (B), and the magnetic pole (salient pole) whose center line is aligned with the easy magnetization direction ED1 of the electromagnetic steel sheet 1000 arranged at the third position from top to bottom is (C). The same is true for the cases of No. 1 to No. 3 from top to bottom, and the magnetic poles (salient poles) whose center line is aligned with the easy magnetization direction ED1 of the electromagnetic steel sheet 1000 are (A), (B), and (C) from top to bottom. That is, if n is an integer greater than 1, the magnetic poles (salient poles) whose center lines coincide with the easy magnetization directions ED1 of the nth, n+1st, n+2nd, and n+3rd electromagnetic steel sheets 300 arranged from top to bottom are (A), (B), and (C), respectively.
[0224] In this way, there is at least one electromagnetic steel sheet 1000, and the easy magnetization direction ED1 or ED2 is consistent with the center line of the magnetic pole on all the magnetic poles (salient poles) of the rotor core 811. If the number of electromagnetic steel sheets 1000 constituting the rotor core 811 is a multiple of 3, the number of easy magnetization directions ED1 or ED2 that are consistent with the center line of the magnetic pole on all the magnetic poles (salient poles) of the rotor core 811 is the same. For example, the number of electromagnetic steel sheets 1000 constituting the rotor core 811 is 300. In this case, the number of electromagnetic steel sheets 1000 whose easy magnetization direction ED1 or ED2 is consistent with the center line of the magnetic pole among all the magnetic poles (salient poles) of the rotor core 811 is 100 (=300÷3).
[0225] In addition, as described in the item (Electromagnetic steel sheet for rotor core), the rotor core 811 is subjected to final annealing and stress relief annealing.
[0226] Summarize
[0227] In the present embodiment as described above, the electromagnetic steel sheets 1000 are rotated and stacked in such a manner that the number of magnetic poles (salient poles) whose center lines coincide with the easy magnetization direction ED1 or ED2 of at least one electromagnetic steel sheet 1000 in the rotor core 811 is greater than the number of magnetic poles (salient poles) whose center lines coincide with the easy magnetization direction ED1 or ED2 in one electromagnetic steel sheet 1000, so that the orientations of the easy magnetization directions ED1 and ED2 of the electromagnetic steel sheets 1000 present periodic differences in the height direction (Z-axis direction). Thus, even in a case where the region of the easy magnetization direction ED1 or ED2 cannot be made to coincide with the center lines of all the magnetic poles (salient poles) of the rotor core 811 in one electromagnetic steel sheet 1000, the magnetic characteristics in the circumferential direction of the rotor core 111 can be made as uniform as possible, and the uniformed magnetic characteristics can be made as excellent as possible.
[0228] In addition, there is at least one electromagnetic steel sheet 1000, and the easy magnetization direction ED1 or ED2 is consistent with the center line of the magnetic pole on all the magnetic poles (salient poles) of the rotor core 811. In addition, among all the magnetic poles (salient poles) whose center lines are consistent with the easy magnetization direction ED1 or ED2 of at least one electromagnetic steel sheet 1000, the number of electromagnetic steel sheets 1000 whose easy magnetization direction ED1 or ED2 is consistent with the center line of the magnetic pole is the same. By adopting at least one of these, the magnetic characteristics in the circumferential direction of the rotor core 811 can be made more uniform.
[0229] Modifications
[0230] <Variation 1>
[0231] In this embodiment, although the rotor core 811 of the switched reluctance motor is described as an example, when the number of magnetic poles of the rotor core of the synchronous reluctance motor is greater than 4, the same effect as that of the present embodiment can be obtained by rotating and stacking the electromagnetic steel sheets as described in the present embodiment. That is, the present embodiment is also applicable to the second embodiment.
[0232] <Variation 2>
[0233] As described above, the number of magnetic poles of the rotor core may not be a multiple of 4, but may be a multiple of 4. In addition, the number of magnetic poles of the rotor core may also be 4 (when the number of magnetic poles of the rotor core is 4, rotation stacking can also be performed by the method of this embodiment). Here, the magnetic properties of the easy magnetization directions ED1 and ED2 are almost the same, but not strictly the same. Therefore, when the number of magnetic poles of the rotor core is 4, the effect of uniformizing the magnetic properties in the circumferential direction of the rotor core can also be obtained by rotation stacking (but it is smaller than the case where the number of magnetic poles of the rotor core is a multiple of 4 of 8 or more). In addition, in the case where the electromagnetic steel sheet 1000 is formed by punching, for example, the alignment of the burrs formed on the electromagnetic steel sheet during the punching process can be suppressed, and the magnetic properties of the rotor core can be further improved.
[0234] <Variation 3>
[0235] The change in the orientation of the easy magnetization directions ED1 and ED2 of the electromagnetic steel sheet 1000 in the height direction (Z-axis direction) may not be periodic. For example, when the stator core 611 of the present embodiment is constructed, the rotation stacking angle may be 60°, the rotation stacking may be performed five times, and the orientation of the easy magnetization directions ED1 and ED2 of the electromagnetic steel sheet 1000 may not be restored to the original state.
[0236] In addition, in this embodiment, various modifications described in the first and second embodiments can also be adopted.
[0237] It should be noted that the embodiments of the present invention described above are only specific examples for implementing the present invention, and the technical scope of the present invention is not limited thereby. That is, the present invention can be implemented in various ways without departing from the technical concept or main features of the present invention.
[0238] Industrial Availability
[0239] According to the present invention, the magnetic characteristics of the rotor can be improved, and therefore the industrial applicability is high.
[0240] Description of Reference Numerals
[0241] 100, 400, 800: Rotating motor
[0242] 110, 410, 810: Rotor
[0243] 111, 411, 811: rotor core
[0244] 120: Stator
[0245] 300, 700, 1000: Magnetic steel sheet
[0246] 310, 710, 1010: rolling direction
[0247] ED1~ED2: easy magnetization direction
Claims
1. A rotor core, which is a rotor core of a reluctance motor or a reluctance generator, having a plurality of electromagnetic steel sheets, characterized in that: The electromagnetic steel sheet has the following chemical composition: Contains by mass %: C: 0.0100% or less, Si: 1.50% to 4.00%, Sol.Al: 0.0001%~1.0%, S: 0.0100% or less, N: 0.0100% or less, One or more selected from the group consisting of Mn, Ni, Co, Pt, Pb, Cu, and Au: 2.50% to 5.00% in total, Sn: 0.000%~0.400%, Sb: 0.000%~0.400%, P: 0.000% to 0.400%, and One or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total; When the Mn content is recorded as [Mn] in mass%, the Ni content is recorded as [Ni] in mass%, the Co content is recorded as [Co] in mass%, the Pt content is recorded as [Pt] in mass%, the Pb content is recorded as [Pb] in mass%, the Cu content is recorded as [Cu] in mass%, the Au content is recorded as [Au] in mass%, the Si content is recorded as [Si] in mass%, and the sol.Al content is recorded as [sol.Al] in mass%, the following formula (A) is satisfied: ([Mn]+[Ni]+[Co]+[Pt]+[Pb]+[Cu]+[Au])-([Si]+[sol.Al])>0%…(A) The remainder consists of Fe and impurities; When B50 in the rolling direction is represented by B50L, B50 in the direction at an angle of 90° to the rolling direction is represented by B50C, B50 in one of the two directions of 45°, the smaller of which is the angle formed with the rolling direction, and B50 in the other direction are represented by B50D1 and B50D2, respectively, the following formulas (B) and (D) are satisfied, the X-ray random intensity ratio of {100}<011> is greater than 5 and less than 30, the plate thickness is less than 0.50 mm, (B50D1+B50D2) / 2>1.7T…(B) (B50D1+B50D2) / 2>1.1×(B50L+B50C) / 2…(D).
2. A rotor core, which is a rotor core of a reluctance motor or a reluctance generator, having a plurality of electromagnetic steel sheets, characterized in that: The electromagnetic steel sheet has the following chemical composition: Contains by mass %: C: 0.0100% or less, Si: 1.50% to 4.00%, Sol.Al: 0.0001%~1.0%, S: 0.0100% or less, N: 0.0100% or less, One or more selected from the group consisting of Mn, Ni, Co, Pt, Pb, Cu, and Au: 2.50% to 5.00% in total, Sn: 0.000%~0.400%, Sb: 0.000%~0.400%, P: 0.000% to 0.400%, and One or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total; When the Mn content is recorded as [Mn] in mass%, the Ni content is recorded as [Ni] in mass%, the Co content is recorded as [Co] in mass%, the Pt content is recorded as [Pt] in mass%, the Pb content is recorded as [Pb] in mass%, the Cu content is recorded as [Cu] in mass%, the Au content is recorded as [Au] in mass%, the Si content is recorded as [Si] in mass%, and the sol.Al content is recorded as [sol.Al] in mass%, the following formula (A) is satisfied: ([Mn]+[Ni]+[Co]+[Pt]+[Pb]+[Cu]+[Au])-([Si]+[sol.Al])>0%…(A) The remainder consists of Fe and impurities; When B50 in the rolling direction is represented by B50L, B50 in the direction at an angle of 90° to the rolling direction is represented by B50C, B50 in one of the two directions of 45°, the smaller of which is the angle formed with the rolling direction, and B50 in the other direction are represented by B50D1 and B50D2, respectively, the following formulas (C) and (F) are satisfied, the X-ray random intensity ratio of {100}<011> is greater than 5 and less than 30, and the plate thickness is less than 0.50 mm, (B50D1+B50D2) / 2>(B50L+B50C) / 2…(C) (B50D1+B50D2) / 2>1.8T…(F).
3. The rotor core according to claim 1 or 2, characterized in that: Satisfies the following formula (E), (B50D1+B50D2) / 2>1.2×(B50L+B50C) / 2…(E).
4. The rotor core according to claim 1 or 2, characterized in that: The electromagnetic steel sheet contains, by mass%, 0.020% to 0.400% of Sn or 0.020% to 0.400% of Sb.
5. A rotor of a reluctance motor or a reluctance generator, comprising a rotor core according to claim 1 or 2, characterized in that: The center line of at least one magnetic pole of the rotor in the circumferential direction coincides with the direction in which the magnetic properties of at least one electromagnetic steel sheet are best; The direction with the best magnetic properties is at least one of the two directions whose smaller angle with the rolling direction is 45°.
6. The rotor according to claim 5, characterized in that The number of magnetic poles of the rotor is a multiple of 4; In a first direction of two directions in which the magnetic properties of at least one of the electromagnetic steel sheets are the best, the two magnetic poles are located at positions facing each other across the axis; In a second direction of the two directions in which the magnetic properties of at least one of the electromagnetic steel sheets are the best, the two magnetic poles are located at positions facing each other across the axis; The center lines in the circumferential direction of the two magnetic poles located at positions opposing each other across the axis in the first direction coincide with the first direction of at least one of the electromagnetic steel sheets; A center line in the circumferential direction of two of the magnetic poles located at positions opposing each other across the axis in the second direction coincides with the second direction of at least one of the electromagnetic steel sheets.
7. The rotor according to claim 6, characterized in that The number of magnetic poles of the rotor is 4; The center lines in the circumferential direction of the two magnetic poles located at positions opposing each other across the axis in the first direction coincide with the first direction of the plurality of electromagnetic steel sheets; A center line in the circumferential direction of two of the magnetic poles located at positions opposing each other across the axis in the second direction coincides with the second direction of the plurality of electromagnetic steel sheets.
8. The rotor according to claim 5, characterized in that The plurality of electromagnetic steel sheets are stacked in a state where the orientations of two directions with the best magnetic properties are shifted.
9. The rotor according to claim 5, characterized in that The plurality of electromagnetic steel sheets are stacked in a state where the orientations of the two directions with the best magnetic properties are periodically shifted in the stacking direction of the electromagnetic steel sheets.
10. The rotor according to claim 5, characterized in that Among all the magnetic poles whose circumferential center lines coincide with the direction in which at least one of the electromagnetic steel sheets has the best magnetic properties, the number of the electromagnetic steel sheets whose directions of the best magnetic properties coincide with the circumferential center lines of the magnetic poles is the same.
11. The rotor according to claim 5, characterized in that At least one of the electromagnetic steel sheets is included, and in all the magnetic poles, the direction in which the magnetic characteristics are best coincides with the center line of the circumferential direction of the magnetic pole.
12. The rotor according to claim 5, characterized in that In each of the plurality of electromagnetic steel sheets, there is at least one direction that coincides with a center line in a circumferential direction of the magnetic pole as a direction in which the magnetic characteristics are best.
13. The rotor according to claim 5, characterized in that In each of the plurality of electromagnetic steel sheets, the regions constituting the magnetic poles of the electromagnetic steel sheet have the same positional relationship with respect to the rolling direction.
14. A rotating electrical machine, characterized in that: A rotor according to any one of claims 5 to 13, which is a reluctance motor or a reluctance generator.