Urethane resin composition and leather sheet

A urethane resin composition using biomass-derived polycarbonate polyol and nonionic emulsifiers addresses the challenges of hand feel and stability in synthetic leather, offering enhanced oleic acid resistance and formulation stability.

CN114729183BActive Publication Date: 2024-12-06DIC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080074900.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-28
Filing Date
2020-09-10
Publication Date
2024-12-06
Estimated Expiration
2040-09-10

AI Technical Summary

Technical Problem

Existing urethane resin compositions used in synthetic leather face challenges in achieving excellent hand feel, stability, and oleic acid resistance, particularly with the increasing demand for biomass raw materials and restrictions on volatile organic compounds.

Method used

A urethane resin composition using polycarbonate polyol derived from biomass, combined with anionic and nonionic groups, nonionic emulsifiers, and water, to enhance oleic acid resistance, hand feel, and formulation stability.

Benefits of technology

The composition provides excellent oleic acid resistance, hand feel, and formulation stability, making it suitable for use as an impregnation resin for fiber substrates, while being environmentally friendly by utilizing biomass-derived materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004740078570000141
    Figure GDA0004740078570000141
  • Figure GDA0004740078570000151
    Figure GDA0004740078570000151
  • Figure GDA0004740078570000152
    Figure GDA0004740078570000152
Patent Text Reader

Abstract

The problem to be solved by the present invention is to provide a carbamate resin composition, which uses biomass raw materials in a carbamate resin composition containing water and has excellent oleic acid resistance, hand feel and formulation stability. The present invention provides a carbamate resin composition, characterized in that it contains a carbamate resin (A) having anionic groups and nonionic groups, a nonionic emulsifier (B) and water (C), wherein the carbamate resin (A) uses polycarbonate polyol (a1) as a raw material, and the polycarbonate polyol (a1) uses decanediol derived from biomass as a raw material. In addition, the present invention provides a leather piece, characterized in that a coagulant of the carbamate resin composition is present in a fiber substrate. The carbamate resin (A) and the nonionic emulsifier (B) both preferably have oxyethylene groups and oxypropylene groups.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a urethane resin composition and a leather sheet. Background Art

[0002] Polyurethane resins are widely used in the manufacture of synthetic leather (including artificial leather) due to their good mechanical strength and hand feel. Among the above uses, solvent-based urethane resins containing N,N-dimethylformamide (DMF) have been the mainstream so far. However, against the background of DMF restrictions in Europe, the strengthening of volatile organic compounds (VOC) emission restrictions in China, and DMF restrictions by large clothing manufacturers, the de-DMFization of urethane resins used in each layer of synthetic leather is sought.

[0003] In order to cope with such environmental changes, urethane resin compositions in which urethane resin is dispersed in water have been widely studied (for example, see Patent Document 1). However, in existing products including the invention described in Patent Document 1, it is difficult to achieve both excellent hand feel and stability of the prepared solution.

[0004] Furthermore, in recent years, against the backdrop of global warming and the depletion of petroleum resources, there has been an increasing global demand for biomass raw materials such as plants in order to reduce the use of fossil resources such as petroleum.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2007-119749 Summary of the invention

[0008] Problems to be solved by the invention

[0009] The problem to be solved by the present invention is to provide a urethane resin composition which uses a biomass raw material in a urethane resin composition containing water and has excellent oleic acid resistance, hand feel and formulation stability.

[0010] Technical means of solving problems

[0011] The present invention provides a urethane resin composition, which contains a urethane resin (A) having anionic groups and nonionic groups, a nonionic emulsifier (B) and water (C), wherein the urethane resin (A) uses a polycarbonate polyol (a1) as a raw material, and the polycarbonate polyol (a1) uses decanediol derived from biomass as a raw material.

[0012] The present invention also provides a leather sheet comprising a fiber base material containing a coagulated product of the urethane resin composition.

[0013] Effects of the Invention

[0014] The urethane resin composition of the present invention contains water and uses biomass raw materials, so it is environmentally friendly. In addition, the urethane resin composition is excellent in oleic acid resistance, hand feel and formulation stability. Therefore, the urethane resin composition can be particularly suitable for use as an impregnation resin for a fiber substrate. DETAILED DESCRIPTION

[0015] The urethane resin composition of the present invention contains a urethane resin (A) having an anionic group and a nonionic group, a nonionic emulsifier (B) and water (C). The urethane resin (A) uses a polycarbonate polyol (a1) as a raw material, and the polycarbonate polyol (a1) uses decanediol derived from biomass as a raw material.

[0016] In order to obtain excellent oleic acid resistance and hand feel, the urethane resin (A) used in the present invention must use a polycarbonate polyol (a1) using decanediol derived from biomass as a raw material. In addition, since the decanediol is also a raw material derived from biomass, a material that is more environmentally friendly can be provided. As the polycarbonate polyol (a1), for example, a reaction product of a diol compound containing decanediol derived from biomass and a carbonate and / or phosgene can be used, specifically, the polycarbonate polyol (a1) described in Japanese Patent Laid-Open No. 2018-127758 Gazette can be used.

[0017] As the decanediol, 1,10-decanediol is preferably used because more excellent oleic acid resistance, hand feel, and low-temperature flexural properties can be obtained.

[0018] As the diol compound that can be used other than the decanediol, for example, ethylene glycol, propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,3-butylene glycol, 1,2-butylene glycol, 2-methyl-1,3-propylene glycol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 1,5-hexanediol, 3-methyl-1,5-pentanediol, 2-methyl-1,8-octanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,8-nonanediol, 2-ethyl-2-butyl-1,3-propylene glycol, 1,12-dodecanediol, 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, trimethylolpropane, trimethylolethane, glycerol, ε-caprolactone, etc. These compounds may be used alone or in combination of two or more. Among these, butanediol is preferably used, and 1,4-butanediol is more preferably used, because more excellent oleic acid resistance, hand feel, and low-temperature flexural properties can be obtained.

[0019] When the biomass-derived decanediol and the butanediol are used in combination, the total amount thereof used is preferably 50 mol% or more, more preferably 70 mol% or more, and even more preferably 80 mol% or more in the diol compound.

[0020] When the biomass-derived decanediol (C10) and butanediol (C4) are used in combination, the molar ratio [(C4) / (C10)] thereof is preferably in the range of 5 / 95 to 95 / 5, more preferably in the range of 50 / 50 to 98 / 2, and still more preferably in the range of 70 / 30 to 95 / 5, in terms of obtaining better oleic acid resistance and low-temperature flexural properties.

[0021] As the carbonate ester, for example, dimethyl carbonate, diethyl carbonate, diphenyl carbonate, ethylene carbonate, propylene carbonate, etc. These compounds may be used alone or in combination of two or more.

[0022] The number average molecular weight of the polycarbonate polyol (a1) is preferably in the range of 500 to 100,000, and more preferably in the range of 700 to 5,000, in order to obtain more excellent oleic acid resistance and low-temperature flexural properties. The number average molecular weight of the polycarbonate polyol (a1) is a value measured by gel permeation chromatography (GPC).

[0023] As the preferred polycarbonate polyol (a1), for example, "Benebiol NL-3010DB" and "Benebiol NL-3030DB" manufactured by Mitsubishi Chemical Corporation are available as commercial products.

[0024] The urethane resin (A) must have anionic groups and nonionic groups in order to achieve both excellent hand feel and stability of the prepared solution. The anionic groups and nonionic groups are provided by the compound (a2) having anionic groups and the compound (a3) ​​having nonionic groups, respectively.

[0025] As the compound (a2) having an anionic group, for example, compounds having a carboxyl group such as 2,2-dimethylol propionic acid, 2,2-dimethylol butanoic acid, and 2,2-dimethylol butyric acid; 3,4-diaminobutanesulfonic acid, 3,6-diamino-2-toluenesulfonic acid, 2,6-diaminobenzenesulfonic acid, N-(2-aminoethyl)-2-aminosulfonic acid, N-(2-aminoethyl)-2-aminoethylsulfonic acid, N-2-aminoethane-2-aminosulfonic acid, and N-(2-aminoethyl)-β-alanine; compounds having a sulfonyl group such as salts thereof, etc. These compounds may be used alone or in combination of two or more.

[0026] As the compound (a3) ​​having a nonionic group, for example, compounds having an oxyethylene structure and / or an oxypropylene group, such as polyethylene glycol, polyoxypropylene glycol, polyoxyethylene polyoxypropylene glycol, polyoxyethylene polyoxytetramethylene glycol, and polyethylene glycol monomethyl ether, can be used. These compounds can be used alone or in combination of two or more.

[0027] The nonionic group possessed by the urethane resin (A) used in the present invention preferably contains oxyethylene groups and oxypropylene groups in terms of obtaining a more excellent texture and a formulated liquid stability. In terms of obtaining a more excellent texture and a formulated liquid stability by incorporating these low-crystalline components into the main chain of the urethane resin (A), it is preferably supplied from a polyol containing oxyethylene groups and oxypropylene groups, and more preferably polyoxyethylene polyoxypropylene glycol.

[0028] The number average molecular weight of the polyoxyethylene polyoxypropylene glycol is preferably in the range of 500 to 10,000, and more preferably in the range of 1,000 to 4,000, in order to obtain a more excellent texture and stability of the prepared solution. The number average molecular weight of the polyoxyethylene polyoxypropylene glycol refers to a value measured by gel permeation chromatography (GPC).

[0029] The molar ratio (EO / PO) of the oxyethylene group (EO) to the oxypropylene group (PO) in the urethane resin (A) is preferably in the range of 20 / 80 to 90 / 10, more preferably in the range of 40 / 60 to 85 / 15, in order to obtain better texture and formulation stability.

[0030] The amount of the compound (a3) ​​having a nonionic group used is preferably in the range of 0.1% by mass to 20% by mass, more preferably in the range of 0.5% by mass to 15% by mass, in the raw materials constituting the urethane resin (A) in order to obtain better hydrolysis resistance, feel and formulation stability.

[0031] Specifically, for example, the urethane resin (A) may be a reaction product of a polyol including the polycarbonate polyol (a1), the compound having an anionic group (a2), the compound having a nonionic group (a3), and a polyisocyanate (a4).

[0032] As the polyol, in addition to using the polycarbonate polyol (a1), other polyols may be used in combination within the range that does not impair the effect of the present invention. As the other polyols, polycarbonate polyols, polyester polyols, polyether polyols, polyacrylic acid polyols, etc. other than the (a1) may be used. These polyols may be used alone or in combination of two or more. As the number average molecular weight of these polyols, for example, a range of 500 to 100,000 may be cited. The number average molecular weight of the polyol represents a value measured by gel permeation chromatography (GPC).

[0033] The polyol may be used together with a chain extender having a number average molecular weight in the range of 50 to 450, if necessary. The number average molecular weight of the chain extender refers to a value calculated from a chemical structural formula.

[0034] As the chain extender, there can be used: a chain extender having a hydroxyl group, such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, hexamethylene glycol, sucrose, methylene glycol, glycerol, sorbitol, bisphenol A, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, etc.; a chain extender having an amino group, such as ethylenediamine, 1,2-propylenediamine, 1,6-hexamethylenediamine, piperazine, 2,5-dimethylpiperazine, isophoronediamine, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4,4'-dicyclohexylmethanediamine, 3,3'-dimethyl-4,4'-dicyclohexylmethanediamine, hydrazine, etc. These chain extenders can be used alone or in combination of two or more. Among these, the chain extender having an amino group is preferred because more excellent hydrolysis resistance and light resistance can be obtained.

[0035] As the polyisocyanate (a4), for example, aromatic polyisocyanates such as phenylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, polymethylene polyphenyl polyisocyanate, and carbodiimidized diphenylmethane polyisocyanate can be used; aliphatic or alicyclic polyisocyanates such as hexamethylene diisocyanate, lysine diisocyanate, dimer acid diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, xylene diisocyanate, tetramethylxylene diisocyanate, and norbornene diisocyanate can be used. These polyisocyanates can be used alone or in combination of two or more. Among these, in terms of obtaining a more excellent light resistance, preferably aliphatic polyisocyanates and / or alicyclic polyisocyanates, more preferably alicyclic polyisocyanates.

[0036] Examples of the method for producing the urethane resin (A) include a method of charging the raw materials together and reacting them, etc. Examples of the method for producing the urethane resin (A) include a method of performing the reaction at a temperature of 50° C. to 100° C. for 3 to 10 hours.

[0037] When the carbamate resin (A) is produced, it is preferred to inactivate the isocyanate groups remaining in the carbamate resin (A). When the isocyanate groups are inactivated, it is preferred to use an alcohol having a hydroxyl group such as methanol. When the alcohol is used, the amount used is preferably in the range of 0.001 to 10 parts by mass relative to 100 parts by mass of the carbamate resin (A).

[0038] In addition, an organic solvent may be used when producing the urethane resin (A). As the organic solvent, for example, ketone compounds such as acetone and methyl ethyl ketone; ether compounds such as tetrahydrofuran and dioxane; acetate compounds such as ethyl acetate and butyl acetate; nitrile compounds such as acetonitrile; amide compounds such as dimethylformamide and N-methylpyrrolidone, etc. can be used. These organic solvents may be used alone or in combination of two or more. Furthermore, the organic solvent is preferably removed by distillation or the like.

[0039] The acid value of the urethane resin (A) is preferably in the range of 0.1 mgKOH / g to 15 mgKOH / g, and more preferably in the range of 1 mgKOH / g to 8 mgKOH / g, in order to obtain more excellent hydrolysis resistance, softness and hand feel. The acid value of the urethane resin (A) can be adjusted by the amount of the compound (a2) having an anionic group, and the determination method thereof is described in the Examples described below.

[0040] The weight average molecular weight of the urethane resin (A) is preferably in the range of 50,000 to 700,000, and more preferably in the range of 100,000 to 500,000, in order to obtain more excellent hydrolysis resistance, light resistance, and heat resistance. The weight average molecular weight of the urethane resin (A) refers to a value measured by gel permeation chromatography (GPC) under the following conditions.

[0041] The nonionic emulsifier (B) is an essential component in order to obtain excellent texture and stability of the prepared liquid.

[0042] As the nonionic emulsifier (B), for example, emulsifiers having oxyethylene groups such as polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene distyrenated phenyl ether, polyoxyethylene lauryl ether, polyoxyethylene oleyl ether, polyoxyethylene stearyl ether, and polyoxyethylene sorbitan tetraoleate; emulsifiers having oxyethylene groups and oxypropylene groups such as polyoxyethylene polyoxypropylene copolymers, etc. These nonionic emulsifiers may be used alone or in combination of two or more.

[0043] Among these, it is preferred to use an emulsifier having an oxyethylene group and an oxypropylene group in terms of obtaining a more excellent feel and stability of the formulated liquid. The average number of moles of the oxyethylene group added is preferably in the range of 5 to 100, and more preferably in the range of 10 to 50. The average number of moles of the oxypropylene group added is preferably in the range of 5 to 50, and more preferably in the range of 10 to 40.

[0044] As for the cloud point of the nonionic emulsifier (B), in terms of rapidly (sharp) solidifying when heated while maintaining excellent stability of the formulated liquid and obtaining a softer feel, it is preferably in the range of 40°C to 80°C, and more preferably in the range of 50°C to 80°C. Furthermore, the cloud point of the nonionic emulsifier (B) is determined according to the following method in accordance with the book (New-Introduction to Surfactants, written by Takehiko Fujimoto, Sanyo Chemical Industries, Ltd., 1992). That is, a 5% by mass aqueous solution of the nonionic emulsifier is kept at a constant temperature for 30 minutes, and it is observed whether the nonionic emulsifier is insoluble in the solution. When the temperature rises, the temperature at which the nonionic emulsifier begins to become insoluble is set as the cloud point.

[0045] The amount of the nonionic emulsifier (B) is preferably in the range of 0.1% by mass to 10% by mass, more preferably in the range of 1% by mass to 6% by mass, relative to 100 parts by mass of the urethane resin (A) (solid content), in order to obtain a more excellent feel and stability of the prepared solution.

[0046] As the water (C), for example, ion exchange water, distilled water, etc. can be used. These waters can be used alone or in combination of two or more. As the content of the water (C), for example, the range of 30% by mass to 90% by mass in the urethane resin composition can be cited.

[0047] The urethane resin composition of the present invention contains the urethane resin (A), the nonionic emulsifier (B), and the water (C) as essential components, but other additives may be used as necessary.

[0048] As the other additives, for example, coagulants, urethanization catalysts, neutralizers, silane coupling agents, tackifiers, fillers, thixotropy imparting agents, adhesion imparting agents, waxes, heat stabilizers, light resistance stabilizers, fluorescent whitening agents, foaming agents, pigments, dyes, conductivity imparting agents, antistatic agents, moisture permeability enhancers, water repellents, oil repellents, hollow foams, flame retardants, water absorbents, moisture absorbents, deodorants, foam stabilizers, anti-caking agents, anti-hydrolysis agents, etc. These additives can be used alone or in combination of two or more.

[0049] As described above, the urethane resin composition of the present invention contains water and uses biomass raw materials, so it is environmentally friendly. In addition, the urethane resin composition is excellent in oleic acid resistance, hand feel and formulation stability. Therefore, the urethane resin composition can be particularly suitable for use as an impregnation resin for a fiber substrate.

[0050] Next, the leather piece of the present invention will be described.

[0051] The leather sheet includes a coagulated product of the urethane resin composition in a fiber base material.

[0052] As the fiber substrate, for example, polyester fiber, polyethylene fiber, nylon fiber, acrylic fiber, polyurethane fiber, acetate fiber, rayon fiber, polylactic acid fiber, cotton, linen, silk, wool, glass fiber, carbon fiber, nonwoven fabrics, woven fabrics, knitted fabrics, etc. formed by blended fibers thereof, etc. can be used.

[0053] Examples of a method for producing the leather sheet include a method of impregnating the fiber base material with the urethane resin composition and then coagulating the urethane resin.

[0054] Examples of a method for impregnating the fiber base with the urethane resin aqueous dispersion include a method of directly immersing the fiber base in a tank storing the urethane resin aqueous dispersion and squeezing the fiber base using a mangle or the like.

[0055] Next, as a method for coagulating the urethane resin (A), for example, there can be mentioned a heat-sensitive coagulation method of heating the fiber base material impregnated with the urethane resin to 50° C. to 130° C., a method of treating with saturated steam (0 MPa to 0.6 MPa) at 100° C. or higher, or superheated steam at 160° C. to 190° C., etc. Thereafter, drying at 80° C. to 180° C. may be performed as necessary.

[0056] The leather sheet can be used for shoes, bags, clothing, furniture components such as chairs and sofas, automotive interior materials such as car seats and steering wheels, moisture-permeable and waterproof materials, artificial leather, abrasive materials, and core materials for felt pens.

[0057] An intermediate layer, an adhesive layer, a surface layer, a surface treatment layer, etc. may be laminated on the leather sheet as necessary.

[0058] Example

[0059] Hereinafter, the present invention will be described in more detail using examples.

[0060] [Example 1]

[0061] In a four-necked flask equipped with a stirrer, a reflux cooling tube, a thermometer and a nitrogen blowing tube, a biomass-derived polycarbonate polyol (using "Benebiol NL-3010DB" manufactured by Mitsubishi Chemical Co., Ltd., 1,4-butanediol and biomass-derived 1,10-decanediol as raw materials, with a number average molecular weight of 3,000, hereinafter referred to as "bio-PC (bio-PC ( PC)(1)”), 400 parts by mass, dimethylolpropionic acid (hereinafter referred to as “DMPA”), 6.2 parts by mass, polyoxyethylene polyoxypropylene glycol (number average molecular weight: 1,750, EO / PO=50 / 50, hereinafter referred to as “EOPO(1)”), and 516 parts by mass of methyl ethyl ketone were uniformly mixed, and then 78 parts by mass of dicyclohexylmethane diisocyanate (hereinafter referred to as “H12MDI”) was added, followed by 0.1 parts by mass of bismuth octylate, and the mixture was reacted at 70°C for about 1 hour to obtain a methyl ethyl ketone solution of a carbamate polymer. Next, 5 parts by mass of triethylamine and 16 parts by mass of a polyoxyethylene polyoxypropylene glycol emulsifier (average number of moles of oxyethylene groups added: 25, average number of moles of oxypropylene groups added: 30, cloud point: 58° C., hereinafter referred to as “EOPO emulsifier (1)”) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method and mixed, and then 797 parts by mass of ion exchange water and 15 parts by mass of isophorone diamine were added. The methyl ethyl ketone was then distilled off under reduced pressure to obtain a urethane resin composition (X-1) containing a urethane resin (A-1) (acid value of urethane resin (A-1): 5 mgKOH / g, weight average molecular weight: 280,000).

[0062] [Example 2]

[0063] Under a nitrogen stream, 400 parts by mass of a biomass-derived polycarbonate polyol (made from "Benebiol NL-3030DB" manufactured by Mitsubishi Chemical Corporation, 1,4-butanediol and biomass-derived 1,10-decanediol as raw materials, number average molecular weight: 3,000, hereinafter referred to as "bio-PC (2)"), 6.2 parts by mass of DMPA, 32 parts by mass of EOPO (1) and 516 parts by mass of methyl ethyl ketone were added to a four-necked flask equipped with a stirrer, a reflux cooling tube, a thermometer and a nitrogen blowing tube. After uniform mixing, 78 parts by mass of H12MDI and then 0.1 parts by mass of bismuth octylate were added, and the mixture was reacted at 70°C for about 1 hour to obtain a methyl ethyl ketone solution of a urethane polymer. Next, 5 parts by mass of triethylamine and 16 parts by mass of EOPO emulsifier (1) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method and mixed, and then 797 parts by mass of ion exchange water and 15 parts by mass of isophorone diamine were added. The methyl ethyl ketone was then distilled off under reduced pressure to obtain a urethane resin composition (X-2) containing a urethane resin (A-2) (acid value of the urethane resin (A-2): 5 mgKOH / g, weight average molecular weight: 310,000).

[0064] [Example 3]

[0065] Under a nitrogen flow, in a four-necked flask including a stirrer, a reflux cooling tube, a thermometer and a nitrogen blowing tube, 400 parts by mass of bio-PC (1), 6.2 parts by mass of DMPA, 32 parts by mass of polyoxyethylene polyoxypropylene glycol (number average molecular weight: 1,400, EO / PO=75 / 25, hereinafter referred to as "EOPO (2)"), and 518 parts by mass of methyl ethyl ketone were added. After uniform mixing, 80 parts by mass of H12MDI was added, followed by 0.1 parts by mass of bismuth octylate, and the mixture was reacted at 70°C for about 1 hour to obtain a methyl ethyl ketone solution of a carbamate polymer. Next, 5 parts by mass of triethylamine and 16 parts by mass of EOPO emulsifier (1) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method and mixed, and then 788 parts by mass of ion exchange water and 7.8 parts by mass of piperazine were added. The methyl ethyl ketone was then distilled off under reduced pressure to obtain a urethane resin composition (X-3) containing a urethane resin (A-3) (acid value of the urethane resin (A-3): 5 mgKOH / g, weight average molecular weight: 280,000).

[0066] [Example 4]

[0067] Under a nitrogen flow, in a four-necked flask including a stirrer, a reflux cooling tube, a thermometer and a nitrogen blowing tube, 400 parts by mass of bio-PC (1), 6.2 parts by mass of DMPA, 32 parts by mass of polyoxyethylene polyoxypropylene glycol (number average molecular weight: 3,000, EO / PO=75 / 25, hereinafter referred to as "EOPO (3)"), and 790 parts by mass of methyl ethyl ketone were added, and after uniform mixing, 75 parts by mass of H12MDI was added, followed by 0.1 parts by mass of bismuth octylate, and the mixture was reacted at 70°C for about 1 hour to obtain a methyl ethyl ketone solution of a carbamate polymer. Next, 5 parts by mass of triethylamine and 15 parts by mass of EOPO emulsifier (1) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method and mixed, and then 790 parts by mass of ion exchange water and 15 parts by mass of isophorone diamine were added. The methyl ethyl ketone was then distilled off under reduced pressure to obtain a urethane resin composition (X-4) containing a urethane resin (A-4) (acid value of the urethane resin (A-4): 5 mgKOH / g, weight average molecular weight: 260,000).

[0068] [Example 5]

[0069] Under a nitrogen flow, 400 parts by mass of bio-PC (1), 6.2 parts by mass of DMPA, 32 parts by mass of EOPO (1), and 516 parts by mass of methyl ethyl ketone were added to a four-necked flask including a stirrer, a reflux cooling tube, a thermometer, and a nitrogen blowing tube. After uniform mixing, 78 parts by mass of H12MDI was added, followed by 0.1 parts by mass of bismuth octylate, and the mixture was reacted at 70° C. for about 1 hour to obtain a methyl ethyl ketone solution of a carbamate polymer. Next, 5 parts by mass of triethylamine and 16 parts by mass of an emulsifier of polyoxyethylene polyoxypropylene glycol (average number of moles of oxyethylene groups added: 20, average number of moles of oxypropylene groups added: 20, cloud point: 70° C., hereinafter referred to as “EOPO emulsifier (2)”) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method and mixed, and then 797 parts by mass of ion exchange water and 15 parts by mass of isophorone diamine were added. The methyl ethyl ketone was then distilled off under reduced pressure to obtain a urethane resin composition (X-5) containing a urethane resin (A-5) (acid value of urethane resin (A-5): 5 mgKOH / g, weight average molecular weight: 240,000).

[0070] [Example 6]

[0071] Under a nitrogen flow, 400 parts by mass of bio-PC (1), 6.2 parts by mass of DMPA, 32 parts by mass of EOPO (1), and 510 parts by mass of methyl ethyl ketone were added to a four-necked flask including a stirrer, a reflux cooling tube, a thermometer, and a nitrogen blowing tube. After uniform mixing, 39 parts by mass of H12MDI and 33 parts by mass of isophorone diisocyanate (hereinafter referred to as "IPDI") were added, followed by 0.1 parts by mass of bismuth octylate. The mixture was reacted at 70° C. for about 1 hour to obtain a methyl ethyl ketone solution of a carbamate polymer. Next, 5 parts by mass of triethylamine and 16 parts by mass of EOPO emulsifier (1) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method and mixed, and then 788 parts by mass of ion exchange water and 15 parts by mass of isophorone diamine were added. The methyl ethyl ketone was then distilled off under reduced pressure to obtain a urethane resin composition (X-6) containing a urethane resin (A-6) (acid value of the urethane resin (A-6): 5 mgKOH / g, weight average molecular weight: 250,000).

[0072] [Comparative Example 1]

[0073] In Example 1, except that a room temperature solid polycarbonate polyol ("ETERNACOLL UH-200" manufactured by Ube Industries, Ltd., number average molecular weight: 2,000, hereinafter referred to as "non-bio PC") was used instead of bio-PC (1), the same procedure as in Example 1 was carried out to obtain a urethane resin composition (XR-1) containing a urethane resin (AR-1).

[0074] [Comparative Example 2]

[0075] Under nitrogen flow, 400 parts by mass of bio-PC (1), 32 parts by mass of EOPO (1), and 492 parts by mass of methyl ethyl ketone were added to a four-necked flask equipped with a stirrer, a reflux cooling tube, a thermometer, and a nitrogen blowing tube. After uniform mixing, 60 parts by mass of H12MDI were added, followed by 0.1 parts by mass of bismuth octylate, and the mixture was reacted at 70°C for about 1 hour to obtain a methyl ethyl ketone solution of a urethane polymer. Subsequently, 16 parts by mass of EOPO emulsifier (1) was added to the methyl ethyl ketone solution of a urethane polymer obtained by the above method, and the mixture was mixed. Then, 755 parts by mass of ion exchange water and 12 parts by mass of isophorone diamine were added, and the methyl ethyl ketone was distilled off under reduced pressure to obtain a urethane resin composition (XR-2) containing a urethane resin (AR-2) (acid value of urethane resin (AR-2): 0 mgKOH / g, weight average molecular weight: 270,000).

[0076] [Comparative Example 3]

[0077] Under nitrogen flow, 400 parts by mass of bio-PC (1), 6.2 parts by mass of DMPA, and 477 parts by mass of methyl ethyl ketone were added to a four-necked flask equipped with a stirrer, a reflux cooling tube, a thermometer, and a nitrogen blowing tube. After uniform mixing, 71 parts by mass of H12MDI were added, followed by 0.1 parts by mass of bismuth octylate, and the mixture was reacted at 70°C for about 1 hour to obtain a methyl ethyl ketone solution of a urethane polymer. Subsequently, 5 parts by mass of triethylamine and 16 parts by mass of EOPO emulsifier (1) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method, and the mixture was mixed. Then, 736 parts by mass of ion exchange water and 14 parts by mass of isophorone diamine were added, and the methyl ethyl ketone was distilled off under reduced pressure to obtain a urethane resin composition (XR-3) containing a urethane resin (AR-3) (acid value of the urethane resin (AR-3): 5 mgKOH / g, weight average molecular weight: 250,000).

[0078] [Comparative Example 4]

[0079] In Example 1, a urethane resin composition (XR-4) containing a urethane resin (AR-4) was obtained in the same manner as in Example 1 except that the EOPO emulsifier (1) was not used.

[0080] [Method for measuring number average molecular weight and weight average molecular weight]

[0081] The number average molecular weight of the polyol and the weight average molecular weight of the urethane resin used in the examples and comparative examples are values ​​measured by gel permeation chromatography (GPC) under the following conditions.

[0082] Measuring device: High-speed GPC device ("HLC-8220GPC" manufactured by Tosoh Corporation)

[0083] Column: The following columns manufactured by Tosoh Corporation were connected in series and used.

[0084] "TSKgel G5000" (7.8mm I.D. × 30cm) × 1 piece

[0085] "TSKgel G4000" (7.8mm I.D. × 30cm) × 1 piece

[0086] "TSKgel G3000" (7.8mm I.D. × 30cm) × 1 piece

[0087] "TSKgel G2000" (7.8mm I.D. × 30cm) × 1 piece

[0088] Detector: RI (differential refractometer)

[0089] Column temperature: 40℃

[0090] Eluent: tetrahydrofuran (THF)

[0091] Flow rate: 1.0mL / min

[0092] Injection volume: 100 μL (sample concentration is 0.4 mass% tetrahydrofuran solution)

[0093] Standard sample: The following standard polystyrene was used to prepare a standard curve.

[0094] (Standard Polystyrene)

[0095] "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation

[0096] "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation

[0097] "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation

[0098] "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation

[0099] "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation

[0100] "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation

[0101] "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation

[0102] "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation

[0103] "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation

[0104] "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation

[0105] "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation

[0106] "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation

[0107] "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation

[0108] "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation

[0109] [Method for measuring the acid value of urethane resin (A)]

[0110] The urethane resin composition obtained in the examples and comparative examples was dried, and 0.05 g to 0.5 g of the dried and solidified resin particles were weighed into a 300 mL conical flask. Then, about 80 mL of a mixed solvent having a mass ratio of tetrahydrofuran to ion exchange water [tetrahydrofuran / ion exchange water] of 80 / 20 was added to obtain a mixed solution.

[0111] Next, after mixing the phenolphthalein indicator in the mixed solution, titration is performed using a pre-calibrated 0.1 mol / L potassium hydroxide aqueous solution. The acid value (mgKOH / g) of the anionic urethane resin (X) is calculated based on the amount of the potassium hydroxide aqueous solution used in the titration and the following calculation formula (1).

[0112] In the calculation formula A = (B × f × 5.611) / S (1), A is the solid acid value of the resin (mgKOH / g), B is the amount of 0.1 mol / L potassium hydroxide aqueous solution used for titration (mL), f is the factor of 0.1 mol / L potassium hydroxide aqueous solution, S is the mass of the resin particles (g), and 5.611 is the formula weight of potassium hydroxide (56.11 / 10).

[0113] [Evaluation method of prepared liquid stability]

[0114] The urethane resin compositions obtained in the examples and comparative examples were diluted with water to a solid content of 20% by mass, and 1 part by mass of sodium chloride was added to 100 parts by mass of the prepared solution to obtain a prepared solution. The prepared solution was allowed to stand at 40° C. for 1 week and evaluated as follows.

[0115] “A”: No change in appearance.

[0116] "B": A slight amount of precipitate was observed.

[0117] "C": A large amount of precipitate was confirmed.

[0118] [Method for producing impregnated nonwoven fabric]

[0119] The urethane resin compositions obtained in the examples and comparative examples were diluted with water so that the solid content was 20% by mass, and 1 part by mass of sodium chloride was added to 100 parts by mass of the prepared solution to obtain a prepared solution. The prepared solution was impregnated into a polyester fiber containing 200 g / m 2 The nonwoven fabric was squeezed by a roller so that the pickup rate (pickup) was 100%. Then, it was left to stand in saturated steam at 100°C for 2 minutes and dried in a dryer at 100°C for 20 minutes to prepare an impregnated nonwoven fabric (leather sheet).

[0120] [Evaluation method of oleic acid resistance]

[0121] The obtained impregnated nonwoven fabric was immersed in oleic acid and allowed to stand overnight at 80° C., and was visually evaluated as follows.

[0122] “A”: No change in appearance.

[0123] "B": Slight swelling occurs.

[0124] "C": A large swelling occurs.

[0125] [Evaluation method of hand feel]

[0126] The obtained impregnated nonwoven fabric was evaluated by touch as follows.

[0127] "A": Soft and supple.

[0128] "B": has a little softness.

[0129] "C": Poor softness.

[0130] [Evaluation method of light resistance]

[0131] The obtained impregnated nonwoven fabric was irradiated with 110 MJ of light under the conditions of 89° C. and 50% humidity using a xenon fade meter, and evaluated visually as follows.

[0132] “A”: No change in appearance.

[0133] "B": Slight yellowing occurs.

[0134] "C": intense yellowing occurs.

[0135] [Table 1]

[0136]

[0137] [Table 2]

[0138]

[0139] [Table 3]

[0140]

[0141] It was found that the prepared liquids of Examples 1 to 6, which are urethane resin compositions of the present invention, are excellent in stability, feel, light resistance, and oleic acid resistance.

[0142] On the other hand, Comparative Example 1 is a form in which a non-biomass polycarbonate polyol was used instead of the polycarbonate polyol (a1), and the texture and oleic acid resistance were poor.

[0143] Comparative Example 2 is a form using a urethane resin having no anionic group, and the stability of the prepared solution is poor.

[0144] Comparative Example 3 is a form using a urethane resin having no nonionic group, and the texture and the stability of the prepared solution are poor.

[0145] Comparative Example 5 is a form in which the nonionic emulsifier (B) is not used, and the texture and the stability of the prepared liquid are poor.

Claims

1. A urethane resin composition, characterized in that The invention comprises: a urethane resin (A) having an anionic group and a nonionic group, a nonionic emulsifier (B) and water (C), wherein the urethane resin (A) is made of a polycarbonate polyol (a1) as a raw material, and the polycarbonate polyol (a1) is made of butanediol and decanediol derived from biomass as raw materials, The nonionic groups in the urethane resin (A) include oxyethylene groups and oxypropylene groups. The molar ratio [(C4) / (C10)] of the butanediol (C4) to the biomass-derived decanediol (C10) in the polycarbonate polyol (a1) is in the range of 70 / 30 to 95 / 5.

2. The urethane resin composition according to claim 1, wherein The oxyethylene group and the oxypropylene group are provided by a polyol having an oxyethylene group and an oxypropylene group.

3. The urethane resin composition according to claim 1 or 2, wherein The nonionic emulsifier (B) has an oxyethylene group and an oxypropylene group.