A kind of high elastic one-way moisture-conducting cycling jersey fabric for children and preparation method thereof

By using a specific proportion of high moisture-absorbent polyester, ordinary polyester and fine-denier spandex in children's cycling clothing fabrics, combined with high-knitting and dyeing, finishing and printing processes, the problem of high elasticity and moisture absorption and quick-drying in the existing technology is solved. problem, achieving an excellent balance of comfortable elasticity, sweat wicking and moisture absorption and quick-drying properties of the fabric.

CN114717736BActive Publication Date: 2024-10-11XIAMEN ANTA SPORTS GOODS CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202111668142.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-30
Publication Date
2024-10-11
Estimated Expiration
2041-12-30

AI Technical Summary

Technical Problem

It is difficult to combine high elasticity, moisture absorption, quick drying and sun protection properties in children's cycling clothing fabrics with existing technology. High spandex content will affect the moisture absorption properties of the fabric, and existing fabrics usually have a thick double-layer structure and are not suitable for sports purposes.

Method used

By selecting a specific proportion of high moisture-absorbent polyester, ordinary polyester and fine-denier spandex, and using a 40-needle high-knitting weaving process, combined with dyeing and finishing and one-way moisture-conducting printing processes, the fabric is comfortable, elastic, sweat-wicking, moisture-absorbing and quick-drying. The best balance of sun protection properties.

Benefits of technology

The prepared one-way moisture-guided cycling jersey fabric has an elastic recovery rate of 90% to 95%, an elastic modulus of 110% to 150%, a one-way transmission index of 400% to 1200%, and an evaporation rate of 0.3g/h to 0.4 g/h, to meet the needs of children's cycling clothing and achieve an excellent balance of comfort, elasticity, sweat wicking, moisture absorption and quick drying.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0003649582270000193
    Figure GDA0003649582270000193
  • Figure GDA0003649582270000201
    Figure GDA0003649582270000201
  • Figure GDA0003649582270000214
    Figure GDA0003649582270000214
Patent Text Reader

Abstract

The present invention provides a one-way moisture-conducting cycling jersey fabric, comprising a fabric body interwoven with two polyester yarns and spandex yarns; the polyester accounts for 80% to 90% of the fabric by mass; the spandex accounts for 10% to 20% of the fabric by mass. The present invention selects a certain proportion of high-hygroscopic polyester, ordinary polyester and fine-denier spandex for blending, and then prepares a high-elasticity and high-density fabric through a 40-needle high-knitting process, and finally undergoes a special dyeing and printing process to achieve the best balance of the fabric in terms of comfort, elasticity, perspiration, moisture absorption and quick drying, sun protection and other properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of one-way moisture-conducting cycling jersey fabrics, and relates to one-way moisture-conducting cycling jersey fabrics and a preparation method thereof, and in particular to one-way moisture-conducting cycling jersey fabrics with high elasticity for children and a preparation method thereof. Background Art

[0002] Balance bikes are one of the most popular sports for children aged 3 to 6 in China, but major sports brands on the market do not sell products specifically for children's cycling wear, which is also a blank area in the current market. According to survey data from international authoritative consulting agencies, the younger the child, the more frequently they go out in the summer. For preschool children (before the age of 6), more than 70% go out to play every day (49% to 55%) or every other day (21% to 22%). Skin problems such as prickly heat and eczema are the most common health problems for children in the summer, followed by colds and chills caused by sweating due to the hot summer weather. Sunburn, colds due to untimely sweating, and smelly sweat are the three major health problems that parents are mainly worried about and troubled by. More than 90% of parents have taken a series of measures to address their children's summer health problems. The first solution is to choose professional sportswear with sweat-wicking function for their children, accounting for 60%.

[0003] Therefore, in view of the major health problems faced by children during exercise and the major health problems that parents worry about, combined with the physiological characteristics of children and the characteristics of cycling, children's cycling fabrics must have the following characteristics:

[0004] (1) The fabric should be very skin-friendly and comfortable to reduce friction with the skin;

[0005] (2) The fabric should be highly elastic and non-oppressive, maintaining comfort while avoiding any impact on children’s growth and development;

[0006] (3) The fabric should have better moisture wicking and quick-drying properties;

[0007] (4) The fabric should have better UV resistance to prevent children’s skin from being sunburned.

[0008] Therefore, how to provide a fabric that combines the functions of comfort, elasticity, perspiration, moisture absorption and quick drying, sun protection and is suitable for children's cycling clothes, and solve the problem that the current stretch fabrics have contradictions and cannot have the functions of moisture absorption, quick drying and perspiration, has become one of the urgent problems to be solved by many R&D companies and front-line researchers in the industry. Summary of the invention

[0009] In view of this, the technical problem to be solved by the present invention is to provide a one-way moisture-conducting cycling jersey fabric and a preparation method thereof, in particular, a preparation method of a high-elastic one-way moisture-conducting cycling jersey fabric for children. The present invention selects a certain proportion of high-hygroscopic polyester, ordinary polyester and fine-denier spandex for blending, and then prepares a high-elastic and high-density fabric through a 40-needle high-knitting process, and finally undergoes a special dyeing and printing process to achieve the best balance of the fabric's performance in terms of comfort, elasticity, perspiration, moisture absorption and quick drying, and sun protection.

[0010] The present invention provides a one-way moisture-conducting cycling jersey fabric, comprising a fabric body interwoven with two polyester yarns and a spandex yarn;

[0011] The polyester accounts for 80% to 90% of the fabric by mass;

[0012] The spandex accounts for 10% to 20% of the fabric mass.

[0013] Preferably, the two polyesters include highly hygroscopic polyester and polyester;

[0014] The mass ratio of the highly hygroscopic polyester to the two polyesters is 50% to 60%;

[0015] The fabric structure is a polyester-covered polyester-spandex single-sided plain weave structure;

[0016] The moisture regain of the highly hygroscopic polyester is 1.6% to 2.0%;

[0017] The moisture regain of the polyester is 0.3% to 0.5%;

[0018] The specification of the polyester yarn is 50D / 36F or 70D / 48F;

[0019] The spandex includes fine denier spandex;

[0020] The density of the spandex yarn is 20D.

[0021] Preferably, in the polyester-covered polyester-spandex single-sided plain weave structure, the face yarn is highly hygroscopic iterative polyester, and the bottom yarn is polyester and spandex;

[0022] The glass transition temperature of the highly hygroscopic polyester is 62-67°C;

[0023] In the highly hygroscopic polyester, the mass content of titanium dioxide is 2% to 4%;

[0024] The highly hygroscopic polyester is highly hygroscopic iterated polyester;

[0025] The fabric weight is 160-180 g / m 2 ;

[0026] The number of interwoven weaving needles is 36 needles, 40 needles or 44 needles;

[0027] The fabric body is a single-sided fabric;

[0028] The one-way moisture-conducting cycling jersey fabric includes a children's high-elastic one-way moisture-conducting cycling jersey fabric;

[0029] The one-way moisture transfer index of the one-way moisture conduction cycling clothing fabric is 400% to 1200%.

[0030] Preferably, the fabric body is compounded with an absorbent and draining finishing agent;

[0031] The suction and discharge finishing agent includes a composite emulsion of a non-ionic hydrophilic polymer and polysiloxane;

[0032] The fabric is a fabric with a hydrophilic front side and a discontinuous water-repellent area on the back side;

[0033] On the reverse side of the fabric, the area ratio of the water-repellent region is 50% to 80%, and the area ratio of the hydrophilic region is 20% to 50%;

[0034] The water-repellent region includes a printed region;

[0035] The fabric is obtained by subjecting the fabric raw material to two moisture absorption and perspiration treatments;

[0036] The two moisture absorption and perspiration treatments include moisture absorption and perspiration finishing and moisture absorption and perspiration shaping;

[0037] A unidirectional moisture conduction printing step is included between the two moisture absorption and perspiration treatment steps.

[0038] The present invention also provides a method for preparing a one-way moisture-conducting cycling jersey fabric, comprising the following steps:

[0039] 1) Weaving high-hygroscopic polyester yarn, polyester yarn and spandex yarn to obtain a fabric body;

[0040] 2) dyeing and finishing the fabric body obtained in the above steps to obtain a dyed and finished fabric body;

[0041] The dyeing and finishing process includes a moisture absorption and perspiration finishing step;

[0042] 3) The dyed and finished fabric body obtained in the above steps is subjected to one-way moisture-conducting printing and moisture-absorbing and perspiration-releasing shaping treatment to obtain a one-way moisture-conducting cycling jersey fabric.

[0043] Preferably, the weaving method includes circular weft knitting;

[0044] The specific process of dyeing and finishing includes: one or more steps of refining, degreasing, washing, pre-forming, dyeing, reduction cleaning, moisture absorption and perspiration finishing and drying;

[0045] The water washing speed of the refining and degreasing water washing step is 15 to 30 m / min;

[0046] The pH value of the cloth surface in the refining, degreasing and washing step is ≤7.5;

[0047] The pre-forming temperature is 180-190°C;

[0048] The speed of the preforming is 18-30 m / min.

[0049] Preferably, the dyeing bath ratio is 1:(10-20);

[0050] The dye bath formula for dyeing comprises:

[0051] Disperse dyes: 0.1~5owf;

[0052] Dispersant: 0.5~2g / L;

[0053] Acetic acid: 0.5-2 g / L;

[0054] water;

[0055] The pH value of the dyeing solution is 5 to 7;

[0056] The temperature of the reduction cleaning is 60-90°C;

[0057] The reduction cleaning time is 10 to 30 minutes.

[0058] Preferably, the moisture absorption and perspiration finishing time is 5 to 10 minutes;

[0059] The bath ratio of the moisture absorption and perspiration finishing is 1: (10-20);

[0060] The moisture-wicking finishing agent for moisture-wicking finishing comprises a composite emulsion of a nonionic hydrophilic polymer and polysiloxane;

[0061] The concentration of the moisture wicking finishing agent for the moisture wicking finishing is 1 to 3 g / L;

[0062] The drying temperature is 150-180°C;

[0063] The drying speed is 10-20 m / min.

[0064] Preferably, the unidirectional wet-conducting printing process includes a rotary screen printing process;

[0065] The viscosity of the printing paste for unidirectional wet-conducting printing is 800 to 1500 centipoise;

[0066] The printing paste formula of the one-way wet-conducting printing comprises

[0067] C6 water repellent 80~120g / L;

[0068] Water repellent enhancer 5-20g / L;

[0069] Thickener 5-20g / L;

[0070] water;

[0071] The C6 water repellent comprises C6 fluorocarbon resin;

[0072] The water repellent synergist includes a cationic block copolyisocyanate;

[0073] The thickener includes sodium alginate and / or polyacrylic acid resin.

[0074] Preferably, the bath ratio of the moisture absorption and perspiration setting is 1:(10-20);

[0075] The moisture absorption and perspiration setting agent formula comprises

[0076] Moisture wicking finishing agent 20-40g / L;

[0077] Softener 30~60g / L;

[0078] water;

[0079] The setting temperature of the moisture absorption and perspiration setting is 150-180°C;

[0080] The speed of moisture absorption and perspiration shaping is 10-20 m / min.

[0081] The present invention also provides the use of the one-way moisture-conducting cycling jersey fabric described in any one of the above technical solutions or the one-way moisture-conducting cycling jersey fabric prepared by the preparation method described in any one of the above technical solutions in children's cycling.

[0082] The present invention provides a one-way moisture-conducting cycling clothing fabric, including a fabric body interwoven with two polyester yarns and spandex yarns; the polyester accounts for 80% to 90% of the fabric mass; the spandex accounts for 10% to 20% of the fabric mass. Compared with the prior art, the present invention is aimed at the fact that the existing knitted fabrics are difficult to meet the application of children's cycling in terms of comprehensive performance. Although some research schemes are also disclosed in the prior art, such as the weaving and dyeing method of the one-way moisture-conducting elastic fabric disclosed in patent CN108301234A, the one-way moisture-conducting elastic fabric is a double-layer structure, the surface layer is made of hydrophilic easy-to-dye fiber, and the inner layer is made of polypropylene liquid-dyed yarn. It is mainly through the one-way moisture-conducting function of the hydrophilic and hydrophobic difference yarns of the surface layer hydrophilic fiber and the inner layer elastic water-repellent fiber. And the one-way moisture-conducting elastic fabric and its manufacturing method disclosed in patent CN110079928A, through special weft knitting process, directly weaves a cylindrical garment or white fabric with an inner surface and an outer surface, wherein the inner surface includes a protrusion with a smaller F number, and each protrusion is connected to a diffusion, when the inner surface contacts the skin sweat, the sweat is absorbed by the loose pores of the protrusion, and the siphon effect is used to quickly discharge the sweat through countless relatively loose pores to the diffusion surface of the one-way moisture-conducting elastic fabric, so as to achieve the effect of strong sweat absorption and moisture discharge, and spandex is added to the yarn, and the fabric itself has excellent elastic effect. The present invention believes that there are two main ways to prepare high-elastic single-conducting fabrics at present, one is to achieve the combination of high elasticity and single-conductivity by weaving, this fabric is usually a double-layer structure, and spandex yarn is used in the weaving process, and the single-conductivity effect is achieved by using yarns with different hydrophilicity and hydrophobicity on the front and back sides or by using a weaving process to make the front and back sides present a high and low F number difference to achieve the single-conductivity effect. The main disadvantage of this technology is that the fabric must be a double-layer structure, and the woven fabric is relatively thick and not suitable for sports; at the same time, spandex will significantly reduce the moisture absorption and quick-drying performance of the fabric. Another method is to use spandex yarn to weave elastic fabrics, and then achieve the function of high elasticity and single guide through single guide printing. In this technology, the high spandex content will prevent the transfer of sweat from the skin-friendly side to the front side, greatly affecting the single guide performance of the fabric. At the same time, spandex will reduce the moisture absorption and quick-drying performance of the fabric. However, high elasticity requires a high spandex content, which is also a dilemma faced by the existing technology.

[0083] Based on this, the present invention provides a one-way moisture-conducting cycling jersey fabric with a specific structure and composition. This is a high-elastic one-way cycling jersey fabric, which is a mixed woven structure of a certain proportion of high-hygroscopic polyester, ordinary polyester and fine-denier spandex. Since spandex is non-hygroscopic, the more its content is, the more it will affect the one-way moisture-conducting and moisture-absorbing properties of the fabric. Too little content will affect the elasticity of the fabric, so it is very important to select a suitable ratio. At the same time, the present invention uses high-hygroscopic polyester with a regain of 1.6% in the veil, and conventional polyester with a regain of 0.4% in the bottom yarn. Due to the difference in hydrophilicity and hydrophobicity between the front and back sides of the fabric, the differential capillary effect can greatly improve the moisture absorption and perspiration capacity of the entire fabric, making up for the negative impact of spandex. Moreover, under normal circumstances, the fabric before single-guide printing is not subjected to moisture absorption and perspiration finishing, which will affect the impact of subsequent water-repellent printing. However, the fabric described in the present invention has a high spandex content. Spandex itself does not absorb moisture and will hinder the moisture conduction effect, so an absorption and discharge finishing is carried out during the dyeing and finishing process, and an absorption and discharge shaping is carried out after single conduction. The fabric prepared by this process not only has a very good perspiration effect, but also has a very high moisture absorption and quick-drying effect. The hygroscopicity of the fabric will not be affected by the high spandex content, and the problem that it is difficult to achieve both high elasticity and moisture absorption and quick drying is effectively solved.

[0084] The present invention selects a certain proportion of high-hygroscopic polyester, ordinary polyester and fine-denier spandex for blending, and then prepares a high-elasticity and high-density fabric through a 40-needle high-knitting process, and finally undergoes a special dyeing and printing process to achieve the best balance of the fabric's properties in terms of comfort, elasticity, perspiration, moisture absorption and quick drying, and sun protection.

[0085] Experimental results show that the one-way moisture-conducting cycling clothing fabric prepared by the present invention has an elastic recovery rate of 90% to 95%, an elasticity of 110% to 150%, a one-way transmission index of 400% to 1200%, and an evaporation rate of 0.3g / h to 0.4g / h, achieving an excellent balance in comfort, elasticity, perspiration, moisture absorption and quick drying, and can meet the needs of children's cycling clothing fabrics. DETAILED DESCRIPTION

[0086] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention.

[0087] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0088] There is no particular restriction on the purity of all raw materials in the present invention. The present invention preferably uses industrial purity or conventional purity used in the field of knitted fabrics.

[0089] The present invention provides a one-way moisture-conducting cycling jersey fabric, comprising a fabric body interwoven with two polyester yarns and a spandex yarn;

[0090] In the present invention, the two polyesters preferably include high-hygroscopic polyester and polyester. Specifically, the polyester is ordinary polyester or conventional polyester. More specifically, the high-hygroscopic polyester can be high-hygroscopic iterated polyester (iteration TM Polyester).

[0091] In the present invention, the mass ratio of the high moisture-absorbent polyester to the two polyesters is preferably 50% to 60%, more preferably 52% to 58%, and more preferably 54% to 56%.

[0092] In the present invention, the moisture regain of the highly hygroscopic polyester is preferably 1.6% to 2.0%, more preferably 1.65% to 1.95%, more preferably 1.7% to 1.9%, and more preferably 1.75% to 1.85%.

[0093] In the present invention, the mass content of titanium dioxide in the highly hygroscopic polyester is preferably 2% to 4%, more preferably 2.4% to 3.6%, and more preferably 2.8% to 3.2%.

[0094] In the present invention, the glass transition temperature of the highly hygroscopic polyester is preferably 62 to 67°C, more preferably 63 to 66°C, and even more preferably 64 to 65°C.

[0095] In the present invention, the moisture regain of the polyester, ie, ordinary polyester or conventional polyester, is preferably 0.3% to 0.5%, more preferably 0.33% to 0.48%, more preferably 0.35% to 0.45%, more preferably 0.38% to 0.43%.

[0096] In the present invention, the mass ratio of the polyester to the fabric is 80% to 90%, preferably 82% to 88%, and more preferably 84% to 86%.

[0097] The spandex accounts for 10% to 20% of the fabric mass, preferably 12% to 18%, and more preferably 14% to 16%.

[0098] In the present invention, the fabric body is preferably a single-sided fabric.

[0099] In the present invention, the structure of the fabric body is preferably a polyester-covered polyester-spandex single-sided plain weave structure. The definition of polyester-covered polyester-spandex is similar to the definition of cotton-covered silk in the art. The fabric body is a single-sided plain weave woven structure. Specifically, in the polyester-covered polyester-spandex single-sided plain weave structure, the face yarn is highly hygroscopic iterated polyester, and the bottom yarn is polyester (conventional polyester) and spandex.

[0100] In the present invention, the specification of the polyester yarn is preferably 50D / 36F or 70D / 48F.

[0101] In the present invention, the spandex preferably includes fine denier spandex.

[0102] In the present invention, the density of the spandex yarn is preferably 20D.

[0103] In the present invention, the weight of the fabric is preferably 160 to 180 g / m 2 , more preferably 164 to 176 g / m 2 , more preferably 168 to 172 g / m 2 .

[0104] In the present invention, the number of interlaced weaving needles is preferably 36 needles, 40 needles or 44 needles.

[0105] In the present invention, the fabric body is preferably compounded with an absorption and discharge finishing agent. Specifically, the fabric body is compounded with a dye. The dyed fabric body is compounded with an absorption and discharge finishing agent or the dye is compounded with an absorption and discharge finishing agent.

[0106] In the present invention, the suction and drainage finishing agent preferably includes a compound emulsion of a non-ionic hydrophilic polymer and polysiloxane. The suction and drainage finishing agent is preferably a non-ionic hydrophilic polymer-polysiloxane suction and drainage finishing agent. Specifically, the suction and drainage finishing agent can be a FERAN ICS suction and drainage finishing agent.

[0107] In the present invention, the fabric is preferably a fabric with a hydrophilic front side and a discontinuous water-repellent region on the back side.

[0108] In the present invention, the area ratio of the water-repellent region on the reverse side of the fabric is preferably 50% to 80%, more preferably 55% to 75%, more preferably 60% to 70%. The area ratio of the hydrophilic region is preferably 20% to 50%, more preferably 25% to 45%, more preferably 30% to 40%.

[0109] In the present invention, the water-repellent region preferably includes a printed region.

[0110] In the present invention, the fabric is preferably obtained by subjecting the fabric raw material to two moisture absorption and perspiration treatments.

[0111] In the present invention, the two moisture wicking treatments preferably include moisture wicking finishing and moisture wicking shaping.

[0112] In the present invention, a unidirectional moisture conduction printing step is preferably included between the two moisture absorption and perspiration treatment steps.

[0113] In the present invention, on the reverse side of the fabric body, on the fabric with the discontinuous water-repellent region, the surface of the absorption and discharge finishing agent is further compounded with a water-repellent material.

[0114] In the present invention, the one-way moisture-conducting cycling jersey fabric preferably includes a high-elastic one-way moisture-conducting cycling jersey fabric, and more preferably a high-elastic one-way moisture-conducting cycling jersey fabric for children.

[0115] In the present invention, the one-way moisture transfer index of the one-way moisture conduction cycling jersey fabric is preferably 400% to 1200%, more preferably 500% to 1100%, more preferably 600% to 1000%, and more preferably 700% to 900%.

[0116] In the present invention, the evaporation rate of the one-way moisture-conducting cycling jersey fabric is preferably 0.3 g / h to 0.4 g / h, more preferably 0.32 g / h to 0.38 g / h, and more preferably 0.34 g / h to 0.36 g / h.

[0117] In the present invention, the elastic recovery rate of the one-way moisture-conducting cycling jersey fabric is preferably 90% to 95%, more preferably 91% to 94%, and more preferably 92% to 93%.

[0118] In the present invention, the elasticity of the one-way moisture-conducting cycling jersey fabric is preferably 110% to 150%, more preferably 115% to 145%, more preferably 120% to 140%, and more preferably 125% to 135%.

[0119] The present invention provides a method for preparing a one-way moisture-conducting cycling jersey fabric, comprising the following steps:

[0120] 1) Weaving high-hygroscopic polyester yarn, polyester yarn and spandex yarn to obtain a fabric body;

[0121] 2) dyeing and finishing the fabric body obtained in the above steps to obtain a dyed and finished fabric body;

[0122] The dyeing and finishing process includes a moisture absorption and perspiration finishing step;

[0123] 3) The dyed and finished fabric body obtained in the above steps is subjected to one-way moisture-conducting printing and moisture-absorbing and perspiration-releasing shaping treatment to obtain a one-way moisture-conducting cycling jersey fabric.

[0124] The invention firstly weaves high-hygroscopic polyester yarn, polyester yarn and spandex yarn to obtain a fabric body.

[0125] In the present invention, the weaving method preferably includes circular weft knitting.

[0126] The present invention further dyes and finishes the fabric body obtained in the above steps to obtain a dyed and finished fabric body.

[0127] The dyeing and finishing process includes a moisture absorption and perspiration finishing step.

[0128] In the present invention, the specific process flow of dyeing and finishing preferably includes: one or more steps of refining and degreasing water washing, pre-forming, dyeing, reduction cleaning, moisture absorption and perspiration finishing and drying steps, more preferably multiple steps of refining and degreasing water washing, pre-forming, dyeing, reduction cleaning, moisture absorption and perspiration finishing and drying steps.

[0129] In the present invention, the water washing speed in the refining and deoiling water washing step is preferably 15 to 30 m / min, more preferably 18 to 27 m / min, and more preferably 21 to 24 m / min.

[0130] In the present invention, the pH value of the cloth in the refining, degreasing and water washing step is preferably ≤7.5, more preferably ≤7, and more preferably ≤6.5.

[0131] In the present invention, the pre-forming temperature is preferably 180-190°C, more preferably 182-188°C, and more preferably 184-186°C.

[0132] In the present invention, the preforming speed is preferably 18 to 30 m / min, more preferably 12 to 28 m / min, more preferably 14 to 26 m / min, more preferably 16 to 24 m / min, more preferably 18 to 22 m / min.

[0133] Finally, the present invention subjects the dyed and finished fabric body obtained in the above steps to unidirectional moisture-conducting printing and moisture absorption and perspiration shaping treatment to obtain a unidirectional moisture-conducting cycling clothing fabric.

[0134] In the present invention, the bath ratio of dyeing is preferably 1:(10-20), more preferably 1:(12-18), and more preferably 1:(14-16).

[0135] In the present invention, the dyeing bath formula preferably includes:

[0136] Disperse dyes: 0.1~5owf;

[0137] Dispersant: 0.5~2g / L;

[0138] Acetic acid: 0.5-2 g / L;

[0139] water.

[0140] Specifically, the disperse dye is preferably 0.1 to 5 owf, more preferably 1 to 4 owf, more preferably 5 to 3 owf, and more preferably 10 to 2 owf.

[0141] The dispersant is preferably 0.5 to 2 g / L, more preferably 0.8 to 1.7 g / L, and more preferably 1.1 to 1.4 g / L.

[0142] The acetic acid is preferably 0.5 to 2 g / L, more preferably 0.8 to 1.7 g / L, and more preferably 1.1 to 1.4 g / L.

[0143] In the present invention, the pH value of the dyeing solution is preferably 5 to 7, more preferably 5.4 to 6.6, and more preferably 5.8 to 6.2.

[0144] In the present invention, the temperature of the reduction cleaning is preferably 60 to 90°C, more preferably 65 to 85°C, and more preferably 70 to 80°C.

[0145] In the present invention, the reduction cleaning time is preferably 10 to 30 minutes, more preferably 14 to 26 minutes, and more preferably 18 to 22 minutes.

[0146] In the present invention, the time for the moisture absorption and perspiration removal finishing is preferably 5 to 10 minutes, more preferably 6 to 9 minutes, and more preferably 7 to 8 minutes.

[0147] In the present invention, the bath ratio of the moisture absorption and perspiration finishing is preferably 1: (10-20), more preferably 1: (12-18), and more preferably 1: (14-16).

[0148] In the present invention, the moisture-wicking finishing agent for moisture-wicking finishing preferably comprises a composite emulsion of a nonionic hydrophilic polymer and polysiloxane.

[0149] In the present invention, the concentration of the moisture wicking finishing agent for moisture wicking finishing is preferably 1 to 3 g / L, more preferably 1.4 to 2.6 g / L, and more preferably 1.8 to 2.2 g / L.

[0150] In the present invention, the drying temperature is preferably 150-180°C, more preferably 155-175°C, and more preferably 160-170°C.

[0151] In the present invention, the drying speed is preferably 10 to 20 m / min, more preferably 12 to 18 m / min, and more preferably 14 to 16 m / min.

[0152] In the present invention, the unidirectional wet-conducting printing process preferably includes a rotary screen printing process.

[0153] In the present invention, the viscosity of the printing paste for unidirectional wet-conducting printing is preferably 800 to 1500 centipoise, more preferably 900 to 1400 centipoise, more preferably 1000 to 1300 centipoise, and more preferably 1100 to 1200 centipoise.

[0154] In the present invention, the printing paste formula for unidirectional wet-conducting printing preferably includes

[0155] C6 water repellent 80~120g / L;

[0156] Water repellent enhancer 5-20g / L;

[0157] Thickener 5-20g / L;

[0158] water.

[0159] Specifically, the C6 water repellent preferably includes C6 fluorocarbon resin. The amount of the C6 water repellent added is preferably 80 to 120 g / L, more preferably 85 to 115 g / L, more preferably 90 to 110 g / L, and more preferably 95 to 105 g / L.

[0160] The water repellent synergist preferably comprises a cationic blocked copolyisocyanate. The amount of the water repellent synergist added is preferably 5 to 20 g / L, more preferably 8 to 17 g / L, and more preferably 11 to 14 g / L.

[0161] The thickener includes sodium alginate and / or polyacrylic acid resin, more preferably sodium alginate or polyacrylic acid resin. The amount of the water repellent enhancer added is preferably 5-20 g / L, more preferably 8-17 g / L, more preferably 11-14 g / L.

[0162] In the present invention, the bath ratio of moisture absorption and perspiration setting is preferably 1: (10-20), more preferably 1: (12-18), and more preferably 1: (14-16).

[0163] In the present invention, the moisture absorption and perspiration setting agent formula preferably includes

[0164] Moisture wicking finishing agent 20-40g / L;

[0165] Softener 30~60g / L;

[0166] water.

[0167] Specifically, the amount of the moisture absorption and perspiration finishing agent added is preferably 20 to 40 g / L, more preferably 24 to 36 g / L, and more preferably 28 to 32 g / L.

[0168] The amount of the softener added is preferably 30 to 60 g / L, more preferably 35 to 55 g / L, and more preferably 40 to 50 g / L.

[0169] In the present invention, the setting temperature of the moisture absorption and perspiration setting is preferably 150-180°C, more preferably 155-175°C, and more preferably 160-170°C.

[0170] In the present invention, the speed of moisture absorption and perspiration setting is preferably 10 to 20 m / min, more preferably 12 to 18 m / min, and more preferably 14 to 16 m / min.

[0171] The present invention is to complete and refine the overall preparation process, better ensure the structure and morphology of the one-way moisture-conducting cycling jersey fabric, and improve the comprehensive performance of the one-way moisture-conducting cycling jersey fabric. The preparation method of the one-way moisture-conducting cycling jersey fabric can specifically include the following steps:

[0172] The present invention mainly comprises the following steps:

[0173] 1. Weaving

[0174] Highly hygroscopic polyester, polyester and spandex are interwoven in a certain proportion on a circular weft knitting machine. The fabric structure is a polyester-covered polyester-spandex plain weave structure. The veil is made of highly hygroscopic iterated polyester, and the base yarn is made of ordinary polyester and spandex. Among them, the highly hygroscopic iterated polyester accounts for 50% to 60%, the total polyester accounts for 80% to 90%, and the spandex accounts for 10% to 20%. The titanium dioxide content in the highly hygroscopic iterated polyester is 2% to 4%, the regain is 1.6%, the glass transition temperature is 62℃ to 67℃, and the preferred specification is 50D / 36F; the preferred specification of ordinary polyester is 50D / 36F, the preferred spandex is 20D, and the gram weight is 160 to 180g / m 2 .

[0175] 2. Dyeing and finishing

[0176] The fabric obtained in step 1 is dyed and finished, and the dyeing and finishing process is: refining and degreasing water washing - pre-forming - dyeing - reduction cleaning - moisture absorption and perspiration finishing - drying

[0177] (1) Refining, degreasing and water washing

[0178] Select a continuous heated spray pre-shrinkage washing machine with a speed of 15 to 30 m / min. The refining formula is: 20 to 30 g / l of high-efficiency refining emulsifier, the emulsifier type is a multi-polymerized multifunctional fatty alcohol or ether non-ionic surfactant, 2 g / l of soda ash, and the pH value of the cloth surface is ≤7.5.

[0179] (2) Pre-form

[0180] Pre-setting process: water through the roller, setting machine temperature 180-190℃, speed 18-30m / min, overfeed 15%, liquid carrying rate controlled at 75%-100%. Since the polyester in the fabric is highly hygroscopic, it will become hard after high temperature, so the setting temperature cannot be higher than 190℃.

[0181] (3) Dyeing

[0182] Immerse the pre-shaped fabric in a 40℃ dye bath with a dye bath ratio of 1:10-1:20, keep the temperature constant for 10-15min, then increase the temperature to 50℃ at a rate of 1.5-2℃, keep the temperature constant for 10min, and finally increase the temperature to 100-115℃ at a rate of 1℃ / min, keep the temperature constant for 10-60min.

[0183] The dye bath formula is:

[0184] Disperse dyes: 0.1~5owf;

[0185] Dispersant: 0.5-2 g / L, dispersant type is aromatic carboxylic acid monoester;

[0186] Acetic acid: 0.5-2g / L, the pH value of the dye solution is controlled at 5-7.

[0187] (4) Reduction cleaning

[0188] Drain the dyeing solution after dyeing, and continue to perform reduction cleaning, the reduction cleaning bath ratio is 1:10-20, heat to 80°C, keep warm for 10-30 minutes and then drain. The reduction cleaning solution includes: 0.3-0.5g / L soda ash, 1-3g / L reducing agent, wherein the reducing agent is hydrosulfite or thiourea dioxide.

[0189] (5) Moisture wicking finishing

[0190] The fabric after reduction cleaning is subjected to moisture absorption and perspiration finishing in a tub, the absorption and perspiration finishing bath ratio is 1:10-20, the finishing bath temperature is room temperature, the processing time is 5-10 minutes, and the finishing liquid includes: 1-3g / l of absorption and perspiration finishing agent, and the rest is water. Among them, the absorption and perspiration finishing agent is a compound emulsion of non-ionic hydrophilic polymer and polysiloxane.

[0191] (6) Drying

[0192] The drying temperature is 150-180°C and the drying speed is 10-20m / min.

[0193] 3. Single guide printing

[0194] The fabric after suction and drainage finishing is subjected to single-guide printing, that is, the reverse side of the fabric is subjected to water-repellent treatment to form a discontinuous water-repellent area. The process of the single-guide printing: preferably the rotary screen printing process, the area of ​​the water-repellent area is 50% to 80%, the area of ​​the hydrophilic area is 20% to 50%, and the drying speed is 8 to 15 m / min. The formula of single-guide printing: the dosage of C6 water-repellent agent is 80 to 120 g / L, the dosage of water-repellent enhancer is 5 to 20 g / L, the dosage of thickener is 5 to 20 g / L, the balance is water, and the viscosity of the printing slurry is 800 to 1500 centipoise. Among them, the water-repellent agent is C6 fluorocarbon resin, the water-repellent enhancer is cationic block copolymer isocyanate, and the thickener is sodium alginate or polyacrylic acid resin.

[0195] 4. Suction and discharge shaping

[0196] The fabric after single-guide printing is subjected to moisture absorption and perspiration setting treatment, and the setting formula is: 20-40g / L of moisture absorption and perspiration finishing agent, which is a compound emulsion of non-ionic hydrophilic polymer and polysiloxane, 30-60g / L of softener, which is polyvinyl alcohol, and the balance is water. The setting temperature is 150-180℃, and the speed is 10-20m / min.

[0197] After the shaping is completed, a high-elastic single-guide cycling jersey fabric is obtained.

[0198] The present invention mainly achieves the best balance of the fabric's properties in terms of comfort, elasticity, perspiration, moisture absorption, quick drying, sun protection, etc. by selecting a certain proportion of high-hygroscopic polyester, ordinary polyester and fine-denier spandex for blending, and then preparing a high-elastic and high-density fabric through a 40-needle high-knitting process, and finally undergoing a special dyeing and printing process.

[0199] The present invention also provides the use of the one-way moisture-conducting cycling jersey fabric described in any one of the above technical solutions or the one-way moisture-conducting cycling jersey fabric prepared by the preparation method described in any one of the above technical solutions in children's cycling.

[0200] The above steps of the present invention provide a high-elastic one-way moisture-conducting cycling jersey fabric for children and a preparation method thereof. The one-way moisture-conducting cycling jersey fabric with a specific structure and composition is a mixed structure of a certain proportion of high-hygroscopic polyester, ordinary polyester and fine-denier spandex. Since spandex is non-hygroscopic, the more the content is, the more it will affect the one-way moisture-conducting and moisture-absorbing properties of the fabric. Too little content will affect the elasticity of the fabric, so it is very important to select a suitable ratio. At the same time, the present invention uses high-hygroscopic polyester with a regain of 1.6% in the veil, and conventional polyester with a regain of 0.4% in the bottom yarn. Due to the difference in hydrophilicity and hydrophobicity between the front and back sides of the fabric, the differential capillary effect can greatly improve the moisture absorption and perspiration capacity of the entire fabric, making up for the negative impact of spandex. Moreover, under normal circumstances, the fabric before single-guide printing is not subjected to moisture absorption and perspiration finishing, which will affect the impact of subsequent water-repellent printing. However, the fabric described in the present invention has a high spandex content. Spandex itself does not absorb moisture and will hinder the moisture conduction effect, so an absorption and discharge finishing is carried out during the dyeing and finishing process, and an absorption and discharge shaping is carried out after single conduction. The fabric prepared by this process not only has a very good perspiration effect, but also has a very high moisture absorption and quick-drying effect. The hygroscopicity of the fabric will not be affected by the high spandex content, and the problem that it is difficult to achieve both high elasticity and moisture absorption and quick drying is effectively solved.

[0201] The present invention selects a certain proportion of high-hygroscopic polyester, ordinary polyester and fine-denier spandex for blending, and then prepares a high-elasticity and high-density fabric through a 40-needle high-knitting process, and finally undergoes a special dyeing and printing process to achieve the best balance of the fabric's properties in terms of comfort, elasticity, perspiration, moisture absorption and quick drying, and sun protection.

[0202] Experimental results show that the one-way moisture-conducting cycling clothing fabric prepared by the present invention has an elastic recovery rate of 90% to 95%, an elasticity of 110% to 150%, a one-way transmission index of 400% to 1200%, and an evaporation rate of 0.3g / h to 0.4g / h, achieving an excellent balance in comfort, elasticity, perspiration, moisture absorption and quick drying, and can meet the needs of children's cycling clothing fabrics.

[0203] In order to further illustrate the present invention, a one-way moisture-conducting cycling jersey fabric and a preparation method thereof provided by the present invention are described in detail below in combination with embodiments. However, it should be understood that these embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operating processes are given only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention, and the protection scope of the present invention is not limited to the following embodiments.

[0204] Example 1

[0205] This embodiment mainly includes the following steps:

[0206] 1. Weaving

[0207] 60% 50D / 36F iterative polyester, 30% 50D / 36F conventional polyester, and 10% 20D spandex are interwoven, of which the iterative polyester is produced by Qingdao Xinwei Textile Development Co., Ltd. and the spandex is produced by South Korea's Hyosung Group. Soft Fit series, the fabric structure is plain single-sided fabric, the fabric weight is 165g / m 2 .

[0208] 2. Dyeing and finishing

[0209] The fabric obtained in step 1 is dyed and finished, and the dyeing and finishing process is: refining and degreasing water washing - pre-forming - dyeing - reduction cleaning - moisture absorption and perspiration finishing - drying

[0210] (1) Refining, degreasing and water washing

[0211] Select a continuous heated spray loose pre-shrinkage washing machine with a speed of 20m / min, refining formula: high-efficiency refining emulsifier 0-15 25g / l, 0-15 is produced by Guangdong Aobo Shun Chemical Co., Ltd., soda ash 2g / l, and the pH value of the cloth surface is 6.9.

[0212] (2) Pre-form

[0213] Pre-forming process: water is passed through the roller, the temperature of the setting machine is 185℃, the speed is 20m / min, the overfeed is 15%, and the liquid rate is controlled at 85%.

[0214] (3) Dyeing

[0215] Immerse the pre-shaped fabric in a 40℃ dye bath with a dye bath ratio of 1:15, keep the temperature constant for 15 minutes, then increase the temperature to 50℃ at a rate of 1.5℃ and keep the temperature constant for 10 minutes, and finally increase the temperature to 105℃ at a rate of 1℃ / min and keep the temperature constant for 30 minutes.

[0216] The dye bath formula is:

[0217] huntsman disperse dyes TERASIL flaming red WW-GS: 1.5owf

[0218] Dispersant: 1g / L, the dispersant is RUCOGAL ERX from Rudolf Chemical

[0219] Acetic acid: 0.5g / L, pH value of dye solution is controlled at 6.5

[0220] (4) Reduction cleaning

[0221] Drain the dyeing solution and continue to perform reduction cleaning, the reduction cleaning bath ratio is 1:15, heat to 80°C, keep warm for 20 minutes and then drain. The reduction cleaning solution includes: 0.5g / l soda ash and 2g / L reduction cleaning agent RUCORIT RGH (produced by Rudolf Chemical).

[0222] (5) Moisture wicking finishing

[0223] The fabric after reduction cleaning is subjected to moisture absorption and perspiration finishing in a tub, the absorption and perspiration finishing bath ratio is 1:15, the finishing bath temperature is room temperature, the treatment time is 10 minutes, and the finishing liquid includes: FERAN ICS 2g / l (produced by Rudolf Chemicals).

[0224] (6) Drying

[0225] The drying temperature is 180°C and the drying speed is 10m / min.

[0226] 3. Single guide printing

[0227] The fabric after suction and discharge is subjected to single-guide printing. The printing pattern is as follows, and the drying speed is 10m / min. The formula for single-guide printing: C6 water repellent dosage 100g / L ( -GUARD AFC6), water repellent synergist 5g / L (Rudolf RUCO-GUARD XCR), thickener dosage 8g / L (Rudolf TH5000), printing paste viscosity is 1200 centipoise.

[0228] 4. Suction and discharge shaping

[0229] The fabric after single-guide printing is subjected to moisture absorption and perspiration setting treatment, and the setting formula is: ICS 30g / L, softener SIH 40g / L (produced by Archroma Chemicals), setting temperature 180℃, and vehicle speed 10m / min.

[0230] After the shaping is completed, a high-elastic single-guide cycling jersey fabric is obtained.

[0231] Comparative Example 1

[0232] Compared with Example 1, the iterative polyester in Comparative Example 1 is replaced with ordinary polyester, and the rest remains unchanged.

[0233] 1. Weaving

[0234] 90% 50D / 36F ordinary polyester and 10% 20D spandex are interwoven, of which the ordinary polyester is produced by Shenghong Group and the spandex is produced by Hyosung Group of South Korea. Soft Fit series, the fabric structure is plain single-sided fabric, the fabric weight is 165g / m 2 .

[0235] 2. Dyeing and finishing

[0236] The fabric obtained in step 1 is dyed and finished, and the dyeing and finishing process is: refining and degreasing water washing - pre-forming - dyeing - reduction cleaning - moisture absorption and perspiration finishing - drying

[0237] (1) Refining, degreasing and water washing

[0238] Select a continuous heated spray loose pre-shrinkage washing machine with a speed of 20m / min, refining formula: high-efficiency refining emulsifier 0-15 25g / l, 0-15 is produced by Guangdong Aobo Shun Chemical Co., Ltd., soda ash 2g / l, and the pH value of the cloth surface is 6.9.

[0239] (2) Pre-form

[0240] Pre-forming process: water is passed through the roller, the temperature of the setting machine is 185℃, the speed is 20m / min, the overfeed is 15%, and the liquid rate is controlled at 85%.

[0241] (3) Dyeing

[0242] Immerse the pre-shaped fabric in a 40℃ dye bath with a dye bath ratio of 1:15, keep the temperature constant for 15 minutes, then increase the temperature to 50℃ at a rate of 1.5℃ and keep the temperature constant for 10 minutes, and finally increase the temperature to 105℃ at a rate of 1℃ / min and keep the temperature constant for 30 minutes.

[0243] The dye bath formula is:

[0244] huntsman disperse dyes TERASIL flaming red WW-GS: 1.5owf

[0245] Dispersant: 1g / L, the dispersant is RUCOGAL ERX from Rudolf Chemical

[0246] Acetic acid: 0.5g / L, pH value of dye solution is controlled at 6.5

[0247] (4) Reduction cleaning

[0248] Drain the dyeing solution and continue to perform reduction cleaning, the reduction cleaning bath ratio is 1:15, heat to 80°C, keep warm for 20 minutes and then drain. The reduction cleaning solution includes: 0.5g / l soda ash and 2g / L reduction cleaning agent RUCORIT RGH (produced by Rudolf Chemical).

[0249] (5) Moisture wicking finishing

[0250] The fabric after reduction cleaning is subjected to moisture absorption and perspiration finishing in a tub, the absorption and perspiration finishing bath ratio is 1:15, the finishing bath temperature is room temperature, the treatment time is 10 minutes, and the finishing liquid includes: FERAN ICS 2g / l (produced by Rudolf Chemicals).

[0251] (6) Drying

[0252] The drying temperature is 180°C and the drying speed is 10m / min.

[0253] 3. Single guide printing

[0254] The fabric after suction and discharge is subjected to single-guide printing. The printing pattern is as follows, and the drying speed is 10m / min. The formula for single-guide printing: C6 water repellent dosage 100g / L ( -GUARD AFC6), water repellent synergist 5g / L (Rudolf RUCO-GUARD XCR), thickener dosage 8g / L (Rudolf TH5000), printing paste viscosity is 1200 centipoise.

[0255] 4. Suction and discharge shaping

[0256] The fabric after single-guide printing is subjected to moisture absorption and perspiration setting treatment, and the setting formula is: ICS 30g / L, softener SIH 40g / L (produced by Archroma Chemicals), setting temperature 180℃, and vehicle speed 10m / min.

[0257] After the shaping is completed, a high-elastic single-guide cycling jersey fabric is obtained.

[0258] Comparative Example 2

[0259] Compared with Example 1, Comparative Example 2 lacks a moisture absorption and perspiration finishing step after reduction cleaning, and the rest remains unchanged.

[0260] 1. Weaving

[0261] 60% 50D / 36F iterative polyester, 30% 50D / 36F conventional polyester, and 10% 20D spandex are interwoven, of which the iterative polyester is produced by Qingdao Xinwei Textile Development Co., Ltd. and the spandex is produced by South Korea's Hyosung Group. Soft Fit series, the fabric structure is plain single-sided fabric, the fabric weight is 165g / m 2 .

[0262] 2. Dyeing and finishing

[0263] The fabric obtained in step 1 is dyed and finished, and the dyeing and finishing process is: refining and degreasing water washing - pre-forming - dyeing - reduction cleaning - moisture absorption and perspiration finishing - drying

[0264] (1) Refining, degreasing and water washing

[0265] Select a continuous heated spray loose pre-shrinkage washing machine with a speed of 20m / min, refining formula: high-efficiency refining emulsifier 0-15 25g / l, 0-15 is produced by Guangdong Aobo Shun Chemical Co., Ltd., soda ash 2g / l, and the pH value of the cloth surface is 6.9.

[0266] (2) Pre-form

[0267] Pre-forming process: water is passed through the roller, the temperature of the setting machine is 185℃, the speed is 20m / min, the overfeed is 15%, and the liquid rate is controlled at 85%.

[0268] (3) Dyeing

[0269] Immerse the pre-shaped fabric in a 40℃ dye bath with a dye bath ratio of 1:15, keep the temperature constant for 15 minutes, then increase the temperature to 50℃ at a rate of 1.5℃ and keep the temperature constant for 10 minutes, and finally increase the temperature to 105℃ at a rate of 1℃ / min and keep the temperature constant for 30 minutes.

[0270] The dye bath formula is:

[0271] huntsman disperse dyes TERASIL flaming red WW-GS: 1.5owf

[0272] Dispersant: 1g / L, the dispersant is RUCOGAL ERX from Rudolf Chemical

[0273] Acetic acid: 0.5g / L, pH value of dye solution is controlled at 6.5

[0274] (4) Reduction cleaning

[0275] Drain the dyeing solution and continue to perform reduction cleaning, the reduction cleaning bath ratio is 1:15, heat to 80°C, keep warm for 20 minutes and then drain. The reduction cleaning solution includes: 0.5g / l soda ash and 2g / L reduction cleaning agent RUCORIT RGH (produced by Rudolf Chemical).

[0276] (5) Drying

[0277] The drying temperature is 180°C and the drying speed is 10m / min.

[0278] 3. Single guide printing

[0279] The fabric after suction and discharge is subjected to single-guide printing. The printing pattern is as follows, and the drying speed is 10m / min. The formula for single-guide printing: C6 water repellent dosage 100g / L ( GUARD AFC6), water repellent synergist 5g / L (Rudolf RUCO-GUARDXCR), thickener dosage 8g / L (Rudolf TH5000), printing paste viscosity is 1200 centipoise.

[0280] 4. Suction and discharge shaping

[0281] The fabric after single-guide printing is subjected to moisture absorption and perspiration setting treatment, and the setting formula is: ICS 30g / L, softener SIH 40g / L (produced by Archroma Chemicals), setting temperature 180℃, and vehicle speed 10m / min.

[0282] After the shaping is completed, a high-elastic single-guide cycling jersey fabric is obtained.

[0283] The samples obtained from Example 1, Comparative Example 1 and Comparative Example 2 of the present invention were tested. The test results are shown in Table 1.

[0284] Table 1 shows the test results of Example 1 and Comparative Examples 1 and 2 of the present invention.

[0285] Table 1

[0286]

[0287]

[0288] Example 2

[0289] This embodiment mainly includes the following steps:

[0290] 1. Weaving

[0291] 50% 50D / 36F iterative polyester, 35% 50D / 36F conventional polyester, and 15% 20D spandex are interwoven, of which the iterative polyester is produced by Qingdao Xinwei Textile Development Co., Ltd. and the spandex is produced by South Korea's Hyosung Group. Soft Fit series, the fabric structure is plain single-sided fabric, the fabric weight is 180g / m 2 .

[0292] 2. Dyeing and finishing

[0293] The fabric obtained in step 1 is dyed and finished, and the dyeing and finishing process is: refining and degreasing water washing - pre-forming - dyeing - reduction cleaning - moisture absorption and perspiration finishing - drying

[0294] (1) Refining, degreasing and water washing

[0295] Select a continuous heated spray loose pre-shrinkage washing machine with a speed of 20m / min, refining formula: high-efficiency refining emulsifier 0-15 25g / l, 0-15 is produced by Guangdong Aobo Shun Chemical Co., Ltd., soda ash 2g / l, and the pH value of the cloth surface is 6.6.

[0296] (2) Pre-form

[0297] Pre-forming process: water through the roller, setting machine temperature 185℃, speed 10m / min, overfeed 12%,

[0298] The liquid carrying rate is controlled at 90%.

[0299] (3) Dyeing

[0300] Immerse the pre-shaped fabric in a 40℃ dye bath with a dye bath ratio of 1:15, keep the temperature constant for 15 minutes, then increase the temperature to 50℃ at a rate of 1.5℃ and keep the temperature constant for 10 minutes, and finally increase the temperature to 105℃ at a rate of 1℃ / min and keep the temperature constant for 30 minutes.

[0301] The dye bath formula is:

[0302] huntsman disperse dyes TERASIL flaming red WW-GS: 1.5owf

[0303] Dispersant: 1g / L, the dispersant is RUCOGAL ERX from Rudolf Chemical

[0304] Acetic acid: 0.5g / L, pH value of dye solution is controlled at 6.5

[0305] (4) Reduction cleaning

[0306] Drain the dyeing solution and continue to perform reduction cleaning, the reduction cleaning bath ratio is 1:15, heat to 80°C, keep warm for 20 minutes and then drain. The reduction cleaning solution includes: 0.5g / l soda ash and 2g / L reduction cleaning agent RUCORIT RGH (produced by Rudolf Chemical).

[0307] (5) Moisture wicking finishing

[0308] The fabric after reduction cleaning is subjected to moisture absorption and perspiration finishing in a tub, the absorption and perspiration finishing bath ratio is 1:15, the finishing bath temperature is room temperature, the treatment time is 20 minutes, and the finishing liquid includes: FERAN ICS 2.5 g / l (produced by Rudolf Chemicals).

[0309] (6) Drying

[0310] The drying temperature is 180°C and the drying speed is 10m / min.

[0311] 3. Single guide printing

[0312] The fabric after suction and discharge is subjected to single-guide printing. The printing pattern is as follows. The drying speed is 10m / min. The formula for single-guide printing: C6 water repellent dosage 110g / L ( -GUARD AFC6), water repellent synergist 5g / L (Rudolf RUCO-GUARD XCR), thickener dosage 8g / L

[0313] (Rudolf TH5000), the viscosity of the printing paste is 1200 centipoise.

[0314] 4. Suction and discharge shaping

[0315] The fabric after single-guide printing is subjected to moisture absorption and perspiration setting treatment, and the setting formula is: ICS 40g / L, softener SIH 50g / L (produced by Angko Chemicals), setting temperature 180°C, speed 10m / min. After setting, a high-elastic single-guide cycling jersey fabric was obtained.

[0316] Functionality tests were performed on the samples obtained in Example 2 of the present invention. The test results are shown in Table 2.

[0317] Table 2 shows the test results of the high-elastic single-guide cycling clothing fabric prepared in Example 2 of the present invention.

[0318] Table 2

[0319]

[0320] Example 3

[0321] This embodiment mainly includes the following steps:

[0322] 1Weaving

[0323] 48% 50D / 36F iterative polyester, 40% 50D / 36F conventional polyester, and 12% 20D spandex are interwoven, of which the iterative polyester is produced by Qingdao Xinwei Textile Development Co., Ltd. and the spandex is produced by South Korea's Hyosung Group. Soft Fit series, the fabric structure is plain single-sided fabric, the fabric weight is 175g / m 2 .

[0324] 2. Dyeing and finishing

[0325] The fabric obtained in step 1 is dyed and finished, and the dyeing and finishing process is: refining and degreasing water washing - pre-forming - dyeing - reduction cleaning - moisture absorption and perspiration finishing - drying

[0326] (1) Refining, degreasing and water washing

[0327] Select a continuous heated spray loose pre-shrinkage washing machine with a speed of 20m / min, refining formula: high-efficiency refining emulsifier 0-15 25g / l, 0-15 is produced by Guangdong Aobo Shun Chemical Co., Ltd., soda ash 2g / l, and the pH value of the cloth surface is 6.6.

[0328] (2) Pre-form

[0329] Pre-forming process: water through the roller, setting machine temperature 185℃, speed 10m / min, overfeed 12%,

[0330] The liquid carrying rate is controlled at 90%.

[0331] (4) Dyeing

[0332] Immerse the pre-shaped fabric in a 40℃ dye bath with a dye bath ratio of 1:15, keep the temperature constant for 15 minutes, then increase the temperature to 50℃ at a rate of 1.5℃ and keep the temperature constant for 10 minutes, and finally increase the temperature to 105℃ at a rate of 1℃ / min and keep the temperature constant for 30 minutes.

[0333] The dye bath formula is:

[0334] huntsman disperse dyes TERASIL flaming red WW-GS: 1.5owf

[0335] Dispersant: 1g / L, the dispersant is RUCOGAL ERX from Rudolf Chemical

[0336] Acetic acid: 0.5g / L, pH value of dye solution is controlled at 6.5

[0337] (4) Reduction cleaning

[0338] Drain the dyeing solution and continue to perform reduction cleaning, the reduction cleaning bath ratio is 1:15, heat to 80°C, keep warm for 20 minutes and then drain. The reduction cleaning solution includes: 0.5g / l soda ash and 2g / L reduction cleaning agent RUCORIT RGH (produced by Rudolf Chemical).

[0339] (5) Moisture wicking finishing

[0340] The fabric after reduction cleaning is subjected to moisture absorption and perspiration finishing in a tub, the absorption and perspiration finishing bath ratio is 1:15, the finishing bath temperature is room temperature, the treatment time is 20 minutes, and the finishing liquid includes: FERAN ICS 2.5 g / l (produced by Rudolf Chemicals).

[0341] (7) Drying

[0342] The drying temperature is 180°C and the drying speed is 10m / min.

[0343] 5. Single guide printing

[0344] The fabric after suction and discharge is subjected to single-guide printing. The printing pattern is as follows, and the drying speed is 10m / min. The formula for single-guide printing: C6 water repellent dosage 100g / L ( GUARD AFC6), water repellent synergist 5g / L (Rudolf RUCO-GUARD XCR), thickener dosage 8g / L (Rudolf TH5000), printing paste viscosity is 1200 centipoise.

[0345] 6. Suction and discharge shaping

[0346] The fabric after single-guide printing is subjected to moisture absorption and perspiration setting treatment, and the setting formula is: ICS 40g / L, softener SIH 50g / L (produced by Angko Chemicals), setting temperature 180°C, speed 10m / min. After setting, a high-elastic single-guide cycling jersey fabric was obtained.

[0347] Functional tests were performed on the samples obtained in Example 3 of the present invention. The test results are shown in Table 3.

[0348] Table 3 shows the test results of the high-elastic single-guide cycling clothing fabric prepared in Example 3 of the present invention.

[0349] Table 3

[0350]

[0351] The above is a detailed introduction to a kind of children's high elastic one-way moisture-conducting cycling clothing fabric and its preparation method provided by the present invention. The principle and implementation method of the present invention are explained in this article using specific examples. The description of the above embodiments is only used to help understand the method and its core idea of ​​the present invention, including the best mode, and also enables any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements that are not different from the text of the claims, or if they include equivalent structural elements that are not substantially different from the text of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. A one-way moisture-conducting cycling jersey fabric, It is characterized in that The main body of the fabric includes two types of polyester yarns and spandex yarns interwoven; The polyester accounts for 80% to 90% of the fabric by mass; The spandex accounts for 10% to 20% of the fabric mass; The two types of polyester include highly hygroscopic iterative polyester and polyester; The fabric structure is a polyester-covered polyester-spandex single-sided plain weave structure; In the polyester-covered polyester-spandex single-sided plain weave structure, the face yarn is highly hygroscopic iterative polyester, and the bottom yarn is polyester and spandex; The glass transition temperature of the highly hygroscopic iterative polyester is 62-67°C; In the highly hygroscopic iterative polyester, the mass content of titanium dioxide is 2% to 4%; The fabric weight is 160-180 g / m 2 ; The number of interwoven weaving needles is 36 needles, 40 needles or 44 needles; The one-way moisture transfer index of the one-way moisture conduction cycling jersey fabric is 400% to 1200%; The fabric body is compounded with an absorption and discharge finishing agent; The suction and discharge finishing agent includes a composite emulsion of a non-ionic hydrophilic polymer and polysiloxane; The fabric is a fabric with a hydrophilic front side and a discontinuous water-repellent area on the back side; On the reverse side of the fabric, the area ratio of the water-repellent region is 50% to 80%, and the area ratio of the hydrophilic region is 20% to 50%; The water-repellent region includes a printed region; The fabric is obtained by subjecting the fabric raw material to two moisture absorption and perspiration treatments; The two moisture absorption and perspiration treatments include moisture absorption and perspiration finishing and moisture absorption and perspiration shaping; A unidirectional moisture conduction printing step is included between the two moisture absorption and perspiration treatment steps.

2. The cycling clothing fabric according to claim 1, It is characterized in that The mass ratio of the highly hygroscopic iterative polyester to the two polyesters is 50% to 60%; The moisture regain of the highly hygroscopic iterative polyester is 1.6% to 2.0%; The moisture regain of the polyester is 0.3% to 0.5%; The specification of the polyester yarn is 50D / 36F or 70D / 48F; The spandex includes fine denier spandex; The density of the spandex yarn is 20D.

3. The cycling clothing fabric according to claim 1, It is characterized in that The one-way moisture-conducting cycling jersey fabric is a highly elastic one-way moisture-conducting cycling jersey fabric for children.

4. A method for preparing the one-way moisture-conducting cycling jersey fabric according to any one of claims 1 to 3, It is characterized in that The following steps are involved: 1) The high moisture absorption iterative polyester yarn, polyester yarn and spandex yarn are weaved to obtain the main body of the fabric; 2) dyeing and finishing the fabric body obtained in the above steps to obtain a dyed and finished fabric body; The dyeing and finishing process includes a moisture absorption and perspiration finishing step; 3) The dyed and finished fabric body obtained in the above steps is subjected to one-way moisture-conducting printing and moisture-absorbing and perspiration-releasing shaping treatment to obtain a one-way moisture-conducting cycling jersey fabric.

5. The preparation method according to claim 4, It is characterized in that The weaving method includes circular weft knitting; The specific process flow of dyeing and finishing includes one or more steps of refining, degreasing, washing, pre-forming, dyeing, reduction cleaning, moisture absorption and perspiration finishing and drying.

6. The preparation method according to claim 5, It is characterized in that The water washing speed of the refining and degreasing water washing step is 15-30 m / min; The pH value of the cloth surface in the refining, degreasing and washing step is ≤7.5; The pre-forming temperature is 180-190°C; The preforming speed is 18-30 m / min.

7. The preparation method according to claim 6, It is characterized in that The dyeing bath ratio is 1: (10-20); The dye bath formula for dyeing comprises: Disperse dyes: 0.1~5owf; Dispersant: 0.5~2g / L; Acetic acid: 0.5~2g / L; water; The pH value of the dyeing solution is 5-7; The temperature of the reduction cleaning is 60-90°C; The reduction cleaning time is 10 to 30 minutes.

8. The preparation method according to claim 6, It is characterized in that The moisture absorption and perspiration finishing time is 5 to 10 minutes; The bath ratio of the moisture absorption and perspiration finishing is 1: (10-20); The moisture-wicking finishing agent for moisture-wicking finishing comprises a composite emulsion of a nonionic hydrophilic polymer and polysiloxane; The concentration of the moisture wicking finishing agent for the moisture wicking finishing is 1-3 g / L; The drying temperature is 150-180°C; The drying speed is 10-20 m / min.

9. The preparation method according to claim 6, It is characterized in that The unidirectional wet-conducting printing process includes a rotary screen printing process; The viscosity of the printing paste for unidirectional wet-conducting printing is 800-1500 centipoise; The printing paste formula for the one-way wet-conducting printing comprises: C6 water repellent 80~120g / L; Water repellent enhancer 5~20g / L; Thickener 5~20g / L; water; The C6 water repellent comprises C6 fluorocarbon resin; The water repellent synergist includes a cationic block copolyisocyanate; The thickener includes sodium alginate and / or polyacrylic acid resin.

10. The preparation method according to claim 6, It is characterized in that The bath ratio of moisture absorption and perspiration setting is 1: (10-20); The moisture absorption and perspiration setting agent formula comprises: Moisture wicking finishing agent 20~40g / L; Softener 30~60g / L; water; The setting temperature of the moisture absorption and perspiration setting is 150-180°C; The speed of moisture absorption and perspiration shaping is 10-20 m / min.

Citation Information

Patent Citations

  • Weaving and dyeing method for unidirectional moisture-conducting elastic fabric

    CN108301234A

  • Unidirectional moisture-guiding elastic fabric and manufacturing method thereof

    CN110079928A

  • Anti-permeability and moisture absorption different-function knitted fabric and production process thereof

    CN103233317A

  • Singe-face water prevention dirt resisting and single-face 3D moisture absorption quick drying technology for cotton fabric

    CN104074061A

  • Preparation method of knitted fabric with one-way moisture conduction and cooling functions

    CN106702767A