A method for manufacturing a carbon fiber composite material blade and a carbon fiber composite material blade
The integration of VAT and VARTM technologies in the manufacturing of carbon fiber composite blades addresses inefficiencies in existing methods, enhancing mechanical properties and interlayer bonding, leading to high-performance blades with reduced labor costs and improved impact resistance.
Patent Information
- Application Number
- CN202011532481.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-22
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-12-22
AI Technical Summary
Existing methods for manufacturing carbon fiber composite material blades for aircraft engines suffer from poor crack resistance, long manufacturing cycles, high labor costs, and inadequate interlayer bonding, particularly in the use of 2.5D or 3D weaving technologies and resin transfer molding processes.
Employing variable angle tacking (VAT) technology to automate the preparation of carbon fiber preforms, combined with vacuum assisted resin transfer molding (VARTM) to create a carbon fiber composite blade, utilizing specific fiber types and densities, and multiple resin injections to enhance mechanical properties and interlayer bonding.
Improves manufacturing efficiency, reduces labor costs, enhances mechanical properties, and increases interlayer bonding strength, resulting in high-performance carbon fiber composite blades with improved impact resistance and delamination capability.
Smart Images

Figure CN114714641B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of manufacturing blades for aircraft engines, and in particular to a manufacturing method for a carbon fiber composite material blade and a carbon fiber composite material blade. Background Art
[0002] Carbon fiber resin-based composite materials have been widely used in aerospace, defense, transportation, construction, sports and other fields due to their light weight, high strength, designability, fatigue resistance, corrosion resistance and many other excellent properties. Using carbon fiber resin-based composite materials to replace aluminum alloys, titanium alloys and other metal materials to manufacture aircraft engine cold end blades has become the current mainstream development trend. The aircraft engines of European and American companies such as GE, Pratt & Whitney, Rolls-Royce have generally adopted this technology, and have been successfully used in commercial and military aircraft such as Boeing and Airbus, which can significantly reduce the weight of the engine, reduce the development cost of the engine, greatly improve the performance of the engine, and achieve significant economic and safety benefits.
[0003] The first generation of composite blades for aircraft engines were made using a prepreg cladding process. The biggest disadvantage was the poor crack resistance between the layers and the low mechanical properties. The current mainstream technology is to use 2.5D or 3D weaving technology to manufacture preforms, and then use the resin transfer molding (RTM) liquid molding process to manufacture composite blades. The damage resistance of the product is significantly improved, meeting the safety performance requirements for long-term use. However, the cycle of manufacturing preforms using 2.5D and 3D weaving technology is very long, and a lot of manpower is required, which is expensive, often more than ten times the cost of raw materials and curing.
[0004] The patent specification with publication number CN106863848A discloses a method for forming a composite blade of an aircraft engine, comprising the following steps: unfolding a carbon fiber tow, impregnating the unfolded carbon fiber tow with a thermoplastic resin slurry to obtain an intermediate tow; drying the intermediate tow; heating the intermediate tow by ultrasonic vibration heating, laying the heated intermediate tow layer by layer by dry laying to form a blade preform after laying; putting a carbon fiber fabric sleeve on the outside of the blade preform, and sewing the edges of the carbon fiber fabric sleeve and the inner blade preform by a three-dimensional sewing method; placing the sewn blade preform and the carbon fiber fabric sleeve into an RTM mold, and using RTM technology to close the mold of the blade preform and the carbon fiber fabric sleeve and solidify them to obtain a composite blade. There are no Z-direction reinforcing fibers between the layers of the thermoplastic blade preform in the invention patent, resulting in its interlayer anti-cracking performance still not being ideal. In addition, there is a problem of poor compatibility between the internal thermoplastic preform and the outer layer of thermosetting epoxy resin, and cracking and separation are prone to occur under impact, humidity, high and low temperature or cyclic fatigue loads. Summary of the invention
[0005] The invention provides a method for manufacturing a carbon fiber composite material blade, which has high preparation efficiency and excellent blade mechanical properties and anti-impact delamination ability.
[0006] A method for manufacturing a carbon fiber composite material blade, comprising:
[0007] (1) Installing carbon fiber yarn, suture thread and carbon fiber surface felt substrate on a variable angle tacking (VAT) device;
[0008] (2) Using professional software to draw the fiber laying path and set the stitching density, the variable angle laying (VAT) equipment lays the carbon fiber onto the substrate according to the planned path to obtain a blade preform;
[0009] (3) The preform is placed in a metal mold, and a composite blade blank is prepared by a vacuum assisted resin transfer molding (VARTM) process. The blade blank is cut and polished to obtain a finished blade.
[0010] The present invention adopts fully automated equipment to manufacture a preform through the fiber variable angle tacking (VAT) technology, and then manufactures the carbon fiber composite material blade through the vacuum assisted resin transfer molding (VARTM) process, which improves the manufacturing efficiency compared with the 2.5-dimensional and 3D weaving process methods; because the entire blade is continuously made of a bundle of carbon fibers, it has higher mechanical properties.
[0011] In step (1),
[0012] The linear density of the carbon fiber does not exceed 800tex.
[0013] The grade specifications of the carbon fiber include T300-1K, T300-3K, T300-6K, T700-12K, T800-6K, T800-12K, T1000-12K, M40-6K, M40-12K, M46-6K, M46-12K, M50-6K, M55-6K, M60-3K or M60-6K.
[0014] The linear density of carbon fiber indicates its thickness. In the actual VAT seam laying process, when the linear density exceeds 800tex, the fiber is too thick to bend easily or the turning radius is too large, which can easily lead to many seam laying defects.
[0015] The suture thread includes aramid fiber, polyethylene fiber, PBO fiber, polyester, nylon and acrylic fiber, etc., and the line density does not exceed 3000D.
[0016] The suture forms include untwisted and / or twisted.
[0017] The sutures are required to be thin, tough and strong. The sutures are man-made organic fibers with good strength and toughness, which are conducive to enhancing the interlayer crack resistance. Sutures with a line density exceeding 3000D are prone to cause the suture arrangement density to be too large, and the Z-direction fibers squeeze the carbon fibers too much to form excessive defects, reduce the interlayer crack resistance, and have an adverse effect on the X / Y-direction carbon fibers.
[0018] The carbon fiber surface felt substrate is used as a stitching substrate, and the surface density does not exceed 50g / m 2 .
[0019] The carbon fiber surface felt substrate may be in the form of an oriented felt or a random felt.
[0020] When the surface felt density is too high, the thickness is large and the volume occupied is also large, which is not conducive to the performance of the composite material. When it is too thick, it is difficult to deform and is not conducive to draping in the mold.
[0021] In step (2),
[0022] The professional software is CAD two-dimensional drawing software, such as AutoCAD, CAXA, etc.
[0023] The stitching density includes 3×3, 5×5 or 8×8 (row spacing×stitch spacing, mm).
[0024] When the suture density is too high, there are too many suture threads, which are easily tangled and cause suture failure; when it is too low, the suture is not firm.
[0025] The carbon fiber paving path is to pave a bundle of carbon fibers layer by layer, with the paving width of each layer decreasing by 1-3 mm from bottom to top, so as to obtain a preformed body which is thick in the middle and thin at both ends.
[0026] The effect of thicker in the middle and thinner at both ends can be achieved by reducing the width of each layer. Reducing each layer by 1 to 3 mm can achieve a smoother transition effect, ensuring the smooth appearance of the blade and meeting the aerodynamic appearance requirements.
[0027] In step (3),
[0028] A layer of T300-3K carbon fiber woven cloth or prepreg is laid on the surface of the female mold and the male mold of the metal mold, and the fiber surface density does not exceed 240g / m 2 .
[0029] The T300-3K carbon fiber woven cloth or prepreg has a plain weave, a twill weave or a satin weave.
[0030] The surface texture of the woven fabric or prepreg is orderly and beautiful, which can cover the fiber gaps in the filled and stitched preform, thereby improving the appearance. T300-3K plain, twill and satin woven fabrics have the advantages of being soft and easy to lay, beautiful texture and high cost performance. The surface density exceeds 240g / m 2 The woven cloth is too thick, the covering deformation is poor, and it is also easy to cause the blade thickness to exceed the standard, or occupy the space of the preform, which has an adverse effect on the strength.
[0031] After one VARTM glue injection is completed, the pressure of the VARTM equipment is unloaded, and the equipment is re-pressed, vacuumed, and glue injected. The above steps are repeated 2-3 times.
[0032] Through multiple injection and extrusion, we can ensure that the residual voids inside the composite material are completely eliminated, and obtain a completely impregnated carbon fiber composite blade. Eliminating residual pores can reduce or even eliminate internal defects of the blade, improve the density of the blade, and ultimately improve the blade's resistance to external force damage and service life.
[0033] The surface of the blade blank after demoulding is polished with 500-1500# sandpaper, and then the blank is put into the mold again for glue injection and heating and curing.
[0034] Most of the first-made blades have tiny closed pores on their surfaces, which are surface defects. Grinding with fine sandpaper can turn these closed pores into open pores, and injecting glue again can fill these pores, thereby eliminating the surface pore defects.
[0035] The present invention also provides a carbon fiber composite material blade prepared by the manufacturing method of the carbon fiber composite material blade. The carbon fiber composite material blade has excellent mechanical properties, surface finish and impact resistance and delamination capability.
[0036] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0037] (1) The present invention adopts VAT technology to prepare carbon fiber composite blade preforms, which improves manufacturing efficiency and reduces labor costs. In addition, machine laying can ensure the precise cutting positioning and direction of the fiber angle, which is beneficial to improving the quality stability of composite blade products.
[0038] (2) The present invention uses a bundle of carbon fibers to continuously lay seams, which can improve the mechanical properties of the fiber material, and the presence of the suture line can increase the interlayer bonding strength, ultimately improving the integrity and anti-impact delamination ability of the composite blade;
[0039] (3) The present invention adopts a combination of VAT and VARTM technology to prepare composite blades, which reduces weight compared to existing traditional methods and meets the requirements for low-cost batch manufacturing of high-performance carbon fiber composite blades. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 It is a schematic diagram of the overall structure of a carbon fiber composite blade;
[0041] Figure 2 Schematic diagram of VAT production of blade preform, where (a) is a schematic diagram of VAT principle, and (b) is a schematic diagram of layer-by-layer seam laying of blade preform. DETAILED DESCRIPTION
[0042] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings so that the purpose, features and advantages of the present invention can be more clearly understood. It should be understood that the embodiments shown in the accompanying drawings are not intended to limit the scope of the present invention, but are only intended to illustrate the essential spirit of the technical solution of the present invention.
[0043] Example 1
[0044] Figure 1 The overall structure diagram of the carbon fiber composite blade is shown in Figure 1. The blade consists of an upper tenon, a blade body, a lower tenon and a base. The upper tenon, blade body and lower tenon are laid out at one time using the VAT technology. Due to the large thickness of the base, multiple layers of carbon fiber woven cloth are laid on the above base to increase thickness. Finally, the VARTM process is used to prepare the carbon fiber composite blade. The manufacturing method includes the following steps:
[0045] (1) Place T700-6K carbon fiber and Kevlar29 (400D) suture yarn rolls on the VAT equipment’s placement head. The two bundles of yarn pass through two sets of independent yarn guide rings and pass through the needle holes at the end. 2 ) Place it on the paving work surface, flatten it, and fix it with cardboard around it to prevent it from sliding during the paving process;
[0046] (2) The basic principle of fiber variable angle traction suture technology is as follows Figure 2 As shown in (a), the carbon fiber yarn is sewn onto the substrate using a sewing thread and a sewing needle according to a set trajectory to prepare a blade preform. The paving path of the carbon fiber yarn is drawn using CAD software and imported into the VAT device; the control terminal is opened and the sewing density is set to 3×3 (row spacing×needle spacing, mm); the program is started, as shown in FIG. Figure 2 (b) As shown in FIG. 1 , the fibers are laid layer by layer until the entire task is completed; finally, the carbon fiber felt is cut along the edge with scissors to obtain a blade preform;
[0047] (3) Clean the surface of the female mold and the male mold, and apply a mold release agent; place the preform into the mold cavity, adjust the position so that it fits the mold cavity tightly, and use scissors or other tools to trim the preform locally when necessary; cut 10 layers of 3K carbon fiber woven cloth of 10 cm × 3 cm size, and place them into the base of the mold cavity for local thickening; to prevent the material from slipping, conventional shaping spray glue can be used for fixing;
[0048] (4) After all materials are placed in the mold cavity, close the female mold and the male mold, put them into the vulcanizer and press them tightly (pressure 2-5MPa), connect the exhaust pipe and the injection pipe, start the vacuum pump to evacuate the mold cavity, maintain the pressure for 15 minutes, observe the changes in the pressure gauge to ensure sealing. If the pressure changes too much, check the leaking position and replace the sealing strip, injection pipe, outlet pipe, gasket and valve if necessary;
[0049] (5) Start the glue injection machine and slowly inject the epoxy resin into the mold cavity with a glue injection pressure of 2MPa and a glue injection time of 3min. After the first glue injection is completed, the pressure of the vulcanizer can be released and re-tightened for a second glue injection, which is conducive to eliminating internal voids and improving the impregnation effect. After the glue injection is completed, turn on the heating for curing (100℃, 2h) and post-curing (150℃, 2h);
[0050] (6) After the mold is naturally cooled to below 60°C, the mold is opened and the product is taken out. The blade is post-processed using tools to finally obtain a finished carbon fiber composite blade;
[0051] The manufacturing cycle of the blade preform is 20 minutes; according to the ASTM D3039 standard test, the tensile strength of the blade composite material reaches 1100MPa; according to the ADTM D7264 standard test, the bending strength reaches 900MPa; according to the ASTM D2344 standard test, the interlaminar shear strength (ILSS) reaches 60MPa; according to the ASTM D7137 standard test, the compressive strength after impact (CAI) reaches 280MPa.
[0052] Example 2
[0053] Figure 1 The overall structure diagram of the carbon fiber composite material blade is shown in FIG. The manufacturing method thereof comprises the following steps:
[0054] (1) Place T700-6K carbon fiber and Kevlar29 (200D) suture yarn rolls on the VAT equipment’s placement head. The two bundles of yarn pass through two sets of independent yarn guide rings and pass through the needle holes at the end. Place the carbon fiber felt (30 g / m 2 ) Place it on the paving work surface, flatten it, and fix it with cardboard around it to prevent it from sliding during the paving process;
[0055] (2) Use professional software to draw the seam path of the carbon fiber yarn and import it into the VAT equipment; open the control terminal and set the stitching density to 3×3 (row spacing×stitch spacing, mm); start the program and start to seam the fiber layer by layer until all tasks are completed; finally, use scissors to cut the carbon fiber felt along the edge to obtain the blade preform;
[0056] (3) Use an automatic cloth cutting machine to cut T300-3K woven cloth or prepreg into 15 cm × 8 cm pieces, two in number, as the upper and lower surface materials of the blade to improve the appearance quality;
[0057] (4) Clean the surface of the female mold and the male mold, and apply a release agent; first, lay the cut T300-3K woven cloth or prepreg in the male mold and the female mold, and use spray glue to fix the position; then put the preform into the mold cavity, adjust the position so that it fits the mold cavity tightly, and use scissors and other tools to trim the preform locally if necessary; cut 10 layers of T300-3K carbon fiber woven cloth of 10cm×3cm size, and put them into the base of the mold cavity for local thickening; to prevent the material from slipping, conventional shaping spray glue can be used to fix it;
[0058] (5) After all materials are placed in the mold cavity, close the female mold and the male mold, put them into the vulcanizer and press them tightly (pressure 2-5MPa), connect the exhaust pipe and the injection pipe, start the vacuum pump to evacuate the mold cavity, maintain the pressure for 15 minutes, observe the changes in the pressure gauge to ensure sealing. If the pressure changes too much, check the leaking position and replace the sealing strip, injection pipe, outlet pipe, gasket and valve if necessary;
[0059] (6) Start the glue injection machine and slowly inject the epoxy resin into the mold cavity with a glue injection pressure of 3MPa and a glue injection time of 5min. After the first glue injection is completed, the pressure of the vulcanizer can be released and re-tightened for a second glue injection, which is conducive to eliminating internal voids and improving the impregnation effect. After the glue injection is completed, turn on the heating for curing (100℃, 2h) and post-curing (150℃, 2h);
[0060] (7) After the mold is naturally cooled to below 60°C, the mold is opened and the product is taken out. The blade is post-processed using tools to finally obtain a finished carbon fiber composite blade;
[0061] The manufacturing cycle of the blade preform is 25 minutes; according to the ASTM D3039 standard test, the tensile strength of the blade composite material reaches 1200MPa; according to the ADTM D7264 standard test, the bending strength reaches 850MPa; according to the ASTM D2344 standard test, the interlaminar shear strength (ILSS) reaches 64MPa; according to the ASTM D7137 standard test, the compressive strength after impact (CAI) reaches 275MPa.
[0062] Example 3
[0063] Figure 1 The overall structure diagram of the carbon fiber composite material blade is shown in FIG. The manufacturing method thereof comprises the following steps:
[0064] (1) Place T700-6K carbon fiber and Kevlar29 (400D) suture yarn rolls on the VAT equipment’s placement head. The two bundles of yarn pass through two sets of independent yarn guide rings and pass through the needle holes at the end. 2 ) Place it on the seam-laying work surface, flatten it, and fix it with cardboard around it to prevent it from sliding during the seam-laying process;
[0065] (2) Use professional software to draw the seam path of the carbon fiber yarn and import it into the VAT equipment; open the control terminal and set the stitching density to 3×3 (row spacing×stitch spacing, mm); start the program and start to seam the fiber layer by layer until all tasks are completed; finally, use scissors to cut the carbon fiber felt along the edge to obtain the blade preform;
[0066] (3) Use an automatic cloth cutting machine to cut T300-3K woven cloth or prepreg into 15 cm × 8 cm pieces, two in number, as the upper and lower surface materials of the blade to improve the appearance quality;
[0067] (4) Clean the surface of the female mold and the male mold, and apply a release agent; first, lay the cut T300-3K woven cloth or prepreg in the male mold and the female mold, and use spray glue to fix the position; then put the preform into the mold cavity, adjust the position so that it fits the mold cavity tightly, and use scissors and other tools to trim the preform locally if necessary; cut 10 layers of T300-3K carbon fiber woven cloth of 10cm×3cm size, and put them into the base of the mold cavity for local thickening; to prevent the material from slipping, conventional shaping spray glue can be used to fix it;
[0068] (5) After all materials are placed in the mold cavity, close the female mold and the male mold, put them into the vulcanizer and press them tightly (pressure 2-5MPa), connect the exhaust pipe and the injection pipe, start the vacuum pump to evacuate the mold cavity, maintain the pressure for 15 minutes, observe the changes in the pressure gauge to ensure sealing. If the pressure changes too much, check the leaking position and replace the sealing strip, injection pipe, outlet pipe, gasket and valve if necessary;
[0069] (6) Start the glue injection machine and slowly inject the epoxy resin into the mold cavity with a glue injection pressure of 3MPa and a glue injection time of 4min. After the first glue injection is completed, the pressure of the vulcanizer can be released and re-tightened for a second glue injection, which is conducive to eliminating internal voids and improving the impregnation effect. After the glue injection is completed, turn on the heating for curing (100℃, 2h) and post-curing (150℃, 2h);
[0070] (7) After the mold cools naturally to below 60°C, open the mold and take out the product. Use 600# or higher sandpaper to carefully polish the surface of the blade. For local pinhole defects, use a pointed tool to break the pinhole to make it open; finally, clean the blade with alcohol and let it dry naturally;
[0071] (8) Put the blade back into the mold and repeat steps (5)-(6). This step can greatly improve the surface smoothness of the blade. The surface roughness is measured using a surface profiler, and the Ra value is reduced from 2-5μm to less than 0.5μm.
[0072] (9) After the mold is naturally cooled to below 60°C, the mold is opened and the product is taken out. The blade is post-processed using tools to finally obtain a finished carbon fiber composite blade;
[0073] The manufacturing cycle of the blade preform is 18 minutes; according to the ASTM D3039 standard test, the tensile strength of the blade composite material reaches 1150MPa; according to the ADTM D7264 standard test, the bending strength reaches 825MPa; according to the ASTM D2344 standard test, the interlaminar shear strength (ILSS) reaches 60MPa; according to the ASTM D7137 standard test, the compressive strength after impact (CAI) reaches 262MPa.
[0074] The preferred embodiments of the present invention have been described in detail above, but it should be understood that after reading the above teachings of the present invention, those skilled in the art may make various changes or modifications to the present invention. These equivalent forms also fall within the scope defined by the appended claims of this application.
Claims
1. A method for manufacturing a carbon fiber composite blade, comprising: (1) Installing carbon fiber yarn, suture thread and carbon fiber surface felt substrate on a fiber variable angle seam laying device; (2) Software is used to draw the fiber laying path, set the stitching density, and the fiber variable angle laying equipment lays the carbon fiber onto the substrate according to the planned path to obtain a blade preform; (3) placing the preform into a metal mold, preparing a composite blade blank by a vacuum-assisted resin transfer molding process, and cutting and polishing the blade blank to obtain a finished blade; In step (2), the carbon fiber laying path is: a bundle of carbon fibers is laid layer by layer, and the laying width of each layer decreases by 1-3 mm from bottom to top, so as to obtain a preform that is thick in the middle and thin at both ends; The suture thread comprises aramid fiber, polyethylene fiber, PBO fiber, polyester, nylon or acrylic fiber, and the linear density does not exceed 3000 D; In step (1), the linear density of the carbon fiber is not more than 800 tex; The grade specifications of the carbon fiber include T300-1K, T300-3K, T300-6K, T700-12K, T800-6K, T800-12K, T1000-12K, M40-6K, M40-12K, M46-6K, M46-12K, M50-6K, M55-6K, M60-3K or M60-6K; In step (1), the carbon fiber surface felt substrate is used as a stitching substrate, and the surface density does not exceed 50 g / m 2 ; In step (2), the stitching density includes 3×3, 5×5 or 8×8 mm; In step (3), a layer of T300-3K carbon fiber woven cloth or prepreg is laid on the surface of the female mold and the male mold of the metal mold, and the fiber surface density does not exceed 240 g / m 2 .
2. The method for manufacturing a carbon fiber composite material blade according to claim 1, characterized in that: In step (3), after the resin transfer molding process is completed, the pressure of the resin transfer molding process equipment is unloaded, and the equipment is re-pressed, vacuumed, and injected. The steps are repeated 2-3 times.
3. The method for manufacturing a carbon fiber composite material blade according to claim 1, characterized in that: In step (3), the surface of the blade blank after demoulding is polished with 500-1500# sandpaper, and then the blade blank is put into the mold again for glue injection and heating and curing.
4. A carbon fiber composite material blade is prepared according to the method for manufacturing a carbon fiber composite material blade according to any one of claims 1 to 3.