A high-nickel multi-element positive electrode material, preparation method thereof and application thereof
Through the high-priced lithium metal acid compound coating method, the problem of poor coating uniformity of high-nickel positive electrode materials in large-scale production is solved, the slurry stability and thermal safety performance of the material are improved, and better electrochemical performance is achieved.
Patent Information
- Application Number
- CN202210262675.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-17
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-03-17
AI Technical Summary
In the mass production of high-nickel multivariate positive electrode materials, there are problems such as poor surface coating uniformity, unstable battery paste viscosity, high internal circulation resistance and poor thermal stability. Existing methods such as physical mixing method and heterogeneous precipitation reaction are difficult to be effective. solve.
The high-valent lithium metal acid compound coating method is used to mix the initial positive electrode material with water and wash it in water, and then filter the alkali solution containing high-valent metal ions for solid-liquid separation, drying and heat treatment to form a uniform high-valent lithium metal acid compound packaging. Covering to improve the structural stability and electrochemical properties of the cathode material.
The slurry stability, cycle stability and thermal safety performance of high-nickel positive electrode materials are improved, the coating uniformity and electrochemical performance are improved, and the unevenness problem of traditional wet coating is avoided.
Smart Images

Figure BDA0003551171690000091 
Figure BDA0003551171690000101 
Figure BDA0003551171690000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a high-nickel multi-element positive electrode material, a preparation method thereof and applications thereof. Background Art
[0002] With the increasing requirements for the range and cost of new energy vehicles, high-nickel multi-element positive electrode materials have become an important research hotspot due to their high energy density and low cost.
[0003] There are many unresolved problems similar to those of LiNiO2 in high-nickel multi-element cathode materials, such as cation mixing, poor thermal safety, high residual alkali, strain and microcracks in secondary particles. Doping and coating strategies have been widely used to modify high-nickel multi-element cathode materials. Bulk doping helps stabilize the crystal structure and improve reaction kinetics, while surface coating helps inhibit side reactions and accelerate the transport of lithium ions. The MO bonds (M represents W, V, Nb, Ta) formed by high-valent cations usually have higher bond strength than TM-O bonds. The stronger binding of MO helps inhibit oxygen release, thereby improving structural stability.
[0004] At present, the laboratory has developed many coating methods, including physical mixing, liquid phase, liquid phase precipitation, sol-gel method, chemical vapor deposition (CVD), hydrothermal method and atomic layer deposition (ALD), etc. However, the industrialization of positive electrodes is limited by mass production requirements and cost control. At present, the surface coating methods of high-nickel multi-element positive electrode manufacturers at home and abroad are still concentrated on the physical mixing method of coating agent and parent material dry method. Although this method is simple and low in cost, the actual coverage rate of the positive electrode surface after modification is low. The exposure of the unmodified active surface often leads to problems such as unstable battery slurry viscosity, severe gas production, high cycle internal resistance and poor thermal stability.
[0005] The Chinese patent with publication number CN111490234A adds the positive electrode material to a water washing solution containing a coating agent, which can effectively remove residual alkali and obtain a fully covered coating layer. However, such methods usually achieve surface coating through a heterogeneous precipitation reaction, and the high-nickel material has a high pH value and a long feeding time for mass production, so the coating uniformity is poor in actual mass production.
[0006] Another example is the Chinese patent with publication number CN112174221A, which improves the coating uniformity of the coating by slowly releasing the metal ions of the coating agent by adding a chelating agent. However, this method requires a long coating time, which easily causes the material to be in contact with the solvent for a long time, resulting in lithium dissolution in the material structure, thereby causing a loss of battery capacity and an increase in internal resistance.
[0007] Therefore, it is of great significance to provide a high-nickel cathode material with a stable surface structure and a preparation method thereof to improve its comprehensive performance. Summary of the invention
[0008] The technical problem solved by the present invention is to provide a high-nickel multi-component positive electrode material and a preparation method thereof. The high-nickel multi-component positive electrode material provided by the present application has high slurry stability, cycle stability and thermal safety performance.
[0009] In view of this, the present application provides a high-nickel multi-element positive electrode material, which is composed of particles having the general formula (I) and a high-valent metal acid lithium compound coated on the surface of the particles.
[0010] Li 1+k Me 1-k O2 (Ⅰ);
[0011] Among them, -0.03≤k≤0.10, Me=Ni c Me' d Co e R f ;
[0012] 0.80≤c≤1, 0.00≤d≤0.20, 0.05≤e≤0.20, 0≤f≤0.05, Me' is selected from one or both of Mn and Al, and R is selected from one or more of Mg, Ti, B, Ba, Sr, Zr, Y and Na;
[0013] The high-valent metal ion in the high-valent metal acid lithium compound is a cation with a valence of not less than +5 and no electrons in the outermost d orbit.
[0014] Preferably, the high-valent metal ion is selected from Nb 5+ 、Mo 6+ 、 5+ and W 6+ One or more of.
[0015] Preferably, the average particle size of the high nickel multi-element positive electrode material is 5 to 20 μm, and the specific surface area is 0.2 to 1.5 m 2 / g.
[0016] Preferably, in the high-nickel multi-element positive electrode material, the content of the high-valent metal ions is 0.05-1 wt %.
[0017] The present application also provides a method for preparing the high-nickel multi-element positive electrode material, comprising the following steps:
[0018] The initial positive electrode material having the general formula (I) is mixed with water, washed with water, and then separated into solid and liquid to obtain a primary filter cake;
[0019] The primary filter cake is filtered through an alkaline solution containing high-valent metal ions, and solid-liquid separation is performed again to obtain a secondary filter cake;
[0020] The secondary filter cake is dried and then heat-treated to obtain a high-nickel multi-element positive electrode material;
[0021] Li 1+k Me 1-k O2 (Ⅰ);
[0022] Among them, -0.03≤k≤0.10, Me=Ni c Me' d Co e R f ;
[0023] 0.80≤c≤1, 0.00≤d≤0.20, 0.05≤e≤0.20, 0≤f≤0.05, Me' is selected from one or both of Mn and Al, and R is selected from one or more of Mg, Ti, B, Ba, Sr, Zr, Y and Na;
[0024] The high-valent metal ion is a cation with a valence of not less than +5 and no electrons in the outermost d orbital.
[0025] Preferably, the moisture content of the primary filter cake is 0.05-30 wt %, and the moisture content of the secondary filter cake is 0.05-20 wt %.
[0026] Preferably, in the alkaline solution containing high-valent metal ions, the concentration of the high-valent metal ions is 0.05 to 3 mol / L, and the concentration of the alkaline solution is 1 to 6 times the concentration of the high-valent metal ions.
[0027] Preferably, the alkali in the alkaline solution is selected from ammonia water, lithium carbonate or lithium hydroxide.
[0028] Preferably, the drying temperature is 50-300° C., the heat treatment atmosphere is an atmosphere in which the concentration of carbon dioxide gas does not exceed 1 wt %, the heat treatment temperature is 150-800° C., and the time is 5-36 h.
[0029] The present application also provides a lithium-ion battery, comprising a positive electrode material and a negative electrode material, characterized in that the positive electrode material is the high-nickel multi-element positive electrode material or the high-nickel multi-element positive electrode material prepared by the preparation method.
[0030] The present application provides a high nickel multi-element positive electrode material, which is composed of Li 1+k Me 1-k O2 particles and high-valent metal acid lithium compounds coated on the surface of the particles; a uniform high-valent metal acid lithium compound is formed on the surface of the primary particles and secondary particles of the positive electrode material of the present application, wherein the high-valent cation-O bond can inhibit oxygen release and improve the thermal stability of the material.
[0031] At the same time, the present application also provides a method for preparing a high-nickel multi-element positive electrode material, which uses a coating metal salt solution dissolved in alkali to uniformly cover the wettable interface of the positive electrode material. Compared with conventional physical dry-mix coating, this wet coating has better uniformity and can coat the internal grain boundaries of secondary particles, thereby improving the slurry stability of the positive electrode material. Furthermore, compared with traditional wet coating, the method provided by the present application can independently control the water washing parameters, avoid the problem of over-washing or uneven coating of the positive electrode material, and can balance the electrochemical performance of various aspects such as material capacity, cycle and safety. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 These are SEM photos of the surface-modified high-nickel multi-component materials prepared in Example 1 of the present invention and Comparative Examples 1 and 2. DETAILED DESCRIPTION
[0033] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0034] In view of a series of problems caused by the unstable surface structure of the current high-nickel positive electrode material, the present application provides a high-nickel multi-element positive electrode material, in which the primary particles and secondary particles of the positive electrode material are coated with high-valent cationic compounds, and the high-nickel multi-element positive electrode material has high slurry stability, cycle stability and thermal safety. Specifically, the embodiment of the present invention discloses a high-nickel multi-element positive electrode material, which is composed of particles having the general formula (I) and a high-valent metal acid lithium compound coated on the surface of the particles,
[0035] Li 1+k Me 1-k O2 (Ⅰ);
[0036] Among them, -0.03≤k≤0.10, Me=Ni c Me' d Co e R f ;
[0037] 0.80≤c≤1, 0.00≤d≤0.20, 0.05≤e≤0.20, 0≤f≤0.05, Me' is selected from one or both of Mn and Al, and R is selected from one or more of Mg, Ti, B, Ba, Sr, Zr, Y and Na;
[0038] The high-valent metal ion in the high-valent metal acid lithium compound is a cation with a valence of not less than +5 and no electrons in the outermost d orbit.
[0039] In the present application, the high-valent metal ion is selected from Nb 5+、Mo 6+ 、 5+ and W 6+ More specifically, the high-valent metal ion is selected from Nb 5+ 、Mo 6+ 、 5+ or W 6+ The high-valent metal ions will affect the gas production and cycle performance of the high-nickel multi-element cathode material; the high-valent metal ion MO bond (M represents Nb, Mo, Ta or W) usually has a higher bond strength than the transition metal Me-O bond in the cathode material, and MO contributes to the overall Me-O covalency and inhibits oxygen release, thereby improving the structural stability of the cathode material.
[0040] For the high nickel multinary positive electrode material described in this application, the average particle size of the high nickel multinary positive electrode material is 5 to 20 μm, and the specific surface area is 0.2 to 1.5 m 2 / g; More specifically, the average particle size of the high-nickel multi-element positive electrode material is 8 to 12 μm, and the specific surface area is 0.25 to 1.3 m 2 / g.
[0041] In the high-nickel multi-element positive electrode material, the content of the high-valent metal ions is 0.05-1 wt %; more specifically, the content of the high-valent metal ions is 0.20-0.80 wt %.
[0042] The present application also provides a method for preparing the high-nickel multi-element positive electrode material, comprising the following steps:
[0043] The initial positive electrode material having the general formula (I) is mixed with water, washed with water, and then separated into solid and liquid to obtain a primary filter cake;
[0044] The primary filter cake is filtered through an alkaline solution containing high-valent metal ions, and solid-liquid separation is performed again to obtain a secondary filter cake;
[0045] The secondary filter cake is dried and then heat-treated to obtain a high-nickel multi-element positive electrode material;
[0046] Li 1+k Me 1-k O2 (Ⅰ);
[0047] Among them, -0.03≤k≤0.10, Me=Ni c Me' d Co e R f ;
[0048] 0.80≤c≤1, 0.00≤d≤0.20, 0.05≤e≤0.20, 0≤f≤0.05, Me' is selected from one or both of Mn and Al, and R is selected from one or more of Mg, Ti, B, Ba, Sr, Zr, Y and Na;
[0049] The high-valent metal ion is a cation with a valence of not less than +5 and no electrons in the outermost d orbital.
[0050] In the process of preparing high-nickel multi-element positive electrode materials, the present application first mixes the initial positive electrode material with water, washes with water, and separates the solid and liquid to obtain a primary filter cake; in this process, the general formula of the initial positive electrode material is shown in formula (I), and its preparation method is prepared according to a method well known to those skilled in the art, and the present application has no special restrictions on this. The water-to-material ratio of the initial positive electrode material to water is 0.5:1 to 5:1, and more specifically, the water-to-material ratio (volume) is 0.8:1 to 2:1. The washing time is 30s to 30min, and more specifically, the washing time is 1min to 15min. The solid-liquid separation equipment is a device well known to those skilled in the art, and can be carried out in a suction filtration equipment, a centrifugal equipment, or a filter press equipment. The water content of the primary filter cake is 0.05 to 30wt%, and more specifically, the water content of the primary filter cake is 2 to 15wt%. The moisture content of the primary filter cake will affect the coating amount of the coating. When the moisture content of the secondary filter cake is constant, if the moisture content of the primary filter cake is too high, the concentration of the coating liquid will decrease and the coating amount will decrease. Otherwise, the coating amount will increase.
[0051] Then, the present application filters the primary filter cake through an alkaline solution containing high-valent metal ions, and separates the solid and liquid again to obtain a secondary filter cake; in this process, high-valent metal acid radical ions (such as MoO3+2OH) are formed in the alkaline solution containing high-valent alkali metal ions. - →MoO4 2- +H2O, 2OH - +WO3→WO4 2-+H2O); the concentration of the high-valent metal ion is 0.05-3 mol / L, more specifically, the concentration of the high-valent metal ion is 0.1-1 mol / L, which will affect the thickness of the coating layer and thus affect the performance of the multi-element positive electrode material. If the concentration is too high, the coating layer will be too thick, which will affect the lithium ion deintercalation during the charge and discharge process and lead to a decrease in capacity. If the concentration is too low, the coating layer will be too thin, resulting in a weak protective effect, and the positive electrode residual alkali consumption is small, which is not conducive to the viscosity stability of the positive electrode pulping; the concentration of the alkaline solution is 1-6 times the concentration of the high-valent metal ion, more specifically, the concentration of the alkaline solution is 1-4 times the concentration of the high-valent metal ion; if the alkali concentration is too high, the residual lithium content of the positive electrode will increase, which is not conducive to the viscosity stability of the positive electrode pulping. If the alkali concentration is too low, it will be not conducive to the dissolution of high-valent metal oxides. In addition, the reduction in pH will also accelerate the lithium removal of the positive electrode in the liquid phase and destroy its layered structure. The alkali of the alkaline solution described in the present application is preferably an alkali that does not bring cationic impurities, and more specifically can be selected from ammonia water, lithium carbonate or lithium hydroxide. The moisture content of the secondary filter cake is 0.05-20wt%, more specifically, the moisture content of the secondary filter cake is 1-12wt%. The moisture content of the secondary filter cake will directly affect the thickness of the coating layer. If the moisture content is too high, the thickness of the coating layer will increase, affecting the lithium ion deintercalation during the charge and discharge process, resulting in a decrease in capacity, and is not conducive to improving the drying efficiency; if the concentration is too low, the coating layer is too thin, resulting in a weak protective effect, which deteriorates the gas production and cycle performance of the positive electrode material.
[0052] The present application finally dries the secondary filter cake and then heat treats it to obtain a high-nickel multi-element positive electrode material. In this process, the initial coating of the positive electrode material is achieved, that is, the metal acid radical ions in the coating solution remaining in the secondary filter cake and the residual lithium on the surface of the multi-element positive electrode material or the lithium ions in the coating alkali solution are dehydrated and crystallized to form a high-valent metal acid lithium compound, which is formed not only on the surface of the secondary particles, but also on the surface of the primary particles. The drying equipment is a conventional drying equipment in the art, but it can be fully mixed and dried without destroying the structure of the positive electrode material. It is preferably a plow dryer, a double cone dryer or a vibration dryer; the drying temperature is 50 to 300°C, more specifically, the drying temperature is 100 to 250°C. The heat treatment is carried out in an atmosphere with a carbon dioxide gas concentration of no more than 1wt%, preferably in an oxygen or vacuum environment; the heat treatment temperature is 150 to 800°C, the time is 5 to 36h, more specifically, the heat treatment temperature is 200 to 600°C, and the time is 10h to 24h.
[0053] The present application also provides a lithium-ion battery, which includes a positive electrode material and a negative electrode material, wherein the positive electrode material is the high-nickel multi-element positive electrode material described in the above scheme.
[0054] In order to further understand the present invention, the high-nickel multi-element positive electrode material provided by the present invention, its preparation method and application are described in detail below in conjunction with the embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0055] Example 1
[0056] The primary sintered cathode powder is obtained by mixing nickel composite hydroxide and lithium hydroxide and sintering them in an oxygen atmosphere. 1.025 Ni 0.90 Co 0.06 Al 0.04 O2 indicates that the average particle size of the high nickel cathode powder is 10.6 μm and the specific surface area is 0.28 m 2 / g; 500g of the primary sintered positive electrode material and deionized water were washed with water in a weight ratio of 1:1 for 10min, and the material liquid was filtered and dehydrated for 30min through a Buchner suction filtration bottle to obtain a primary filter cake with a water content of 10wt%; 8.69g of tungsten oxide (WO3) was added to the aqueous solution formed by dissolving 3.15g of lithium hydroxide (LiOH·H2O) in 150mL of pure water to form a tungsten-containing alkaline solution with a tungsten concentration of 0.25mol / L; the alkali solution was evenly poured on the primary filter cake, and then filtered to obtain a secondary filter cake with a water content of 8wt%; the secondary filter cake was then placed in a double-cone vacuum dryer and dried at 120°C for 6h to obtain a washed and dried material; the dried material was heated to 400°C at 2°C / min in an oxygen atmosphere for 10h, and the heat-treated material was sieved through a 325-mesh sieve to obtain a multi-element high-nickel material uniformly coated with W. The composition of the obtained positive electrode active material was analyzed by ICP method, and it was confirmed that the content of W was 0.20 wt %.
[0057] Example 2
[0058] A tungsten-containing alkaline solution with a tungsten concentration of 0.50 mol / L was prepared by adding 17.38 g of tungsten oxide (WO3) to an aqueous solution prepared by dissolving 6.30 g of lithium hydroxide (LiOH·H2O) in 150 mL of pure water. A multi-element high-nickel material was obtained in the same manner as in Example 1 except for the above.
[0059] Example 3
[0060] A multi-element high-nickel material was obtained in the same manner as in Example 1 except that the heat treatment temperature was set to 550°C.
[0061] Example 4
[0062] The multi-element high-nickel material was obtained in the same manner as in Example 1 except that the moisture content of the secondary filter cake was controlled at 16 wt %.
[0063] Example 5
[0064] A niobium-containing alkaline solution with a niobium concentration of 0.25 mol / L was prepared by adding 4.98 g of niobium pentoxide (Nb2O5) to an aqueous solution formed by dissolving 4.72 g of lithium hydroxide (LiOH·H2O) in 150 mL of pure water. A multi-element high-nickel material was obtained in the same manner as in Example 1 except for the above.
[0065] Example 6
[0066] A vanadium-containing alkaline solution with a vanadium concentration of 0.25 mol / L was prepared by adding 3.41 g of vanadium pentoxide (V2O5) to an aqueous solution formed by dissolving 4.72 g of lithium hydroxide (LiOH·H2O) in 150 mL of pure water.
[0067] Example 7
[0068] A tantalum-containing alkaline solution with a tantalum concentration of 0.25 mol / L was prepared by adding 8.29 g of tantalum pentoxide (Ta2O5) to an aqueous solution formed by dissolving 1.57 g of lithium hydroxide (LiOH·H2O) in 150 mL of pure water. A multi-element high-nickel material was obtained in the same manner as in Example 1 except for the above.
[0069] Comparative Example 1
[0070] 150 mL of pure water was evenly poured on the primary filter cake, and then suction filtered to obtain a secondary filter cake with a water content of 8 wt %. Other than this, the multi-element high-nickel material was obtained in the same manner as in Example 1.
[0071] Comparative Example 2
[0072] 500g of Li 1.025 Ni 0.90 Co 0.06 Al 0.04 O2, average particle size is 10.6 μm, specific surface area is 0.28 m 2 / g of primary sintered positive electrode material and deionized water are washed with water in a weight ratio of 1:1 for 10 minutes, and the material liquid is filtered and dehydrated for 30 minutes through a Buchner suction filter funnel to obtain a primary filter cake with a moisture content of 10wt%; 150mL of pure water is evenly poured on the primary filter cake, and then filtered to obtain a secondary filter cake with a moisture content of 8wt%; the secondary filter cake is then placed in a double-cone vacuum dryer and dried at 120°C for 6h to obtain a washed and dried material; 1.01g of nano tungsten oxide (WO3) and 0.19g of lithium hydroxide (LiOH·H2O) are added to 400g of the washed and dried material, and the mixture is mechanically mixed evenly with a high-speed mixer; the nano-coated dried material is heated to 400°C at 2°C / min in an oxygen atmosphere, and the insulation time is 10h, and the heat-treated material is sieved through a 325-mesh sieve to obtain a multi-element high-nickel material uniformly coated with W. The composition of the obtained positive electrode active material was analyzed by ICP method, and it was confirmed that the content of W was 0.20 wt %.
[0073] Comparative Example 3
[0074] 8.69 g of tungsten oxide (WO3) was added to an aqueous solution formed by dissolving 12.60 g of lithium hydroxide (LiOH·H2O) in 150 mL of pure water to form a tungsten-containing alkaline solution with a tungsten concentration of 0.25 mol / L and an alkali concentration of 2.00 mol / L. Except for this, the multi-element high-nickel material was obtained in the same manner as in Example 1.
[0075] Comparative Example 4
[0076] By shortening the first stage of filtration time, a primary filter cake with a water content of 35 wt % was obtained. Except for this, the multi-element high-nickel material was obtained in the same manner as in Example 1.
[0077] Comparative Example 5
[0078] By shortening the second stage of filtration time, a secondary filter cake with a water content of 25 wt % was obtained. In addition, the multi-element high-nickel material was obtained in the same manner as in Example 1.
[0079] The above-mentioned examples and comparative examples were subjected to physicochemical property tests and electrochemical tests under the same test conditions. The test results are shown in Table 1 below.
[0080] Table 1 Comparison of physical, chemical and electrical properties of the embodiments and comparative examples
[0081]
[0082]
[0083]
[0084] Figure 1The SEM photos of the surface-modified high-nickel multi-component materials prepared in Example 1 of the present invention and Comparative Examples 1 and 2 are shown in the figure. It can be seen from the figure that the method in Example 1 of the present invention can form a uniform film-like coating on the surface of the primary particles and secondary particles of the high-nickel multi-component material, which is significantly improved compared with the traditional dry coating uniformity and coating area of Comparative Example 2 in the figure. Figure 1 The results show that the surface of high-nickel multi-element materials fully covered with fast ion conductive membranes has greatly improved lithium ion transmission and enhanced thermal stability of the materials.
[0085] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0086] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A high-nickel multi-element positive electrode material, comprising particles of general formula (I) and a high-valent metal acid lithium compound coated on the surface of the particles, Li 1+k Me 1-k O2(Ⅰ); in, -0.03≤k≤0.10,Me=Ni c Along with' d Co e R f ; 0.80≤c≤1, 0.00≤d≤0.20, 0.05≤e≤0.20, 0≤f≤0.05, Me' is selected from one or both of Mn and Al, and R is selected from one or more of Mg, Ti, B, Ba, Sr, Zr, Y and Na; The high-valent metal ion in the high-valent metal acid lithium compound is a cation with a valence of not less than +5 and no electrons in the outermost d orbital; The high-valent metal ion is selected from Nb 5+ 、Mo 6+ 、 5+ and W 6+ One or more of; The method for preparing the high-nickel multi-element positive electrode material comprises the following steps: The initial positive electrode material having the general formula (I) is mixed with water, washed with water, and then separated into solid and liquid to obtain a primary filter cake; The primary filter cake is filtered through an alkaline solution containing high-valent metal ions, and solid-liquid separation is performed again to obtain a secondary filter cake; The secondary filter cake is dried and then heat-treated to obtain a high-nickel multi-element positive electrode material; Li 1+k Me 1-k O2(Ⅰ); Among them, -0.03≤k≤0.10, Me=Ni c Me' d Co e R f ; 0.80≤c≤1, 0.00≤d≤0.20, 0.05≤e≤0.20, 0≤f≤0.05, Me' is selected from one or both of Mn and Al, and R is selected from one or more of Mg, Ti, B, Ba, Sr, Zr, Y and Na; The moisture content of the primary filter cake is 2-15wt%, and the moisture content of the secondary filter cake is 1-20wt%; In the alkaline solution containing high-valent metal ions, the concentration of high-valent metal ions is 0.1 to 1 mol / L; A uniform high-valent metal acid lithium compound is formed on the surfaces of the primary particles and secondary particles of the positive electrode material.
2. The high-nickel multi-element positive electrode material according to claim 1, characterized in that: The high-nickel multi-element positive electrode material has an average particle size of 5 to 20 μm and a specific surface area of 0.2 to 1.5 m 2 / g.
3. The high-nickel multi-element positive electrode material according to claim 1, characterized in that: In the high-nickel multi-element positive electrode material, the content of the high-valent metal ions is 0.05-1 wt %.
4. The method for preparing the high-nickel multi-element positive electrode material according to claim 1 comprises the following steps: The initial positive electrode material having the general formula (I) is mixed with water, washed with water, and then separated into solid and liquid to obtain a primary filter cake; The primary filter cake is filtered through an alkaline solution containing high-valent metal ions, and solid-liquid separation is performed again to obtain a secondary filter cake; The secondary filter cake is dried and then heat-treated to obtain a high-nickel multi-element positive electrode material; The moisture content of the primary filter cake is 2-15wt%, and the moisture content of the secondary filter cake is 1-20wt%; In the alkaline solution containing high-valent metal ions, the concentration of high-valent metal ions is 0.1-1 mol / L; Li 1+k Me 1-k O2(Ⅰ); Among them, -0.03≤k≤0.10, Me=Ni c Me' d Co e R f ; 0.80≤c≤1, 0.00≤d≤0.20, 0.05≤e≤0.20, 0≤f≤0.05, Me' is selected from one or both of Mn and Al, and R is selected from one or more of Mg, Ti, B, Ba, Sr, Zr, Y and Na; The high-valent metal ion is a cation with a valence of not less than +5 and no electrons in the outermost d orbital.
5. The preparation method according to claim 4, characterized in that: In the alkaline solution containing high-valent metal ions, the concentration of the alkaline solution is 1 to 6 times the concentration of the high-valent metal ions.
6. The preparation method according to claim 4, characterized in that: The alkali in the alkali solution is selected from ammonia water, lithium carbonate or lithium hydroxide.
7. The preparation method according to claim 4, characterized in that: The drying temperature is 50-300° C., the heat treatment atmosphere is an atmosphere in which the concentration of carbon dioxide gas does not exceed 1wt%, the heat treatment temperature is 150-800° C., and the time is 5-36 hours.
8. A lithium ion battery comprising a positive electrode material and a negative electrode material, characterized in that: The positive electrode material is the high-nickel multinary positive electrode material described in any one of claims 1 to 3 or the high-nickel multinary positive electrode material prepared by the preparation method described in any one of claims 4 to 7.