A novel metal chalcogenide solid solution electrode material and its preparation method and application

By using branch-leaf composite structure and high-temperature treatment technology in metal chalcogenide electrode materials, CNS@CoSX@C electrode materials are formed, which solves the problems of slow ion transmission rate and volume expansion of the electrode materials, and achieves high capacity and long Lifespan and high rate performance, suitable for sodium ion batteries.

CN114725353BActive Publication Date: 2024-11-26YANGTZE NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210472554.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-29
Publication Date
2024-11-26
Estimated Expiration
2042-04-29

AI Technical Summary

Technical Problem

The existing metal chalcogenide electrode materials have problems such as slow ion transmission rates and serious volume expansion, which is difficult to meet the demand for large capacity and high rate performance in the electric vehicle market.

Method used

Using a metal chalcogenide solid solution electrode material with a branch-leaf composite structure, the chemical of CNS@CoSX@C is formed by combining carbon network scaffolding and metal chalcogenide solid solution nanosheets, combined with high-temperature carbonization, vulcanization and selenization treatment. Composition to improve ion transport dynamics and cycling stability.

Benefits of technology

It has achieved ultra-high reversible capacity, ultra-long cycle life and good structural stability at ultra-high magnification, significantly improved electrochemical performance, solved the problems of volume expansion and capacity attenuation, and had good application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003623463610000011
    Figure HDA0003623463610000011
  • Figure HDA0003623463610000021
    Figure HDA0003623463610000021
  • Figure HDA0003623463610000022
    Figure HDA0003623463610000022
Patent Text Reader

Abstract

The present invention discloses a novel metal sulfide solid solution electrode material and a preparation method and application thereof. The electrode material has a branch-leaf structure at the microscopic level, and is composed of a carbon network support as a "branch" and a metal sulfide solid solution nanosheet as a "leaf". The electrode material has a chemical composition represented by CNS@CoSX@C, wherein X is a non-metallic element Se or Te. The electrode material of the present invention has a high specific capacity, and still has good retention after 13,000 cycles, showing good and cycle-stable electrochemical performance, and still has good structural stability and cycle life at ultra-high rates. At the same time, the present invention has low raw material cost, simple process, low energy consumption, and easier reaction conditions to achieve, can be mass-produced, and is convenient for commercial application, showing great application prospects in sodium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion battery materials, and in particular relates to a novel metal chalcogenide solid solution electrode material and a preparation method and application thereof. Background Art

[0002] The widespread use of fossil energy has made environmental pollution and energy crisis the two major problems facing the world today. The development of new energy devices based on electrochemistry is of great significance to alleviate environmental pollution and solve the energy crisis. As an energy carrier that drives the rapid progress of human society, using batteries for mobile or fixed energy storage is a topic with broad social value and economic significance. At the same time, its successful development and utilization must depend on the two most critical factors of high performance and economy. Lithium-ion batteries, as the most common and successful secondary batteries, have now become the main energy storage device in the portable electronics market. However, we should be aware that the increasingly scarce lithium resources not only make the cost of battery production gradually increase, but also cannot meet the huge demand for widely available electric vehicles and hybrid vehicles, so that lithium batteries may no longer be the best choice. Therefore, finding alternative rechargeable battery systems has become the focus of energy researchers. Metallic sodium and lithium are in the same main group and have similar physical and chemical properties and working principles. At the same time, compared with metallic lithium, metallic sodium is more abundant in the earth's crust (2.4% vs 0.0017%, Na vs Li), and can be mined and extracted at a lower cost from oceans, natural sodium salt fields, and mirabilite mines; more importantly, sodium has a lower redox potential (-2.71V) and a higher mass / volume capacity than lithium (-3.0V), and due to the low melting point of sodium, battery safety problems caused by sodium dendrites can be effectively avoided. Therefore, the development of metallic sodium batteries with excellent electrochemical performance will be one of the future development trends. Among them, sodium-ion batteries are considered to be one of the most competitive electrochemical energy storage devices in the "post-lithium-ion battery" era due to their advantages such as low cost and high operating voltage. However, the larger radius of sodium metal ions usually leads to slow reaction kinetics, unstable solid electrolyte interphase layers, and collapse of the crystal structure of the host material, resulting in a decrease in electrochemical performance. In this case, it is very necessary to explore suitable negative electrode materials with high capacity and cycle stability.

[0003] In the past few years, several classic anode materials for storing alkali metal ions have been studied, such as carbon materials, traditional intercalation compounds, metal compounds, etc. +Compared with the storage capacity of Na+, conversion materials can provide higher theoretical capacity, thus showing great potential. In particular, transition metal chalcogenide (TMC) shows higher theoretical capacity and faster ion diffusion rate due to its multi-electron redox reaction and easy breakage of MS or M-Se bond (M represents metal). However, most of them still suffer from the defects of inherent low conductivity and severe volume expansion during long-term cycling, which will lead to poor rate performance and rapid capacity decay. In order to solve the above problems, guest elements are usually introduced into the monometallic TMC matrix, and the matrix is ​​subjected to atomic-level bulk tailoring to form a TMC-based solid solution, which is an effective way to reduce Na+. + The energy barrier of diffusion is an important way to promote ion transport kinetics and improve cycle stability. Compared with TMC with heterogeneous properties, the solid solution structure inherits the advantages of the parent TMC and the compensatory effect introduced by the guest element, forming a multi-element material with single-phase characteristics, and the internal interaction is stronger than that within the heterogeneous body, so it shows more stable structural characteristics. In addition, the composition of TMC solid solution can be adjusted more easily and accurately than that of heterogeneous TMC (in some cases, the composition of the solid solution can be adjusted continuously), and their easy-to-adjust properties further lead to the diversity of active materials. In addition, compared with single metal TMC, TMC solid solution exhibits better synergistic sodium storage characteristics due to its multi-component characteristics. However, with the increasing market demand for electric vehicles, the requirements for electrode materials with large capacity and high rate performance are getting higher and higher. Therefore, it is still a huge challenge to develop metal chalcogenide solid solution electrode materials with excellent structures to improve ion transport kinetics and cycle life and effectively suppress volume expansion. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a new type of metal sulfide solid solution electrode material and its preparation method and application, and propose a metal sulfide solid solution electrode material with a branch-leaf composite structure, which has ultra-high reversible capacity, ultra-long cycle life and good structural stability at ultra-high rate, and solves the problems of slow ion transfer rate and severe volume expansion existing in existing metal sulfide electrode materials.

[0005] To achieve the above-mentioned object, the present invention provides the following technical solution: a novel metal chalcogenide solid solution electrode material, wherein the electrode material has a branch-leaf structure at the microscopic level, and is composed of a carbon network support as a "branch" and a metal chalcogenide solid solution nanosheet as a "leaves", and the electrode material has a chemical composition represented by CNS@CoSX@C, wherein X is a non-metallic element Se or Te, and CNS is specifically a carbon network support (carbon network supporting).

[0006] Preferably, the carbon network support is a carbon fiber support derived from polyacrylonitrile membrane, a carbon fiber support derived from bacterial cellulose, a hollow carbon tube support derived from biomass rush, carbon cloth or graphite felt; and the metal sulfide solid solution is a Co-based solid solution.

[0007] Another object of the present invention is to provide a method for preparing the novel metal chalcogenide solid solution electrode material, comprising the following steps:

[0008] 1) Soaking the prepared carbon network scaffold in a 2-methylimidazole aqueous solution containing a cobalt source for 0.5 to 3 hours, and then washing the obtained product with deionized water and anhydrous ethanol in turn, and drying, to obtain a branch-leaf-shaped CNS@ZIF-67 composite material;

[0009] 2) heating the CNS@ZIF-67 composite material obtained in step 1) to 200-400° C. in a protective atmosphere for 1-6 hours, then subjecting it to high-temperature carbonization treatment, and cooling it naturally after the reaction to obtain a CNS@Co@C composite material;

[0010] 3) putting the CNS@Co@C and the sulfur source obtained in step 2) into two porcelain boats and wrapping them with a piece of tin foil, and then subjecting them to high-temperature vulcanization treatment in a protective atmosphere. After the reaction is completed, the temperature is naturally lowered to prepare a CNF@CoS2@C composite material;

[0011] 4) The CNS@CoS2@C and selenium powder or tellurium powder prepared in step 3) are placed in two porcelain boats respectively and wrapped with a piece of tin foil, and then subjected to selenization or tellurization treatment in a protective atmosphere. After the reaction is completed, the temperature is naturally lowered to obtain the novel metal sulfide solid solution electrode material.

[0012] Preferably, the cobalt source is one or more of cobalt nitrate, cobalt acetate and cobalt chloride; and the sulfur source is sublimated sulfur and / or thiourea.

[0013] Preferably, the molar ratio of the cobalt source to 2-methylimidazole in the 2-methylimidazole aqueous solution containing the cobalt source is 1:6 to 1:10.

[0014] Preferably, the mass ratio of the CNS@Co@C to the sulfur source is 1:1 to 1:5; the mass ratio of the CNS@CoS2@C to selenium powder or tellurium powder is 2:1 to 1:2.

[0015] Preferably, the high temperature carbonization treatment is heated to 500-900°C at a heating rate of 3-8°C / min, and the treatment time is 0.5-5h; the high temperature vulcanization treatment is heated to 400-700°C at a heating rate of 1-5°C / min, and the treatment time is 0.5-5h.

[0016] Preferably, the selenization or tellurization treatment is carried out at a heating rate of 1 to 5°C / min to 500 to 800°C, and the treatment time is 0.5 to 5h.

[0017] Preferably, the protective atmosphere is argon or nitrogen.

[0018] Another object of the present invention is to provide the use of the above-mentioned novel metal sulfide solid solution electrode material or the novel metal sulfide solid solution electrode material prepared by the above-mentioned method in sodium ion batteries.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The novel metal sulfide solid solution electrode material provided by the present invention has a branch-leaf structure by using a CNS scaffold as a skeleton and stacking metal sulfide solid solution nanosheets on the skeleton. Among them, this structure not only has good structural flexibility during the charge and discharge process, but also can serve as a protective layer for the solid solution activator for a long time; and all the solid solution nanosheet units are anchored on the CNS scaffold in turn, ensuring good electronic conductivity between each unit, and preventing the dissolution of polymer molecules during the sodium ion extraction and insertion process. More importantly, the three-dimensional network structure composed of carbon fibers can increase the contact area between the electrolyte and the activator, promote the penetration of the electrolyte, and shorten the distance of sodium ion insertion. In addition, each MOFs-derived solid solution unit has a good multi-level reaction interface protection layer, which can provide space for volume expansion for the internal active material step by step. In addition, the introduction of guest anion Se or Te elements into the TMC matrix of the present invention can significantly improve the charge transfer kinetics and effectively inhibit the volume expansion of TMC. At the same time, the intervention of larger Se or Te atoms is expected to expand the interlayer distance of TMC, thereby changing its lattice parameters, which is beneficial to Na + ion diffusion. And because the electronegativity of Se or Te is lower than that of S, this means that the M-Se / Te bond is easier to break than the MS bond, which is conducive to the occurrence of the conversion reaction. More importantly, the replacement of S in TMC with Se or Te can minimize the band gap of the material, thereby improving the conductivity of TMC. Therefore, the "branch-leaf" shaped metal sulfide solid solution formed by the present invention can provide channels and more active sites for electron and ion transmission and penetration, thereby improving the electrochemical performance. The electrode material of the present invention has a high specific capacity and still has good retention after 13,000 cycles, showing good and cyclically stable electrochemical performance, and still has good structural stability and cycle life at ultra-high rates. It solves the problems of slow ion transmission rate and severe volume expansion of existing metal sulfide electrode materials, and has good application prospects.

[0021] 2. The novel "branch-leaf" shaped metal sulfide solid solution electrode material prepared by the present invention uses a carbon network scaffold as the main raw material, and is prepared and synthesized by means of high-temperature carbonization, sulfurization, and selenization / tellurization treatment. Compared with metal sulfide solid solutions synthesized by other methods, the raw material cost of the present invention is low, the process is simple, the energy consumption is low, and the reaction conditions are easier to achieve. It can be mass-produced and is convenient for commercial application. The "branch-leaf" shaped metal sulfide solid solution electrode material of the present invention exhibits an ultra-long cycle life, a large reversible specific capacity, and excellent rate performance, showing great application prospects in sodium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Scanning electron microscope images of PAN@ZIF-67 and CNF@Co@C obtained in Example 1; a and b are PAN@ZIF-67, and c and d are CNF@Co@C.

[0023] Figure 2 These are the scanning electron microscope and transmission electron microscope images of CNF@CoSSe@C obtained in Example 1.

[0024] Figure 3 This is the X-ray diffraction pattern of the CNF@CoSSe@C electrode material obtained in Example 1.

[0025] Figure 4 This is the thermogravimetric analysis diagram of the CNF@CoSSe@C electrode material obtained in Example 1.

[0026] Figure 5 This is the X-ray photoelectron spectrum of the CNF@CoSSe@C electrode material obtained in Example 1.

[0027] Figure 6 CV curves of the CNF@CoSSe@C electrode material obtained in Example 1 at different scan rates.

[0028] Figure 7 This is the rate performance diagram of the CNF@CoSSe@C electrode material obtained in Example 1.

[0029] Figure 8 The half-cell prepared for CNF@CoSSe@C electrode material was subjected to 1.0 A g -1 Charge and discharge curves under current density (a) and cycle stability test (b).

[0030] Fig. 9 The half-cell prepared with CNF@CoSSe@C electrode material at 20.0A g -1 Cyclic voltammetry curves at different current densities. DETAILED DESCRIPTION

[0031] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, but the embodiments are not intended to limit the present invention. Experimental methods without specific conditions in the preferred embodiments are usually carried out under conventional conditions or under conditions recommended by the reagent manufacturer.

[0032] 1. Preparation method of a new type of metal chalcogenide solid solution electrode material

[0033] Example 1

[0034] 1) Preparation of carbon network scaffold: 1 g of polyacrylonitrile with a molecular weight of 15,000 was dissolved in 10 ml of NN dimethylformamide solution and stirred for 6 h to obtain a spinning solution, which was then injected into a syringe and spun by an electrospinning machine at a spinning speed of 0.6 ml / h, an applied voltage of 16.0 kV, and a distance from the needle tip to the receiver of 15 cm, thereby preparing a PAN nanofiber film.

[0035] 2) Preparation of "branch-leaf" shaped PAN@ZIF-67 precursor: Dissolve 0.594Co(NO3)2.6H2O in 40ml of deionized water to form solution A; dissolve 1.3g of 2-methylimidazole in 40ml of deionized water to form solution B; then quickly pour solution A into solution B and continue stirring for 30s to obtain a purple solution of 2-methylimidazole containing a cobalt source. Cut the PAN fiber membrane obtained in step 1) into a 10×10cm square film and spread it flat in a culture dish, then pour the purple solution into the culture dish containing the fiber membrane, soak it for 1h, take out the purple fiber membrane, wash it with deionized water and anhydrous ethanol, and dry it to obtain a "branch-leaf" shaped PAN@ZIF-67 precursor.

[0036] 3) Preparation of "branch-leaf" shaped CNF@Co@C composite materials: The PAN@ZIF-67 fiber membrane prepared in step 2) was further cut into 1.5×3 cm rectangular films and placed in a porcelain boat. The films were then heated to 350°C at a heating rate of 2°C / min in an argon atmosphere in a tubular furnace and kept for 1 h. The films were then heated to 600°C at a heating rate of 5°C / min and carbonized for 2 h. After the reaction was completed, the film was cooled naturally to obtain a CNF@Co@C composite material.

[0037] 4) Preparation of "branch-leaf" shaped CNF@CoS2@C composite material: 0.2 g of CNF@Co@C obtained in step 3) and 0.8 g of sublimated sulfur were placed in two porcelain boats respectively and wrapped with a piece of tin foil. They were then directly transferred into an argon-filled tubular furnace and heated to 500°C at a heating rate of 2°C / min and maintained for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the CNF@CoS2@C composite material.

[0038] 5) Preparation of "branch-leaf" shaped CNF@CoSSe@C composite material: 0.2 g of CNF@CoS2@C obtained in step 4) and 0.2 g of selenium powder were placed in two porcelain boats respectively and wrapped with a piece of tin foil. They were then directly transferred into an argon-filled tubular furnace and heated to 500°C at a heating rate of 2°C / min and maintained for 2 h. After the reaction was completed, the temperature was naturally lowered to obtain the CNF@CoSSe@C composite material.

[0039] Example 2

[0040] 1) Preparation of carbon network scaffold: A 10×10 cm carbon cloth was immersed in 100 ml of concentrated nitric acid, treated with acid at 80°C for 8 h, and then ultrasonically treated with deionized water and anhydrous ethanol five times each to obtain a carbon cloth (CC) with rich functional groups.

[0041] 2) Preparation of "branch-leaf" shaped PAN@ZIF-67 precursor: Dissolve 0.594Co(NO3)2.6H2O in 40ml of deionized water to form solution A; dissolve 1.3g of 2-methylimidazole in 40ml of deionized water to form solution B; then quickly pour solution A into solution B and continue stirring for 30s to obtain a purple solution of 2-methylimidazole containing a cobalt source. Spread the CC obtained in step 1) in a culture dish, and then pour the purple solution into the culture dish containing the fiber membrane. After soaking for 1h, take out the purple fiber membrane, wash it with deionized water and anhydrous ethanol, and dry it to obtain a "branch-leaf" shaped CC@ZIF-67 precursor.

[0042] 3) Preparation of "branch-leaf" shaped CC@Co@C composite materials: The CC@ZIF-67 fiber membrane obtained in step 2) was further cut into 1.5×3 cm rectangular films and placed in a porcelain boat. The films were then heated to 350°C at a heating rate of 2°C / min in an argon atmosphere in a tubular furnace and kept for 1 h. The films were then heated to 600°C at a heating rate of 5°C / min and carbonized for 2 h. After the reaction was completed, the film was cooled naturally to obtain a CC@Co@C composite material.

[0043] 4) Preparation of "branch-leaf" shaped CC@CoS2@C composite material: 0.2 g of CC@Co@C obtained in step 3) and 0.8 g of sublimated sulfur were placed in two porcelain boats respectively and wrapped with a piece of tin foil. They were then directly transferred into a tubular furnace filled with argon and heated to 500°C at a heating rate of 2°C / min and maintained for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the CC@CoS2@C composite material.

[0044] 5) Preparation of "branch-leaf" shaped CC@CoSSe@C composite material: 0.2 g of CC@CoS2@C obtained in step 4) and 0.2 g of selenium powder were placed in two porcelain boats respectively and wrapped with a piece of tin foil. Then, they were directly transferred into a tubular furnace filled with argon and heated to 500°C at a heating rate of 2°C / min and maintained for 2 h. After the reaction was completed, the temperature was naturally lowered to obtain the CC@CoSSe@C composite material.

[0045] Example 3

[0046] 1) Preparation of carbon network scaffold: 10×10 cm graphite felt was immersed in 100 ml of concentrated nitric acid, treated with acid at 80° C. for 8 h, and then ultrasonically treated with deionized water and anhydrous ethanol five times each to obtain carbon cloth (GF) with rich functional groups.

[0047] 2) Preparation of "branch-leaf" GF@ZIF-67 precursor: Dissolve 0.594Co(NO3)2.6H2O in 40ml deionized water to form solution A; dissolve 1.3g of 2-methylimidazole in 40ml deionized water to form solution B; then quickly pour solution A into solution B and continue stirring for 30s to obtain a purple solution of 2-methylimidazole containing a cobalt source. Cut the GF obtained in step 1) into a 3×6cm strip structure and soak it in the purple solution for 1h, then take out the purple fiber membrane, wash it with deionized water and anhydrous ethanol and dry it to obtain a "branch-leaf" GF@ZIF-67 precursor.

[0048] 3) Preparation of "branch-leaf" shaped GF@Co@C composite material: The GF@ZIF-67 fiber membrane obtained in step 2) was further cut into a rectangular film of 1.5×3 cm and placed in a porcelain boat. The film was then heated to 350°C at a heating rate of 2°C / min in an argon atmosphere in a tubular furnace and kept for 1 hour. The film was then heated to 600°C at a heating rate of 5°C / min and carbonized for 2 hours. After the reaction was completed, the film was cooled naturally to obtain a GF@Co@C composite material.

[0049] 4) Preparation of "branch-leaf" shaped GF@CoS2@C composite material: 0.2 g of GF@Co@C obtained in step 3) and 0.8 g of sublimated sulfur were placed in two porcelain boats respectively and wrapped with a piece of tin foil. They were then directly transferred into a tubular furnace filled with argon and heated to 500°C at a heating rate of 2°C / min and maintained for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the GF@CoS2@C composite material.

[0050] 5) Preparation of "branch-leaf" shaped GF@CoSSe@C composite material: 0.2 g of GF@CoS2@C obtained in step 4) and 0.2 g of selenium powder were placed in two porcelain boats respectively and wrapped with a piece of tin foil. Then, they were directly transferred into a tubular furnace filled with argon and heated to 500°C at a heating rate of 2°C / min and maintained for 2 h. After the reaction was completed, the temperature was naturally lowered to obtain the GF@CoSSe@C composite material.

[0051] Example 4

[0052] 1) Preparation of carbon network scaffold: The bacterial cellulose membrane was cut into 3×4 cm rectangular films, and then transferred into an argon-filled tubular furnace and heated to 800°C at a heating rate of 2°C / min and maintained for 2 h to obtain bacterial cellulose mesoporous carbon nanofiber membrane (BPCNF).

[0053] 2) Preparation of "branch-leaf" shaped BPCNF@ZIF-67 precursor: Dissolve 0.594Co(NO3)2.6H2O in 40ml deionized water to form solution A; dissolve 1.3g of 2-methylimidazole in 40ml deionized water to form solution B; then quickly pour solution A into solution B and continue stirring for 30s to obtain a purple solution of 2-methylimidazole containing a cobalt source. Spread the BPCNF obtained in step 1) in a culture dish, and then pour the purple solution into the culture dish containing the BPCNF fiber membrane. After soaking for 1h, take out the purple fiber membrane, wash it with deionized water and anhydrous ethanol, and dry it to obtain a "branch-leaf" shaped BPCNF@ZIF-67 precursor.

[0054] 3) Preparation of "branch-leaf" shaped BPCNF@Co@C composite materials: The BPCNF@ZIF-67 fiber membrane obtained in step 2) was further cut into 1.5×1.5 cm films and placed in a porcelain boat. The film was then heated to 350°C at a heating rate of 2°C / min in an argon atmosphere in a tubular furnace and kept for 1 h. The film was then heated to 600°C at a heating rate of 5°C / min and carbonized for 2 h. After the reaction was completed, the film was cooled naturally to obtain the BPCNF@Co@C composite material.

[0055] 4) Preparation of "branch-leaf" shaped BPCNF@CoS2@C composite material: 0.2 g of BPCNF@Co@C obtained in step 3) and 0.8 g of sublimated sulfur were placed in two porcelain boats respectively and wrapped with a piece of tin foil. They were then directly transferred into an argon-filled tubular furnace and heated to 500°C at a heating rate of 2°C / min and maintained for 2 h. After the reaction was completed, the temperature was naturally lowered to obtain the BPCNF@CoS2@C composite material.

[0056] 5) Preparation of "branch-leaf" shaped BPCNF@CoSSe@C composite material: 0.2 g of BPCNF@CoS2@C obtained in step 4) and 0.2 g of selenium powder were placed in two porcelain boats respectively and wrapped with a piece of tin foil. Then, they were directly transferred into a tubular furnace filled with argon and heated to 500°C at a heating rate of 2°C / min and maintained for 2 h. After the reaction was completed, the temperature was naturally lowered to obtain the BPCNF@CoSSe@C composite material.

[0057] Example 5

[0058] 1) Preparation of carbon network scaffold: The biomass rush was soaked in deionized water for 10 h to remove the soluble ions or dust contained in the material, and then dried. It was then heated to 800 °C in a tubular furnace at a heating rate of 5 °C / min and maintained for 2 h. After natural cooling, a biomass rush-derived carbon scaffold structure (BJDC) was obtained.

[0059] 2) Preparation of "branch-leaf" shaped BJDC@ZIF-67 precursor: Dissolve 0.594Co(NO3)2.6H2O in 40ml of deionized water to form solution A; dissolve 1.3g of 2-methylimidazole in 40ml of deionized water to form solution B; then quickly pour solution A into solution B and continue stirring for 30s to obtain a purple solution of 2-methylimidazole containing a cobalt source. Put the BJDC in step 1) directly into the purple solution, soak for 1h, wash with deionized water and anhydrous ethanol and dry to obtain a "branch-leaf" shaped BJDC@ZIF-67 precursor.

[0060] 3) Preparation of "branch-leaf" shaped BJDC@Co@C composite material: The BJDC@ZIF-67 prepared in step 2) was placed in a porcelain boat, and then heated to 350°C at a heating rate of 2°C / min in an argon atmosphere in a tubular furnace and kept warm for 1 hour, then heated to 600°C at a heating rate of 5°C / min and carbonized for 2 hours. After the reaction was completed, the temperature was naturally lowered to obtain the BJDC@Co@C composite material.

[0061] 4) Preparation of "branch-leaf" shaped BJDC@CoS2@C composite material: 0.2 g of BJDC@Co@C obtained in step 3) and 0.8 g of sublimated sulfur were placed in two porcelain boats respectively and wrapped with a piece of tin foil. They were then directly transferred into an argon-filled tubular furnace and heated to 500°C at a heating rate of 2°C / min and maintained for 2 h. After the reaction was completed, the temperature was naturally lowered to prepare the BJDC@CoS2@C composite material.

[0062] 5) Preparation of "branch-leaf" shaped BJDC@CoSSe@C composite material: 0.2 g of BJDC@CoS2@C obtained in step 4) and 0.2 g of selenium powder were placed in two porcelain boats respectively and wrapped with tin foil. They were then directly transferred into an argon-filled tubular furnace and heated to 500°C at a heating rate of 2°C / min and maintained for 2 h. After the reaction was completed, the temperature was naturally lowered to obtain the BJDC@CoSSe@C composite material.

[0063] 2. Performance Testing

[0064] 1. The morphology of PAN@ZIF-67, CNF@Co@C and CNF@CoSSe@C electrode materials prepared in Example 1 was observed under a scanning microscope and a projection microscope. The results are as follows: Figure 1 and Figure 2 shown.

[0065] Depend on Figure 1 a and Figure 1 b It can be seen that a large number of ultra-thin ZIF-67 nanosheets with uniform morphology grow on the PAN nanofibers in the intermediate product PAN@ZIF-67, forming a "branch-leaf" morphology structure. Figure 1 c and Figure 1 d It can be seen that the CNF@Co@C obtained after carbonization of PAN@ZIF-67 precursor maintains a good "branch-leaf" morphology, but a large number of nanoparticles are attached to the surface of the nanosheets. Figure 2 It can be seen that the CNF@CoSSe@C composite material obtained after sulfidation and selenization treatment of CNF@Co@C still maintains the "branch-leaf" structural characteristics, but the particles on the surface of the nanosheets become larger and the surface is rougher than that of CNF@Co@C.

[0066] 2. The CNF@CoSSe@C electrode material prepared in Example 1 was subjected to X-ray diffraction, X-ray photoelectron spectroscopy and thermogravimetric analysis. The results are as follows: Figures 3 to 5 shown.

[0067] from Figure 3 From the X-ray diffraction pattern, it can be seen that the CNF@CoSSe@C composite material is mainly composed of cubic phase CoSSe, and a very broad diffraction peak appears at around 26°, proving that CNF has an amorphous crystal structure. Figure 4From the thermogravimetric analysis diagram, it can be seen that there is a mass loss from room temperature to 200°C, which is mainly caused by the volatilization of the attached water inside the sample. The mass loss from 200°C to 700°C is due to the reaction of S, Se and C with oxygen in the air to produce SO2, SeO2 and CO2 gases. The final stability at 700°C is due to the production of Co3O4. Through analysis, the mass percentage of CoSSe in the composite material is about 58.6%. Figure 5 It can be seen from the X-ray photoelectron spectrum that the CNF@CoSSe@C composite electrode material is mainly composed of four elements: Co, S, Se and C.

[0068] 3. Take the CNF@CoSSe@C composite material prepared in Example 1 as the negative electrode material and mix it with Ketjen black and CMC binder in a mass percentage of 60:30:10, then add an appropriate amount of deionized water, grind it in an agate mortar to a paste, apply it on a copper foil with a diameter of 13 mm, and then vacuum dry the copper foil at 80°C for 12 hours to obtain the negative electrode sheet of the sodium ion battery, and then transfer it to an argon-filled glove box for assembly of button batteries. The button battery model is CR2032, the metal sodium sheet is used as the counter electrode, the diaphragm is glass fiber, and the electrolyte is 1 mol / L NaCF3SO3 solution (the solvent is diethylene glycol dimethyl ether solution). The assembled battery was subjected to cyclic voltammetry (CV) tests at different scan rates of 0.2 to 2.0 mV / s (electrochemical workstation CHI-660E, voltage range of 0.01 to 3.0 V, the same below), and the results are as follows Figure 6 shown.

[0069] As can be seen from the figure, all the CV curves obtained detected the presence of 4 redox peaks, and the peak current gradually increased with the increase of the scan rate. In addition, as the scan rate increases, the curve shape remains good, indicating that the CNF@CoSSe@C composite material has good rate performance and small polarizability.

[0070] 4. CR2032 button cells assembled with CNF@CoSSe@C electrode materials were heated to 0.2~20.0Ag. -1 The discharge capacity was measured under the current density condition (on Land 2001A test system, the voltage range was 0.01~3.0V, the same below), and the results were as follows Figure 7 shown.

[0071] It can be seen from the figure that when the current density is 0.2A g -1 When the discharge capacity is 713.9 mAh g -1 When the current density changes rapidly to 20.0A g -1 When the specific capacity is still maintained at 0.2A g -1Then, when the current density gradually recovered to 0.2A g -1 When the capacity is restored to 607.0mAh g -1 , and its capacity retention rate is 85%, indicating that the CNF@CoSSe@C composite material has excellent rate performance.

[0072] 5. CR2032 button cells assembled with CNF@CoSSe@C electrode materials were heated to 1.0A g -1 The cycle stability test was carried out at a current density of Figure 8 shown.

[0073] from Figure 8 As can be seen from a, the initial charge and discharge capacities of the CNF@CoSSe@C electrode material prepared in the present invention are 661.6 mAh g -1 and 480.9mAh g -1 , the corresponding initial Coulomb efficiency is 72.7%. Figure 8 As can be seen in b, after the electrode has been cycled 250 times, its discharge capacity is still 432.5 mAh g -1 , the capacity retention is 65.4% of the initial discharge capacity, indicating that the material has a large specific capacity and excellent cycle stability.

[0074] 6. CR2032 button cells assembled with CNF@CoSSe@C electrode materials were heated at 20.0A g -1 The cycle stability test was carried out at a current density of Fig. 9 shown.

[0075] It can be seen from the figure that the initial discharge capacity of the CNF@CoSSe@C electrode material prepared by the present invention is 310.7 mAh g -1 After 13,000 cycles, its discharge capacity is still 158.2 mAh g -1 The average capacity decay rate per cycle is only 0.01%, indicating that the material still has good structural stability and cycle life at ultra-high rates. It should be noted that the electrode materials prepared in Examples 2 to 5 also have good and cycle-stable electrochemical properties, which are not listed here one by one.

[0076] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A novel metal chalcogenide solid solution electrode material, characterized in that: The electrode material has a branch-leaf structure at the microscopic level, consisting of a carbon network support as a "branch" and a metal chalcogenide solid solution nanosheet as a "leaves", and the electrode material has a chemical composition represented by CNS@CoSX@C, wherein X is a non-metallic element Se or Te, and the CNS is a carbon network support and has an amorphous crystal structure; The method for preparing the novel metal chalcogenide solid solution electrode material comprises the following steps: 1) The prepared carbon network scaffold was immersed in a 2-methylimidazole aqueous solution containing a cobalt source for 0.5 to 3 h, and then the obtained product was washed with deionized water and anhydrous ethanol in sequence and dried to obtain a branch-leaf-shaped CNS@ZIF-67 composite material; 2) The CNS@ZIF-67 composite material prepared in step 1) is heated to 200-400°C in a protective atmosphere and kept at this temperature for 1-6 hours, and then subjected to high-temperature carbonization treatment. After the reaction is completed, the temperature is naturally lowered to prepare a CNS@Co@C composite material; 3) The CNS@Co@C and the sulfur source prepared in step 2) are placed in two porcelain boats respectively and wrapped with a piece of tin foil, and then subjected to high-temperature vulcanization treatment in a protective atmosphere. After the reaction is completed, the temperature is naturally lowered to prepare a CNS@CoS2@C composite material; 4) The CNS@CoS2@C and selenium powder or tellurium powder prepared in step 3) are placed in two porcelain boats respectively and wrapped with a piece of tin foil, and then subjected to selenization or tellurization treatment in a protective atmosphere. After the reaction is completed, the temperature is naturally lowered to obtain the novel metal sulfide solid solution electrode material.

2. The novel metal chalcogenide solid solution electrode material according to claim 1, characterized in that: The carbon network support is a carbon fiber support derived from polyacrylonitrile membrane, a carbon fiber support derived from bacterial cellulose, a hollow carbon tube support derived from biomass rush, carbon cloth or graphite felt; The metal chalcogenide solid solution is a Co-based solid solution.

3. The novel metal chalcogenide solid solution electrode material according to claim 1, characterized in that: The cobalt source is one or more of cobalt nitrate, cobalt acetate and cobalt chloride; the sulfur source is sublimated sulfur and / or thiourea.

4. The novel metal chalcogenide solid solution electrode material according to claim 1, characterized in that: The molar ratio of the cobalt source to 2-methylimidazole in the 2-methylimidazole aqueous solution containing the cobalt source is 1:6 to 1:

10.

5. The novel metal chalcogenide solid solution electrode material according to claim 1, characterized in that: The mass ratio of the CNS@Co@C to the sulfur source is 1:1 to 1:5; the mass ratio of the CNS@CoS2@C to selenium powder or tellurium powder is 2:1 to 1:

2.

6. The novel metal chalcogenide solid solution electrode material according to claim 1, characterized in that: The high temperature carbonization treatment is carried out at a heating rate of 3 to 8 °C / min to 500 to 900 °C, and the treatment time is 0.5 to 5 h; the high temperature vulcanization treatment is carried out at a heating rate of 1 to 5 °C / min to 400 to 700 °C, and the treatment time is 0.5 to 5 h.

7. The novel metal chalcogenide solid solution electrode material according to claim 1, characterized in that: The selenization or tellurization treatment is carried out at a heating rate of 1 to 5 °C / min to 500 to 800 °C, and the treatment time is 0.5 to 5 h.

8. The novel metal chalcogenide solid solution electrode material according to claim 1, characterized in that: The protective atmosphere is argon or nitrogen.

9. Use of the novel metal sulfide solid solution electrode material according to any one of claims 1 to 8 in sodium ion batteries.