Polycrystalline diamond self-supporting substrate and preparation method thereof
By attaching diamond particles below 100 nm to the semiconductor substrate and growing a polycrystalline diamond layer, controlling the particle size and polishing treatment, the mechanical strength, bondability and heat dissipation of the polycrystalline diamond independent substrate is solved, and the polycrystalline diamond independent substrate is realized. Excellent performance.
Patent Information
- Application Number
- CN202111597288.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-24
- Filing Date
- 2021-12-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-12-24
AI Technical Summary
The existing polycrystalline diamond independent substrates are insufficient after removing the substrate and cannot achieve good bonding between the front and the different substrates and high heat dissipation on the back.
By attaching diamond particles with an average particle size of 100 nm or less as cores on the semiconductor substrate, a polycrystalline diamond layer of 300 μm or more was grown by CVD method, and the diamond particle sizes on the front and back sides were controlled to be 100 nm or less and 1000 nm or more respectively during the growth process. , combined with polishing treatment, a polycrystalline diamond independent substrate with excellent bonding and heat dissipation was prepared.
It realizes excellent bonding between the front and the different substrates of the polycrystalline diamond independent substrate and high heat dissipation on the back, and is suitable for the production of high-frequency devices or power devices.
Smart Images

Figure CN114672879B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polycrystalline diamond self-supporting substrate and a preparation method thereof. Background Art
[0002] Polycrystalline diamond self-supporting substrates have attracted attention as substrates for manufacturing high-voltage semiconductor devices such as high-frequency devices and power devices.
[0003] Patent document 1 records that a polycrystalline diamond layer with a thickness of 5 to 2000 μm is grown on a substrate by a chemical vapor deposition method (CVD method), and then the substrate is removed to make the polycrystalline diamond layer into a self-supporting substrate. Patent document 1 records that by containing nitrogen in the atmosphere during film formation, the particle size of the diamond particles will not increase with the increase of the film thickness, thereby forming a polycrystalline diamond layer with a particle size of less than 1 μm on both the growth surface and the inside. Therefore, if the substrate is removed after the polycrystalline diamond layer is formed, a polycrystalline diamond self-supporting substrate with a particle size of less than 1 μm on both sides should be obtained.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent document 1: Japanese Patent Application Laid-Open No. 7-172988. Summary of the invention
[0007] Problems to be solved by the invention
[0008] However, in Patent Document 1, since the thickness of the polycrystalline diamond layer is as thin as 5 to 2000 μm, sufficient mechanical strength cannot be obtained as a self-supporting substrate, and the polycrystalline diamond layer will break after the substrate is removed. In addition, even when a thick polycrystalline diamond layer is formed to obtain sufficient mechanical strength as a self-supporting substrate, the inventors still recognize the following problems.
[0009] It is assumed that a heterogeneous substrate is attached to one side of a polycrystalline diamond self-supporting substrate, and a semiconductor device is manufactured on the heterogeneous substrate. Of the two sides of the polycrystalline diamond self-supporting substrate, the above-mentioned side is called the "front side" and the other side is called the "back side". In this case, for the front side of the polycrystalline diamond self-supporting substrate, good bonding with the heterogeneous substrate is required. In addition, if the self-heating of the semiconductor device is considered, high heat dissipation is required for the back side of the polycrystalline diamond self-supporting substrate. It is known in patent document 1 that even if a thick polycrystalline diamond layer is formed to obtain sufficient mechanical strength as a self-supporting substrate, the bonding with the heterogeneous substrate on the front side and the heat dissipation on the back side cannot be fully obtained.
[0010] In view of the above problems, the present invention aims to provide a polycrystalline diamond self-supporting substrate having excellent bonding properties with a different substrate on the front side and excellent heat dissipation properties on the back side, and an advantageous method for producing the same. In addition, the present invention aims to provide a laminated substrate using the polycrystalline diamond self-supporting substrate and a method for producing the same.
[0011] Means of solving problems
[0012] In order to solve the above-mentioned problem, the inventor has carried out in-depth research and obtained the following opinion. First, it is known that in order to obtain the excellent bonding property of the front side with the heterogeneous substrate, it is necessary to make the arithmetic mean roughness Ra of the front side be below 3nm. In addition, it is known that in order to obtain the excellent heat dissipation of the back side, it is important to make the average grain size of the diamond particles on the front side be such extremely fine below 100nm, and intentionally make the average grain size of the diamond particles on the back side be increased to more than 1000nm.
[0013] In addition, in order to make diamond particles become the extremely fine of average grain size below 100nm on the front side, and make diamond particles become the coarse of average grain size above 1000nm on the back side, it is found that it is advisable to adopt the following preparation method. First, the diamond particles with average grain size below 100nm are attached on the semiconductor substrate, and the diamond particles are cores. By CVD method, the polycrystalline diamond layer with thickness above 300μm and below 3mm is grown on the semiconductor substrate. The polycrystalline diamond layer has the growth start face connected with the semiconductor substrate and the growth face on the opposite side of the semiconductor substrate. Then, the semiconductor substrate is removed to obtain a polycrystalline diamond self-supporting substrate. At this time, since the diamond particles with average grain size below 100nm are cores, the average grain size of the diamond particles on the growth start face of the polycrystalline diamond layer is below 100nm. Therefore, as long as the growth start face of the polycrystalline diamond layer is set as the front side of the polycrystalline diamond self-supporting substrate. On the other hand, during the film formation process, as the thickness of the polycrystalline diamond layer increases, the particle size of the diamond particles increases, so the average particle size of the diamond particles on the growth surface of the polycrystalline diamond layer is more than 1000nm. Therefore, it is sufficient to set the growth surface of the polycrystalline diamond layer as the back side of the polycrystalline diamond self-supporting substrate.
[0014] And find that, if the average grain size of the diamond particles on the front is below 100nm, then the arithmetic mean roughness Ra on the front can be easily made to be below 3nm. Specifically, if the average grain size of the diamond particles on the front is below 3nm, then Ra can be made to be below 3nm without polishing the front basically. Even when the average grain size of the diamond particles on the front surpasses 3nm, as long as it is below 100nm, then Ra can also be easily made to be below 3nm by polishing the front.
[0015] The gist of the present invention completed based on the above findings is as follows.
[0016] [1] A polycrystalline diamond self-supporting substrate having a front side and a back side, wherein:
[0017] The average particle size of the diamond particles on the front side is not less than 1 nm and not more than 100 nm,
[0018] The average particle size of the diamond particles on the back side is not less than 1000 nm and not more than 4000 nm,
[0019] The arithmetic mean roughness Ra of the front surface is greater than or equal to 1 nm and less than or equal to 3 nm,
[0020] The thickness is 300 μm or more and 3 mm or less.
[0021] [2] A laminate substrate comprising:
[0022] The polycrystalline diamond self-supporting substrate described in [1] above, and
[0023] A SiC substrate, a GaN substrate, a Ga2O3 substrate or a single crystal diamond substrate is bonded to the front surface.
[0024] [3] A method for preparing a polycrystalline diamond self-supporting substrate, comprising:
[0025] The step of attaching diamond particles having an average particle size of 1 nm to 100 nm on a semiconductor substrate,
[0026] A step of growing a polycrystalline diamond layer having a thickness of 300 μm or more and 3 mm or less on the semiconductor substrate by chemical vapor growth method using the diamond particles as cores, wherein the polycrystalline diamond layer has a growth start surface in contact with the semiconductor substrate and a growth surface on the opposite side of the semiconductor substrate,
[0027] Then, the step of removing the semiconductor substrate to expose the growth start surface and obtaining a polycrystalline diamond self-supporting substrate composed of the polycrystalline diamond layer, and
[0028] The step of setting the growth start surface of the polycrystalline diamond layer to the front surface of the polycrystalline diamond self-supporting substrate and setting the growth surface of the polycrystalline diamond layer to the back surface of the polycrystalline diamond self-supporting substrate;
[0029] The polycrystalline diamond self-supporting substrate is obtained, wherein the average particle size of the diamond particles on the front side is greater than 1 nm and less than 100 nm, the average particle size of the diamond particles on the back side is greater than 1000 nm and less than 4000 nm, the arithmetic mean roughness Ra of the front side is greater than 1 nm and less than 3 nm, and the thickness is greater than 300 μm and less than 3 mm.
[0030] [4] The method for producing a polycrystalline diamond self-supporting substrate described in [3] above, further comprising the step of polishing the front surface of the polycrystalline diamond self-supporting substrate.
[0031] [5] The method for preparing a polycrystalline diamond self-supporting substrate described in [3] or [4] above, wherein the semiconductor substrate is a silicon substrate, a sapphire substrate or a SiC substrate.
[0032] [6] A method for preparing a laminated substrate, comprising:
[0033] A method for preparing a polycrystalline diamond self-supporting substrate as described in any one of [3] to [5] above, and
[0034] A process of bonding a SiC substrate, a GaN substrate, a Ga2O3 substrate or a single crystal diamond substrate to the front surface of the polycrystalline diamond self-supporting substrate to obtain a stacked substrate.
[0035] Effects of the Invention
[0036] The polycrystalline diamond self-supporting substrate of the present invention has excellent bonding with a different substrate on the front side and excellent heat dissipation on the back side. According to the method for producing a polycrystalline diamond self-supporting substrate of the present invention, a polycrystalline diamond self-supporting substrate having excellent bonding with a different substrate on the front side and excellent heat dissipation on the back side can be produced. In addition, the present invention can provide a laminated substrate using the polycrystalline diamond self-supporting substrate and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] [ Figure 1 ] A schematic cross-sectional view of a polycrystalline diamond freestanding substrate 100 according to an embodiment of the present invention.
[0038] [ Figure 2 ] (A) to (E) are schematic cross-sectional views illustrating a method for preparing a polycrystalline diamond self-supporting substrate 100 according to an embodiment of the present invention.
[0039] [ Figure 3 ] A schematic cross-sectional view of a stacked substrate 200 according to an embodiment of the present invention.
[0040] [ Figure 4 ] (A) and (B) are schematic cross-sectional views illustrating a method for preparing a laminate substrate 200 according to an embodiment of the present invention.
[0041] [ Figure 5 ] Raman spectrum of the polycrystalline diamond self-supporting substrate of Invention Example 1. DETAILED DESCRIPTION
[0042] (Polycrystalline diamond self-supporting substrate)
[0043] Reference Figure 1 According to one embodiment of the present invention, a polycrystalline diamond self-supporting substrate 100 has a front side 100A and a back side 100B, the average particle size of the diamond particles on the front side 100A is greater than 1 nm and less than 100 nm, the average particle size of the diamond particles on the back side 100B is greater than 1000 nm and less than 4000 nm, the arithmetic mean roughness Ra of the front side 100A is greater than 1 nm and less than 3 nm, and the thickness is greater than 300 μm and less than 3 mm.
[0044] [Average particle size of diamond particles]
[0045] In the present embodiment, it is important that the average particle diameter of the diamond particles of the front 100A of the polycrystalline diamond self-supporting substrate 100 is more than 1nm and less than 100nm. When the average particle diameter exceeds 100nm, the heat dissipation from the back is insufficient. It is believed that the reason is that if large diamond particles are formed on the surface of the front side, the gap between the particles becomes larger, heat is retained in the gap, and the heat transfer to the back is poor. If small diamond particles are formed at a high density on the surface of the front side, the gap between the particles becomes smaller, the heat transfer to the back is improved, and the heat dissipation of the back is excellent. Therefore, the average particle diameter is set to less than 100nm. In addition, by setting the average particle diameter to less than 100nm, the arithmetic mean roughness Ra of the front 100A can be easily made to be less than 3nm. It should be noted that, from the viewpoint of the lower limit of the average particle diameter of the diamond particles attached as the core (with reference to the preparation method described later), the average particle diameter of the diamond particles of the front 100A is more than 1nm.
[0046] In this embodiment, it is important that the average particle size of the diamond particles on the back side 100B of the polycrystalline diamond self-supporting substrate 100 is greater than 1000nm and less than 4000nm. When the average particle size is less than 1000nm, the heat dissipation of the back side is insufficient. When the average particle size exceeds 4000nm, there is a risk of causing adsorption errors when the back side is vacuum-adsorbed for substrate transportation.
[0047] In the present invention, the "average particle size of diamond particles" of each of the front surface 100A and the back surface 100B is defined as follows. That is, on each of the front and back surfaces, three regions of 10 μm×10 μm, centered at three points, which are the center point of the polycrystalline diamond self-supporting substrate and two intersection points of the circumference of 95% of the radius of the polycrystalline diamond self-supporting substrate and the diameter, are observed with an optical microscope, and the arithmetic mean of the particle size of all diamond particles in these three regions is defined as the "average particle size of diamond particles". It should be noted that the "particle size of diamond particles" is the length of the major axis of the diamond particles.
[0048] Due to the manufacturing method described below, the average grain size of diamond grains in the thickness direction of the polycrystalline diamond self-supporting substrate 100 gradually increases from the front surface 100A to the back surface 100B and then gradually saturates.
[0049] [Arithmetic mean roughness Ra of the front surface]
[0050] In the present embodiment, it is important that the arithmetic mean roughness Ra of the front side 100A of the polycrystalline diamond self-supporting substrate 100 is greater than 1 nm and less than 3 nm. Therefore, the bonding property of the front side with the heterogeneous substrate is excellent. When the Ra exceeds 3 nm, the bonding property of the front side with the heterogeneous substrate is insufficient. It should be noted that in the present invention, the "arithmetic mean roughness Ra of the front side" is the arithmetic mean roughness according to JIS B0601-2001. Specifically, on the front side, an atomic force microscope (AFM: Atomic Force Microscope) with a probe having a diameter of 7 nm is used to observe three areas of 20 μm × 20 μm centered on the center point of the polycrystalline diamond self-supporting substrate and the two intersection points of the radius 95% of the polycrystalline diamond self-supporting substrate and the diameter, respectively, and the surface shape is imaged. From the obtained surface shape, the arithmetic mean roughness Ra of each area is calculated according to JIS B0601-2001, and its arithmetic mean is used as the "arithmetic mean roughness Ra of the front side".
[0051] [Thickness and diameter of polycrystalline diamond self-supporting substrate]
[0052] The thickness of the polycrystalline diamond self-supporting substrate 100 is greater than 300 μm and less than 3 mm. When the thickness is less than 300 μm, sufficient mechanical strength cannot be obtained as a self-supporting substrate, and the polycrystalline diamond layer will break after removing the semiconductor substrate 10. When the thickness exceeds 3 mm, the processing time becomes too long. The diameter of the polycrystalline diamond self-supporting substrate 100 is not particularly limited, for example, it can be set to greater than 50 mm and less than 300 mm. It should be noted that for the "thickness of the polycrystalline diamond self-supporting substrate", the average value of the thickness measured by cross-sectional observation using an optical microscope is adopted, which is centered on a total of 3 points of 10 μm × 10 μm in 3 areas, which are centered on the center point of the polycrystalline diamond self-supporting substrate and 2 intersection points of the circumference of 95% of the radius of the polycrystalline diamond self-supporting substrate and the diameter.
[0053] In the present invention, the "front" of the polycrystalline diamond self-supporting substrate is the surface on which semiconductor devices are made or heterogeneous substrates are attached, and the "back" of the polycrystalline diamond self-supporting substrate is the surface on the opposite side of the front. Here, an identifier (laser mark) recording product information is engraved on the front or back of the polycrystalline diamond self-supporting substrate. Therefore, the front and back of the polycrystalline diamond self-supporting substrate are clearly distinguished. It should be noted that in this embodiment, it is preferred to engrave a laser mark on the back of the polycrystalline diamond self-supporting substrate.
[0054] (Method for preparing polycrystalline diamond self-supporting substrate)
[0055] Reference Figure 2 (A) to (E), a method for preparing a polycrystalline diamond self-supporting substrate 100 according to an embodiment of the present invention comprises the following steps. First, Figure 2 As shown in (A) and (B), diamond particles 12 having an average particle size of 1 nm or more and 100 nm or less are attached to a semiconductor substrate 10. Then, as Figure 2 As shown in (B) and (C), a polycrystalline diamond layer 14 having a thickness of 300 μm or more and 3 mm or less is grown on a semiconductor substrate 10 by chemical vapor deposition (CVD) with diamond particles 12 as cores. At this time, the polycrystalline diamond layer 14 has a growth start surface 14A in contact with the semiconductor substrate 10 and a growth surface 14B on the opposite side of the semiconductor substrate 10. Then, as Figure 2 As shown in (D) and (E), the semiconductor substrate 10 is removed to expose the growth start surface 14A, thereby obtaining a polycrystalline diamond self-supporting substrate 100 composed of the polycrystalline diamond layer 14. Here, in this embodiment, it is important to set the growth start surface 14A of the polycrystalline diamond layer 14 as the front surface 100A of the polycrystalline diamond self-supporting substrate 100, and to set the growth surface 14B of the polycrystalline diamond layer 14 as the back surface 100B of the polycrystalline diamond self-supporting substrate 100. Figure 2 (E) Figure 2 (D) The polycrystalline diamond free-standing substrate is inverted.
[0056] In the method for preparing the polycrystalline diamond self-supporting substrate 100 of the present embodiment, as an optional step, before removing the semiconductor substrate 10 ( Figure 2 (C) After and Figure 2 (D) Before) The growth surface 14B of the polycrystalline diamond layer 14 is polished to be flattened.
[0057] In the method for preparing the polycrystalline diamond self-supporting substrate 100 of the present embodiment, as an optional step, after removing the semiconductor substrate 10 ( Figure 2(D) After that, the growth start surface 14A of the polycrystalline diamond layer is polished to be flattened.
[0058] In this way, we can get Figure 1 The polycrystalline diamond self-supporting substrate 100 is shown. Hereinafter, each step of this embodiment will be described in detail.
[0059] [Preparation of semiconductor substrate]
[0060] Reference Figure 2 (A), first, prepare a semiconductor substrate 10. The semiconductor substrate 10 is preferably a silicon substrate, a sapphire substrate or a SiC substrate. The thickness of the semiconductor substrate 10 is preferably set to be greater than 200 μm and less than 3 mm. In the case where the thickness is less than 200 μm, the polycrystalline diamond layer may be peeled off due to the warping of the semiconductor substrate, or the semiconductor substrate may be cracked. In addition, in the case where the thickness exceeds 3 mm, it is not preferred from the perspective of the processing time or material cost of the removal step of the semiconductor substrate 10 described later. The diameter of the semiconductor substrate 10 can be set to be the same as the diameter of the desired polycrystalline diamond self-supporting substrate 100.
[0061] [Attachment of diamond particles]
[0062] like Figure 2 As shown in (A) and (B), diamond particles 12 having an average particle size of 1 nm to 100 nm are attached to the semiconductor substrate 10. The method of attaching the diamond particles 12 to the semiconductor substrate 10 is not particularly limited, and the following method can be cited as an example.
[0063] [[Coating of solution containing diamond particles]]
[0064] First, a solution containing diamond particles is applied on the semiconductor substrate 10 to form a liquid film containing diamond particles on the semiconductor substrate 10. As a coating method, spin coating, spraying and immersion can be listed, and spin coating is particularly preferred. According to the spin coating, the solution containing diamond particles can be evenly applied only on the surface of one side where the diamond particles 12 are to be attached in the two sides of the semiconductor substrate 10.
[0065] Importantly, the average grain size of the diamond particles contained in the solution that contains diamond particles is more than 1nm and below 100nm. If this average grain size is more than 1nm, then in the initial stage of making polycrystalline diamond layer 14 grow, the phenomenon that diamond particles are bounced off from the surface of semiconductor substrate 10 because of sputtering can be suppressed, and in addition, the average grain size of the diamond particles 12 that can be attached to the semiconductor substrate 10 is more than 1nm. If this average grain size is below 100nm, then the polycrystalline diamond layer can not abnormal growth and can dense film forming, and in addition, the average grain size of the diamond particles 12 that can be attached to the semiconductor substrate 10 is below 100nm. The diamond particles of such size can be suitably made by graphite by known detonation method, implosion method or comminution method. It should be noted that the “average particle size of diamond particles contained in the solution containing diamond particles” is an average particle size calculated in accordance with JIS 8819-2, and refers to an average particle size calculated assuming that the particle size distribution measured by a known laser diffraction particle size distribution measuring apparatus follows a normal distribution.
[0066] Here, in the semiconductor substrate 10 before the solution containing diamond particles is applied, hydrofluoric acid or the like is usually used for acid washing in order to remove the metal impurities attached to its surface. Since the surface of the semiconductor substrate 10 after acid washing is an active hydrophobic surface, particles are easily attached to its surface. Therefore, it is preferred to wash the semiconductor substrate 10 after acid washing with pure water or the like so that the surface of the semiconductor substrate 10 becomes a hydrophilic surface formed with a natural oxide film. Alternatively, it is preferred to place the semiconductor substrate 10 after acid washing in a clean room for a long time to form a natural oxide film on the surface of the semiconductor substrate 10. Thus, particles can be inhibited from attaching to the surface of the semiconductor substrate 10. At this time, a fixed charge with a positive charge is generated in the natural oxide film. Therefore, if a solution containing diamond particles containing negatively charged diamond particles is applied on the positively charged natural oxide film, the semiconductor substrate 10 and the diamond particles 12 are firmly combined due to Coulomb attraction. Thus, the adhesion of the polycrystalline diamond layer 14 to the semiconductor substrate 10 is improved. Negatively charged diamond particles can be obtained by subjecting the diamond particles to oxidation treatment so that the diamond particles are terminated with carboxyl groups or keto groups. For example, as oxidation treatment, a method of thermally oxidizing the diamond particles or a method of immersing the diamond particles in an ozone solution, a nitric acid solution, an aqueous hydrogen peroxide solution or a perchloric acid solution can be cited.
[0067] Examples of the solvent of the solution containing diamond particles include organic solvents such as methanol, ethanol, 2-propanol and toluene in addition to water. These solvents may be used alone or in combination of two or more.
[0068] The content of the diamond particles in the solution that contains diamond particles is preferably set to more than 0.03 mass % and below 10 mass % relative to the entire solution that contains diamond particles. The reason is that, if more than 0.03 mass %, diamond particles 12 can be uniformly attached on the semiconductor substrate 10, if below 10 mass %, the abnormal growth of the diamond particles 12 attached in the growth process of polycrystalline diamond layer 14 can be suppressed.
[0069] From the viewpoint of improving the adhesion of diamond particles 12 and semiconductor substrate 10, preferably the solution containing diamond particles is made into gelatin, and thickener can also be contained in the solution containing diamond particles. As thickener, agar, carrageenan, xanthan gum, gellan gum, guar gum, polyvinyl alcohol, polyacrylate thickener, water-soluble cellulose, polyethylene oxide etc. can be listed, and one or more of them can be used. When containing thickener, the pH of the solution containing diamond particles is preferably set to the scope of more than 6 and less than 8.
[0070] The solution containing diamond particles can be prepared by mixing diamond particles in the above-mentioned solvent and stirring to disperse the diamond particles in the solvent. The stirring speed is preferably set to 500 rpm or more and 3000 rpm or less, and the stirring time is preferably set to 10 minutes or more and 1 hour or less.
[0071] [[Heat treatment]]
[0072] Next, the semiconductor substrate 10 is subjected to heat treatment. As a result, the solvent in the liquid film containing diamond particles evaporates, and the bonding force between the surface of the semiconductor substrate 10 and the diamond particles 12 is strengthened, so that the diamond particles 12 are attached to the semiconductor substrate 10. The temperature of the semiconductor substrate 10 during the heat treatment is preferably set to be lower than 100°C, and more preferably set to be 30°C or higher and 80°C or lower. If it is lower than 100°C, the generation of bubbles associated with the boiling of the solution containing diamond particles can be suppressed, so that there will be no local area on the semiconductor substrate 10 where the diamond particles 12 are not present, and there is no risk of the polycrystalline diamond layer 14 peeling off from this area. If it is above 30°C, the semiconductor substrate 10 and the diamond particles 12 are fully bonded, so in the process of growing the polycrystalline diamond layer 14 by the CVD method, the diamond particles 12 can be suppressed from being ejected due to the sputtering effect, and the polycrystalline diamond layer 14 can be uniformly grown. In addition, the heat treatment time is preferably set to be 1 minute or more and 30 minutes or less. It should be noted that a known heat treatment apparatus may be used as the heat treatment apparatus, and for example, the heat treatment may be performed by placing the semiconductor substrate 10 on a heated hot plate.
[0073] [[Other attachment methods]]
[0074] As another example of a method for attaching the diamond particles 12 to the semiconductor substrate 10, a damage method can be cited. In the damage method, the diamond particles 12 are attached to the semiconductor substrate 10 by embedding the diamond particles 12 on the surface of the semiconductor substrate 10. Examples of methods for embedding the diamond particles include: (1) a method of distributing dry diamond powder on the surface of a silicon wafer and applying a pressing force to the surface of the semiconductor substrate, (2) a method of spraying a high-speed gas containing diamond particles onto the surface of the semiconductor substrate, (3) a method of placing the semiconductor substrate in a fluidized bed of diamond particles, and (4) a method of ultrasonically cleaning the semiconductor substrate in a solution in which diamond particles are dispersed.
[0075] [Growth of polycrystalline diamond layer]
[0076] Then, if Figure 2 As shown in (B) and (C), a polycrystalline diamond layer 14 having a thickness of 300 μm to 3 mm is grown on a semiconductor substrate 10 by CVD using diamond particles 12 as cores. As the CVD method, a plasma CVD method, a hot filament CVD method, and the like can be suitably used.
[0077] When a plasma CVD method is used, for example, hydrogen is used as a carrier gas, a source gas such as methane is introduced into the chamber, and the temperature of the semiconductor substrate 10 is set to be above 700°C and below 1300°C, so that the polycrystalline diamond layer 14 grows. From the viewpoint of improving the uniformity of the thickness of the polycrystalline diamond layer 14, it is preferred to use a microwave plasma CVD method. The microwave plasma CVD method is a method of decomposing a source gas such as methane into plasma using microwaves in a plasma chamber, and guiding the plasmatized source gas onto the heated semiconductor substrate 10, thereby growing the polycrystalline diamond layer 14. Here, the pressure in the plasma chamber, the power of the microwave, and the temperature of the semiconductor substrate 10 are preferably set as follows. The pressure in the plasma chamber is preferably set to 1.3×10 3 Pa or more and 1.3×10 5 Pa or less, more preferably 1.1×10 4 Pa or more and 4.0×10 4 The power of the microwave is preferably 0.1 kW to 100 kW, more preferably 1 kW to 10 kW. The temperature of the semiconductor substrate 10 is preferably 700° C. to 1300° C., more preferably 900° C. to 1200° C.
[0078] In the case of using the hot filament CVD method, a filament made of tungsten, tantalum, rhenium, molybdenum, iridium, etc. is used, and the filament temperature is set to be above 1900°C and below 2300°C, and carbon radicals are generated from a hydrocarbon source gas such as methane. The carbon radicals are guided onto the heated semiconductor substrate 10 to grow a polycrystalline diamond layer 14. The hot filament CVD method can easily cope with the increase in the diameter of the substrate. Here, the pressure in the chamber, the distance between the filament and the semiconductor substrate 10, and the temperature of the semiconductor substrate 10 are preferably set as follows. The pressure in the chamber is preferably set to 1.3×10 3 Pa or more and 1.3×10 5 The distance between the filament and the semiconductor substrate 10 is preferably set to 5 mm or more and 20 mm or less. The temperature of the semiconductor substrate 10 is preferably set to 700° C. or more and 1300° C. or less.
[0079] Since the polycrystalline diamond layer 14 constitutes the polycrystalline diamond self-supporting substrate 100 , the thickness of the polycrystalline diamond layer 14 grown on the semiconductor substrate 10 is set to be 300 μm or more and 3 mm or less.
[0080] In the present embodiment, since the CVD method is performed using diamond particles 12 having an average particle size of 1 nm or more and 100 nm or less as cores, the average particle size of the diamond particles can be made to be 1 nm or more and 100 nm or less on the growth start surface 14A of the polycrystalline diamond layer 14. In addition, during the film formation process, as the thickness of the polycrystalline diamond layer 14 increases, the particle size of the diamond particles increases, so that on the growth surface 14B of the polycrystalline diamond layer 14, the average particle size of the diamond particles is 1000 nm or more and 4000 nm or less.
[0081] [Polishing of the growth surface]
[0082] Then, before removing the semiconductor substrate 10 ( Figure 2 (C) After and Figure 2 (D) before), the growth surface 14B of the polycrystalline diamond layer 14 can be polished to make it flat. Excessive unevenness is formed on the surface (growth surface 14B) of the polycrystalline diamond layer 14 after film formation. By flattening the surface of the polycrystalline diamond layer 14, the polycrystalline diamond self-supporting substrate 100 obtained thereafter can be reliably placed (clamped) on the sample table of the semiconductor processing device. The flattening method is not particularly limited, for example, the well-known chemical mechanical polishing (CMP: Chemical Mechanical Polishing) method can be suitably used. It should be noted that after flattening, the thickness of the polycrystalline diamond layer 14 is also set to be greater than 300μm and less than 3mm.
[0083] [Removal of semiconductor substrate]
[0084] Then, if Figure 2 As shown in (D) and (E), the semiconductor substrate 10 is removed to expose the growth start surface 14A, thereby obtaining a polycrystalline diamond self-supporting substrate 100 composed of a polycrystalline diamond layer 14. The method for removing the semiconductor substrate 10 is not particularly limited, and one or more of grinding, polishing and chemical etching can be used. For example, the semiconductor substrate 10 is ground from the surface on the opposite side of the interface with the polycrystalline diamond layer 14 to reduce the thickness to a certain extent, and then chemical etching is performed using an etching solution that does not dissolve diamond but only dissolves the semiconductor substrate 10, thereby removing the semiconductor substrate 10 and exposing the growth start surface 14A. In grinding and polishing, known or arbitrary grinding methods and polishing methods can be appropriately used, specifically, surface grinding methods and mirror polishing methods can be used. In addition, as an etching solution, an alkaline etching solution such as potassium hydroxide (KOH) and tetramethylammonium hydroxide (TMAH) can be used.
[0085] [Front / Back settings]
[0086] The growth start surface 14A of the polycrystalline diamond layer 14 is set as the front surface 100A of the polycrystalline diamond self-supporting substrate 100, and the growth surface 14B of the polycrystalline diamond layer 14 is set as the back surface 100B of the polycrystalline diamond self-supporting substrate 100. Figure 2 (E) Figure 2 The polycrystalline diamond self-supporting substrate (D) is reversed, for example, specifically, the growth surface 14B is adsorbed on the tweezers for conveying, and the growth start surface 14A is configured as the positive side. In addition, an identifier (laser mark) recording product information is engraved on the growth start surface 14A on the front side of the polycrystalline diamond self-supporting substrate or the growth surface 14B on the back side. In the case where the polycrystalline diamond self-supporting substrate 100 is bonded to a heterogeneous substrate for use, if there is a laser mark on the bonding surface, poor bonding will occur. Therefore, it is preferred to engrave a laser mark on the growth surface 14B on the back side of the polycrystalline diamond self-supporting substrate. Thus, a polycrystalline diamond self-supporting substrate 100 can be obtained in which the average particle size of the diamond particles on the front side 100A is greater than 1nm and less than 100nm, and the average particle size of the diamond particles on the back side 100B is greater than 1000nm and less than 4000nm.
[0087] [Polishing of the front side (growth start side)]
[0088] After removing the semiconductor substrate 10 ( Figure 2(D) after), the growth start surface 14A of the polycrystalline diamond layer (the front side 100A of the polycrystalline diamond self-supporting substrate) can be polished to make it flat. If the average particle size of the diamond particles on the front side 100A of the polycrystalline diamond self-supporting substrate is less than 3nm, the Ra can be made less than 3nm without polishing the front side 100A. However, in the case where the average particle size of the diamond particles on the front side 100A exceeds 3nm, the Ra of the front side 100A can be made less than 3nm by polishing the front side 100A. It should be noted that if the average particle size of the diamond particles on the front side 100A exceeds 100nm, it is difficult to adjust the Ra to less than 3nm by polishing. If the average particle size is less than 100nm, the Ra can be easily made less than 3nm by polishing the front side.
[0089] (Laminated substrate)
[0090] Reference Figure 3 According to one embodiment of the present invention, a stacked substrate 200 includes a polycrystalline diamond self-supporting substrate 100 and a heterogeneous substrate 20 bonded to the front surface 100A of the polycrystalline diamond self-supporting substrate. Since the arithmetic mean roughness Ra of the front surface 100A of the polycrystalline diamond self-supporting substrate 100 is 1 nm or more and 3 nm or less, the bonding property with the heterogeneous substrate is excellent. Therefore, the bonding property between the polycrystalline diamond self-supporting substrate 100 and the heterogeneous substrate 20 of the stacked substrate 200 according to the present embodiment is good. A desired semiconductor device such as a high-frequency device or a power device can be formed on the heterogeneous substrate 20.
[0091] (Method for producing laminated substrate)
[0092] Reference Figure 4 (A), (B), in a method for preparing a stacked substrate 200 according to an embodiment of the present invention, the method for preparing the polycrystalline diamond self-supporting substrate 100 described above is carried out, and then, a heterogeneous substrate 20 is bonded to the front side 100A of the polycrystalline diamond self-supporting substrate 100 to obtain the stacked substrate 200.
[0093] [Preparation of heterogeneous substrates]
[0094] The heterogeneous substrate 20 can be a SiC substrate, a GaN substrate, a Ga2O3 substrate or a single crystal diamond substrate. The thickness of the heterogeneous substrate 20 can be appropriately determined in consideration of its strength, and is preferably set to be greater than 300 μm and less than 1000 μm. The diameter of the heterogeneous substrate 20 can be set to be the same as the diameter of the polycrystalline diamond self-supporting substrate 100.
[0095] [Lamination of different types of substrates]
[0096] The method of bonding the different-type substrate 20 to the polycrystalline diamond self-supporting substrate 100 is not particularly limited, and examples thereof include bonding by a known vacuum room temperature bonding method or a plasma bonding method.
[0097] The vacuum normal temperature bonding method is a method of bonding the polycrystalline diamond self-supporting substrate 100 and the heterogeneous substrate 20 at room temperature without heating them. In this embodiment, the front surface 100A of the polycrystalline diamond self-supporting substrate 100 and the surface of the heterogeneous substrate 20 are activated by irradiating an ion beam or a neutral atom beam at vacuum normal temperature, so that the surfaces of both sides become activated surfaces. As a result, dangling bonds appear on the activated surfaces. Therefore, if the activated surfaces of the above two sides are continuously brought into contact at vacuum normal temperature, the bonding force instantly acts, and the polycrystalline diamond self-supporting substrate 100 and the heterogeneous substrate 20 are firmly bonded with the above activated surfaces as bonding surfaces.
[0098] The plasma bonding method is a wafer bonding method in which the front surface 100A of the polycrystalline diamond self-supporting substrate 100 and the surface of the heterogeneous substrate 20 are exposed to a plasma atmosphere, dangling bonds are formed on each surface, and the dangling bonds are bonded to each other. Usually, since the plasma activation treatment and the wafer bonding treatment are implemented by different devices, once the activated dangling bonds are exposed to the atmosphere, the dangling bond density decreases and the wafer bonding strength decreases. Therefore, in order to ensure the wafer bonding strength, it is preferred to perform a heat treatment after wafer bonding.
[0099] [Thickness reduction of heterogeneous substrates]
[0100] Then, the heterogeneous substrate 20 can be reduced in thickness. Specifically, the heterogeneous substrate 20 can be reduced in thickness by grinding and polishing the surface opposite to the bonding surface. The thickness of the heterogeneous substrate 20 after thickness reduction can be appropriately determined according to the type or structure of the semiconductor device formed therein, and is preferably set to be greater than 1 μm and less than 500 μm. It should be noted that in the grinding and polishing, a known or arbitrary grinding method and polishing method can be appropriately used, and specifically, a plane grinding method and a mirror polishing method can be used. Example
[0101] (Invention Examples 1 to 6)
[0102] go through Figure 2 The polycrystalline diamond self-supporting substrates of Invention Examples 1 to 6 were produced by the steps shown in (A) to (E).
[0103] First, a silicon wafer with a diameter of 2 inches, a thickness of 3 mm, a plane orientation of (100), a resistivity of 10 Ω·cm, and an oxygen concentration (ASTM F121-1979) of 1.0×10 18atoms / cm 3 p-type silicon wafer.
[0104] Next, diamond particles having an average particle size shown in Table 1 were prepared by a detonation method. The diamond particles were immersed in an aqueous hydrogen peroxide solution to terminate with a carboxyl group (COOH) to make them negatively charged. Next, the diamond particles were mixed into a solvent (H2O) and stirred to prepare a solution containing diamond particles having a content of 0.2% by mass of diamond particles. It should be noted that the stirring speed was set to 1100 rpm, the stirring time was set to 50 minutes, and the temperature of the solution containing diamond particles during stirring was set to 25°C. Next, the silicon wafer was washed with pure water, and after a natural oxide film was formed on the surface, a solution containing diamond particles was applied on the silicon wafer by spin coating to form a liquid film containing diamond particles.
[0105] Next, the silicon wafer was placed on a hot plate set at 90° C. for 3 minutes to perform a heat treatment for strengthening the bonding between the silicon wafer and the diamond particles, thereby allowing the diamond particles to adhere to the silicon wafer.
[0106] Next, hydrogen was used as a carrier gas and methane was used as a source gas, and the microwave plasma CVD method described above was used to grow polycrystalline diamond layers of various thicknesses using the diamond particles attached to the silicon substrate as cores. It should be noted that the pressure in the plasma chamber was set to 1.5×10 4 Pa, the microwave power was set to 5 kW, and the temperature of the silicon wafer was set to 1050°C.
[0107] Next, the growth surface of the polycrystalline diamond layer is polished and planarized by CMP.
[0108] Next, the silicon wafer is removed by grinding and subsequent etching with KOH to expose the growth start surface of the polycrystalline diamond layer.
[0109] In Invention Examples 1 to 6, the growth start surface of the polycrystalline diamond layer is set to the front side of the polycrystalline diamond self-supporting substrate, and the growth surface of the polycrystalline diamond layer is set to the back side of the polycrystalline diamond self-supporting substrate. This is recorded as "with inversion" in Table 2. Specifically, a laser mark is engraved on the growth surface that becomes the back side.
[0110] Next, as shown in the column “Front surface polishing” in Table 1, in some of the inventive examples, the front surface of the polycrystalline diamond self-supporting substrate was polished and planarized by the CMP method.
[0111] (Comparative Examples 1 and 2)
[0112] In Comparative Examples 1 and 2, the growth start surface of the polycrystalline diamond layer is set to the back side of the polycrystalline diamond self-supporting substrate, and the growth surface of the polycrystalline diamond layer is set to the front side of the polycrystalline diamond self-supporting substrate. This is recorded as "no inversion" in Table 2. Specifically, a laser mark is engraved on the growth start surface that becomes the back side. Except for this point, the polycrystalline diamond self-supporting substrate is made in the same manner as Invention Examples 1 to 6.
[0113] (Comparative Example 3)
[0114] An attempt was made to produce a polycrystalline diamond self-supporting substrate under the same conditions as in Invention Example 1, except that the thickness of the polycrystalline diamond layer was 100 μm. However, after the silicon wafer was removed, the polycrystalline diamond layer cracked, and a self-supporting substrate could not be produced.
[0115] [Analysis using Raman spectroscopy]
[0116] In Invention Examples 1 to 6, the surface of the polycrystalline diamond self-supporting substrate was evaluated using Raman analysis. As a representative example, the Raman spectrum of Invention Example 1 is shown in FIG. Figure 5 In. It is found that there is a 3 The D peak (D line, 1330-1340cm -1 ) and by sp 2 The G peak (G line, 1580-1620cm -1 ), the signal intensity of the D peak is greater than that of the G peak. That is, it is found that sp 3 The structure is superior and can be made into sp 3 Structure-based diamond self-supporting substrate.
[0117] [Thickness, average particle size of the front and back surfaces, and arithmetic mean roughness Ra of the front surface]
[0118] The thickness, average grain size of the front and back surfaces, and arithmetic mean roughness Ra of the front surface of the polycrystalline diamond self-supporting substrates were measured in Inventive Examples 1 to 6 and Comparative Examples 1 and 2 by the above-described methods. The results are shown in Table 1.
[0119] [Evaluation of front bonding properties]
[0120] An attempt was made to bond the polycrystalline diamond self-supporting substrates (diameter: 2 inches) of Inventive Examples 1 to 6 and Comparative Examples 1 and 2 to a SiC substrate (diameter: 2 inches) by vacuum room temperature bonding. -5Pa under vacuum and room temperature, argon ions were irradiated on the front side of the polycrystalline diamond self-supporting substrate and the surface of the SiC substrate to make both surfaces active surfaces. Then, the above-mentioned active surfaces were brought into contact under vacuum and room temperature, and the polycrystalline diamond self-supporting substrate and the SiC substrate were attempted to be bonded. In Inventive Examples 1 to 6, since a strong bond can be achieved, it is marked as ○ in the "front bondability" column of Table 1. In Comparative Examples 1 and 2, the two substrates were misaligned and judged to be unbondable, so they were marked as × in the "front bondability" column of Table 1.
[0121] [Evaluation of back heat dissipation]
[0122] The polycrystalline diamond self-supporting substrates of Inventive Examples 1 to 6 and Comparative Examples 1 and 2 were heat treated so that the temperature of the front surface reached 200°C. The thermal conductivity of the polycrystalline diamond self-supporting substrate was determined by measuring the resistance before and after the heat treatment. The higher the heat dissipation from the back surface, the higher the thermal conductivity can be obtained. Table 1 shows how much higher the thermal conductivity is relative to 350 W / mK.
[0123] [Table 1]
[0124]
[0125] As can be seen from Table 1, both the front bonding property with the different-type substrate and the back heat dissipation property are excellent in Inventive Examples 1 to 6. In contrast, in Comparative Examples 1 and 2, both the front bonding property with the different-type substrate and the back heat dissipation property are insufficient.
[0126] Industrial Applicability
[0127] The polycrystalline diamond self-supporting substrate and the laminated substrate according to the present invention are suitable as substrates for manufacturing high-voltage semiconductor devices such as high-frequency devices and power devices.
[0128] Explanation of symbols
[0129] 100 Polycrystalline Diamond Self-supporting Substrate
[0130] 100A polycrystalline diamond free-standing substrate front side
[0131] 100B Polycrystalline diamond self-supporting substrate backside
[0132] 10 Semiconductor substrate
[0133] 12 Diamond particles
[0134] 14 Polycrystalline diamond layer
[0135] 14A Polycrystalline diamond layer growth start surface
[0136] 14B Growth surface of polycrystalline diamond layer
[0137] 200 Laminated Substrate
[0138] 20 Heterogeneous substrates.
Claims
1. A laminate substrate comprising: a polycrystalline diamond free-standing substrate having a front side and a back side, and The SiC substrate, GaN substrate, and GaN substrate bonded to the front surface 2 O 3 substrate or single crystal diamond substrate, in, For the polycrystalline diamond self-supporting substrate, the average particle size of the diamond particles on the front side is greater than 1 nm and less than 100 nm, the average particle size of the diamond particles on the back side is greater than 1000 nm and less than 4000 nm, and the arithmetic mean roughness Ra of the front side is greater than 1 nm and less than 3 nm, The polycrystalline diamond self-supporting substrate has a thickness of 300 μm or more and 3 mm or less.
2. A method for preparing a laminated substrate, comprising: A method for preparing a polycrystalline diamond self-supporting substrate, and A SiC substrate, a GaN substrate, and a GaN substrate are bonded to the front surface of the polycrystalline diamond self-supporting substrate. 2 O 3 substrate or single crystal diamond substrate, a step of obtaining a laminated substrate, The method for preparing the polycrystalline diamond self-supporting substrate comprises: The step of attaching diamond particles having an average particle size of 1 nm to 100 nm on a semiconductor substrate, A step of growing a polycrystalline diamond layer having a thickness of 300 μm or more and 3 mm or less on the semiconductor substrate by chemical vapor growth method using the diamond particles as cores, wherein the polycrystalline diamond layer has a growth start surface in contact with the semiconductor substrate and a growth surface on the opposite side of the semiconductor substrate, Then, the step of removing the semiconductor substrate to expose the growth start surface and obtaining a polycrystalline diamond self-supporting substrate composed of the polycrystalline diamond layer, and The step of setting the growth start surface of the polycrystalline diamond layer to the front surface of the polycrystalline diamond self-supporting substrate and setting the growth surface of the polycrystalline diamond layer to the back surface of the polycrystalline diamond self-supporting substrate; Obtaining the polycrystalline diamond self-supporting substrate, in, The average particle size of the diamond particles on the front side is 1 nm to 100 nm, the average particle size of the diamond particles on the back side is 1000 nm to 4000 nm, the arithmetic mean roughness Ra of the front side is 1 nm to 3 nm, and the thickness is 300 μm to 3 mm. The semiconductor substrate is a silicon substrate, a sapphire substrate or a SiC substrate. 3 . The method for producing a laminated substrate according to claim 2 , wherein the method for producing the polycrystalline diamond self-supporting substrate further comprises a step of polishing the front surface of the polycrystalline diamond self-supporting substrate.