A nickel-based welding wire drawing process
Through the nickel-based welding wire drawing process, through heat treatment, pickling, alkaline washing and control of the drawing speed, the problems of long cycle and large loss of traditional welding wire cold drawing process are solved, and the processing cycle and loss are shortened, while achieving the same Mechanical properties.
Patent Information
- Application Number
- CN202210470351.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-04-28
AI Technical Summary
The traditional cold-drawing process of welding wire requires repeated heat treatment, pickling, alkaline washing and grinding, resulting in a long processing cycle and large losses.
Using nickel-based welding wire drawing process, the drawing speed and temperature are controlled through heat treatment, pickling, alkaline washing, high-pressure water washing, lubrication and drawing, so that the temperature of the welding wire when the drawing mold comes out is not less than 50℃, reducing heat treatment and Number of washes.
It effectively shortens the processing cycle, reduces losses, and achieves the mechanical properties of traditional cold drawing processes, including tensile strength and elongation.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of welding wire drawing technology, and in particular to a nickel-based welding wire drawing technology. Background Art
[0002] When the welding wire is subjected to external forces, it will change from large to small and from thick to thin, and stress will be generated during the deformation. When the stress inside the welding wire cannot be eliminated and exceeds the bearing capacity of the material, the material will naturally crack or break, seriously affecting the yield and quality. In order to eliminate the stress during the drawing process of the welding wire, heating and heat preservation processes are generally added during the drawing process.
[0003] The traditional welding wire cold drawing process is to cold draw the material blank once, reduce the size once, then heat treat, pickle, alkali wash, grind, cold draw again, reduce the size once again, heat treat, pickle, alkali wash, grind, repeat several times, the material can be processed from the blank into the finished product. Its processing cycle is long, the processing loss is large, and the cost is also high. Summary of the invention
[0004] In view of the problems existing in the prior art, the technical problem to be solved by the present invention is that the traditional cold drawing process of welding wire requires repeated heat treatment, pickling, alkali cleaning and grinding processes, resulting in a long processing cycle and large processing losses.
[0005] The technical solution adopted by the present invention to solve the technical problem is: the present invention provides a nickel-based welding wire drawing process, which is carried out according to the following steps:
[0006] (1) placing a nickel-based welding wire blank with a diameter of φ=6.5-8 mm in a pit-type heating furnace for heat treatment at a temperature of 650±50° C. for a heat treatment time of 1-2 h;
[0007] (2) After the heat treatment is completed, the welding wire is pickled, alkaline washed, high-pressure washed, and dried. Then, the temperature of the nickel-based welding wire is heated to 300±20°C, kept warm for 30-40 minutes, and then drawn after lubrication. The total surface reduction rate is 95%-97%. By controlling the drawing speed, the surface temperature of the welding wire after the surface reduction is maintained above 50°C by the 6 wire drawing dies with decreasing apertures;
[0008] (3) The drawn welding wire is cooled to room temperature in air to obtain a finished nickel-based welding wire.
[0009] Specifically, the grade of the nickel-based welding wire is ERNiCrMo-3 wire.
[0010] Specifically, the pulling speed is 3-5 m / s.
[0011] Specifically, the pickling is carried out by mixing 25% sulfuric acid, 5% nitric acid and 5% hydrofluoric acid in a ratio of 1:1:1, or by mixing 13% nitric acid and 8% hydrofluoric acid in a ratio of 1:1, and the pickling time is 10-25 minutes.
[0012] Specifically, the alkaline washing liquid used in the alkaline washing is a NaOH aqueous solution with a mass concentration of 15-20 g / l, the alkaline washing temperature is 700° C., and the alkaline washing time is 10-20 min.
[0013] The beneficial effects of the present invention are:
[0014] Through continuous exploration and experimentation, the present invention discovered that by controlling the starting temperature and drawing speed of the welding wire during the entire drawing process, the temperature of the welding wire when it comes out of the last drawing die is not lower than 50°C. The entire drawing process does not require multiple heat treatments, acid washes, and alkaline washes. The tensile strength and elongation of the obtained welding wire can also reach the mechanical properties achieved by the traditional multi-pass cold drawing process, effectively shortening the processing cycle and reducing processing losses. DETAILED DESCRIPTION
[0015] The present invention will now be further described in detail with reference to embodiments.
[0016] The apertures of the six wire drawing dies used in the following embodiments of the present invention are Φ5.8, Φ4.5, Φ3.4, Φ2.7, Φ2.0, and Φ1.4, respectively.
[0017] The pickling solution used in the following embodiments of the present invention is 25% sulfuric acid, 5% nitric acid and 5% hydrofluoric acid mixed in a ratio of 1:1:1, or 13% nitric acid and 8% hydrofluoric acid mixed in a ratio of 1:1, and the pickling time is 10-25 minutes.
[0018] The alkali washing liquid used in the following embodiments of the present invention is a NaOH aqueous solution with a mass concentration of 15-20 g / l, the alkali washing temperature is 700° C., and the alkali washing time is 10-20 min.
[0019] The lubricant used in the following embodiments of the present invention is composed of 40% graphite powder, 50% lime powder, and 10% 000# lubricating grease in terms of mass percentage.
[0020] Example 1
[0021] (1) placing a H08Mn2SiA welding wire blank with a diameter of φ=6.5 mm in a pit-type vacuum heat treatment furnace for heat treatment at a temperature of 650°C for a heat treatment time of 1.5 h;
[0022] (2) After the heat treatment is completed, the welding wire is pickled, alkaline washed, high-pressure water washed, and dried. Then, the welding wire is heated to 300°C and kept constant for 30 minutes. Then, it is lubricated and drawn. The drawing speed is controlled at 3m / s. The welding wire is reduced in surface by 6 drawing dies with decreasing apertures. The temperature of the welding wire when it comes out of the last drawing die is 52°C.
[0023] (3) The finished welding wire is cooled to room temperature in air to obtain the finished welding wire.
[0024] Example 2
[0025] The H08Mn2SiA welding wire blank with a diameter of φ=6.5mm is placed in a pit type vacuum heat treatment furnace for heat treatment at a temperature of 600°C for a heat treatment time of 2h;
[0026] (2) After the heat treatment is completed, the welding wire is pickled, alkaline washed, high-pressure water washed, and dried. Then, the welding wire is heated to 300°C and kept constant for 40 minutes. Then, it is lubricated and drawn. The drawing speed is controlled to be 4m / s. The welding wire is reduced in surface by 6 drawing dies with decreasing apertures. The temperature of the welding wire when it comes out of the last drawing die is 62°C.
[0027] (3) The finished welding wire after drawing is cooled to room temperature in air to obtain the finished welding wire.
[0028] Example 3
[0029] The 4J36 precision alloy wire blank with a diameter of φ=6.5 mm was placed in a pit type vacuum heat treatment furnace for heat treatment at a temperature of 650°C for a heat treatment time of 1.5 h.
[0030] (2) After the heat treatment is completed, the welding wire is pickled, alkaline washed, high-pressure water washed, and dried. Then, the welding wire is heated to 300°C and kept constant for 35 minutes. Then, it is lubricated and drawn. The drawing speed is controlled to be 5m / s. The welding wire is reduced in surface by 6 drawing dies with decreasing apertures. The temperature of the welding wire when it comes out of the last drawing die is 70°C.
[0031] (3) The finished welding wire after drawing is cooled to room temperature in air to obtain the finished welding wire.
[0032] Example 4
[0033] The 4J36 precision alloy wire blank with a diameter of φ = 6.5 mm was placed in a pit-type vacuum heat treatment furnace for heat treatment at a temperature of 680°C for a heat treatment time of 1 h.
[0034] (2) After the heat treatment is completed, the welding wire is pickled, alkaline washed, high-pressure water washed, and dried. Then, the welding wire is heated to 300°C and kept constant for 40 minutes. Then, it is lubricated and drawn. The drawing speed is controlled to be 3m / s. The welding wire is reduced in surface by 6 drawing dies with decreasing apertures. The temperature of the welding wire when it comes out of the last drawing die is 51°C.
[0035] (3) The finished welding wire after drawing is cooled to room temperature in air to obtain the finished welding wire.
[0036] Comparative Example 1 is the same as Example 1, except that the drawing speed of Comparative Example 1 is reduced to 0.5 m / s, resulting in a temperature of the welding wire of 35° C. when the welding wire comes out of the sixth drawing die.
[0037] Comparative Example 2 is the same as Example 1, except that the welding wire in Comparative Example 2 is cold drawn in a conventional manner, and the specific process is as follows:
[0038] Place the H08Mn2SiA welding wire blank with a diameter of φ=6.5mm in a pit-type vacuum heat treatment furnace, and perform constant temperature heat treatment at 650℃ for 1.5h. Then, pickle, alkali, high-pressure water washing, dry and lubricate the welding wire, and perform surface reduction treatment through the first wire drawing hole die. Then, place it in a pit-type vacuum heat treatment furnace, and perform constant temperature heat treatment at 650℃ for 1.5h. Then, pickle, alkali, high-pressure water washing and dry the welding wire. Then, continue to perform surface reduction treatment through the second wire drawing hole die. Then, place the welding wire in a pit-type vacuum heat treatment furnace, and perform constant temperature heat treatment at 650℃ for 1.5h. Then, pickle, alkali, high-pressure water washing and dry the welding wire. Repeat the above steps until the welding wire passes through the sixth wire drawing hole die for surface reduction treatment to obtain a finished welding wire.
[0039] Comparative Example 3 is the same as Example 4, except that the welding wire in Comparative Example 3 is cold drawn in a conventional manner, and the specific process is as follows:
[0040] The 4J36 precision alloy wire with a diameter of φ6.5 mm was placed in a pit-type vacuum heat treatment furnace for heat treatment at a temperature of 680°C for 1 h.
[0041] The welding wire is then pickled, alkali washed, high-pressure water washed, dried, lubricated, and then subjected to surface reduction treatment through the first wire drawing hole die. The wire is then placed in a pit-type vacuum heat treatment furnace and subjected to constant temperature heat treatment at 680°C for 1 hour. The welding wire is then pickled, alkali washed, high-pressure water washed, dried, and then subjected to constant temperature heat treatment at 680°C for 1 hour through the second wire drawing hole die. The wire is then placed in a pit-type vacuum heat treatment furnace and subjected to constant temperature heat treatment at 680°C for 1 hour. The welding wire is then pickled, alkali washed, high-pressure water washed, dried, and the above steps are repeated until the welding wire passes through the sixth wire drawing hole die for surface reduction treatment to obtain a finished welding wire.
[0042] Comparative Example 4 is the same as Example 1, except that the nickel-based welding wire used in Comparative Example 4 is ENiCrMo-3.
[0043] Performance Test:
[0044] Relevant performance tests were performed on the welding wire products obtained in Examples 1-4 and Comparative Examples 1-4.
[0045] Tensile strength and elongation of welding wire: test standard GB / T 5117-1995.
[0046] The specific test results are shown in Table 1.
[0047] Table 1
[0048] Test items Tensile strength(MPa) Elongation(%) Example 1 1360 20 Example 2 1420 21 Example 3 1450 25 Example 4 1450 25 Comparative Example 1 1300 15 Comparative Example 2 1361 20 Comparative Example 3 1448 23 Comparative Example 4 1210 10
[0049] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A nickel-based welding wire drawing process, characterized in that: Follow these steps: (1) A 4J36 precision alloy wire blank with a diameter of φ = 6.5 mm was placed in a pit-type vacuum heat treatment furnace for heat treatment at a temperature of 650°C for a heat treatment time of 1.5 h; (2) After the heat treatment is completed, the welding wire is pickled, alkaline washed, high-pressure water washed, and dried. Then, the welding wire is heated to 300°C and kept constant for 35 minutes. Then, it is lubricated and drawn. The drawing speed is controlled to be 5m / s. The welding wire is reduced in surface by 6 drawing dies with decreasing apertures. The temperature of the welding wire when it comes out of the last drawing die is 70°C. (3) The finished welding wire after drawing is cooled to room temperature in air to obtain the finished welding wire; The apertures of the six wire drawing dies are Φ5.8, Φ4.5, Φ3.4, Φ2.7, Φ2.0, and Φ1.4 respectively; The pickling solution used for the pickling is 25% sulfuric acid, 5% nitric acid and 5% hydrofluoric acid mixed in a ratio of 1:1:1, or 13% nitric acid and 8% hydrofluoric acid mixed in a ratio of 1:1, and the pickling time is 10-25 minutes; The alkaline washing liquid used in the alkaline washing is a NaOH aqueous solution with a mass concentration of 15-20 g / l, the alkaline washing temperature is 700° C., and the alkaline washing time is 10-20 min; The lubricant used for lubrication is composed of 40% graphite powder, 50% lime powder and 10% 000# grease in terms of mass percentage.