A method for preparing hydrogel, a method for preparing hydrogel and a gas diffusion layer

By using hydrogel and metal ions to coordinate to form a metal frame in a fuel cell, the problem of low mechanical strength of the gas diffusion layer is solved, mechanical performance improvement and self-repair capability are achieved, and the overall performance of the fuel cell is improved.

CN114736395BActive Publication Date: 2024-11-12DONGFENG MOTOR GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210329543.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-31
Publication Date
2024-11-12
Estimated Expiration
2042-03-31

AI Technical Summary

Technical Problem

The gas diffusion layer in existing fuel cells has low mechanical strength and is prone to damage due to external forces, resulting in unstable membrane electrode structure and affecting fuel cell performance.

Method used

A hydrogel preparation method is adopted to process lebronine and methanol, sodium bicarbonate and other compounds through a series of treatments to form a hydrogel with excellent mechanical properties, and coat it on the surface of the gas diffusion layer to combine metal ions. Coordinate to form a metal frame, enhance mechanical properties and achieve self-healing.

Benefits of technology

It effectively improves the mechanical strength and conductivity of the gas diffusion layer, reduces the possibility of damage due to external forces, and gives self-repair ability, improving the overall performance of the fuel cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114736395B_ABST
    Figure CN114736395B_ABST
Patent Text Reader

Abstract

The present invention particularly relates to a method for preparing a hydrogel, a method for preparing a hydrogel and a gas diffusion layer, and belongs to the field of fuel cell technology. A method for preparing a hydrogel, which can prepare a hydrogel with excellent mechanical properties, and the hydrogel is coated on the surface of the gas diffusion layer, which can effectively improve the mechanical strength of the gas diffusion layer and reduce the possibility of damage to the gas diffusion layer due to external factors; and the hydrogel can coordinate with metal ions to form a metal skeleton inside, further improving the mechanical properties while effectively enhancing the conductivity of the gas diffusion layer; and after the hydrogel coordinates with the metal, the metal center maintains a connection with the ligand through a coordination bond, so that the three-dimensional network of the hydrogel can be reversibly dissociated and reorganized, achieving self-healing, so that the gas diffusion layer has self-repairing ability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fuel cells, and in particular relates to a method for preparing a hydrogel, and a method for preparing a hydrogel and a gas diffusion layer. Background Art

[0002] A fuel cell is a chemical device that converts the chemical energy of a fuel directly into electrical energy, also known as an electrochemical generator. It is the fourth power generation technology after hydroelectric power generation, thermal power generation, and atomic power generation. Since fuel cells convert part of the Gibbs free energy in the chemical energy of a fuel into electrical energy through electrochemical reactions, they are not limited by the Carnot cycle effect and therefore have high efficiency. In addition, fuel cells use fuel and oxygen as raw materials and have no mechanical transmission parts, so they emit very little harmful gas and have a long service life. It can be seen that from the perspective of energy conservation and ecological protection, fuel cells are the most promising power generation technology.

[0003] The main membrane electrode of the fuel cell is composed of a catalyst layer and a gas diffusion layer. The diffusion layer can be divided into a substrate layer and a microporous layer. The substrate layer is in direct contact with the catalyst layer, supporting the microporous layer and the catalyst layer, collecting current, conducting gas and discharging water. The main materials used are carbon paper and carbon cloth.

[0004] Currently, during the stacking process, the gas diffusion layer may be damaged due to compression and other factors, resulting in reduced mechanical strength and unstable membrane electrode structure, which may lead to a decrease in the overall performance of the fuel cell. Summary of the invention

[0005] The purpose of the present application is to provide a method for preparing a hydrogel to solve the technical problem of low mechanical strength of a gas diffusion layer in the prior art.

[0006] The present invention provides a method for preparing a hydrogel, comprising the following steps:

[0007] Dissolving asparagine in methanol, adding concentrated sulfuric acid, stirring and cooling to room temperature to obtain a first mixed solution;

[0008] titrating the first mixed solution with a sodium bicarbonate solution to a pH value of 7-8.5 to obtain a treated solution;

[0009] The treated liquid is concentrated under reduced pressure and extracted with ethyl acetate to obtain a first organic phase;

[0010] The first organic phase is dried and filtered to obtain a first compound;

[0011] adding the first compound, allyl bromide and potassium carbonate into anhydrous acetone and stirring to obtain a second mixed solution;

[0012] The second mixed solution is refluxed in an inert atmosphere, cooled and filtered to obtain a second organic phase;

[0013] The second organic phase is dried and concentrated for a second time to obtain a second compound;

[0014] The second compound is dissolved in tetrahydrofuran, and then a sodium hydroxide solution is added, and the mixture is stirred at a first temperature for a first time and then filtered to obtain SPD;

[0015] Dissolving acrylamide in deionized water, adding the SPD, ethanol and potassium persulfate to obtain a third mixed solution;

[0016] The third mixed liquid is degassed with an inert gas, and then 1,3,5-benzenetricarboxylic acid is added to carry out a polymerization reaction to obtain the hydrogel.

[0017] Optionally, the mass ratio of asparagine to concentrated sulfuric acid is 5:3.

[0018] Optionally, the first drying and the second drying are both performed using anhydrous sodium sulfate.

[0019] Optionally, the mass ratio of the first compound, allyl bromide and potassium carbonate is 3:5:12.

[0020] Optionally, the reflux heating temperature is 20-25° C., and the reflux heating time is 24 h.

[0021] Optionally, the first temperature is 50° C. and the first time is 4 hours.

[0022] Based on the same inventive concept, an embodiment of the present invention further provides a hydrogel prepared by any one of the above-mentioned preparation methods.

[0023] Based on the same inventive concept, an embodiment of the present invention further provides a method for preparing a gas diffusion layer, comprising the following steps:

[0024] Get the basal layer;

[0025] The hydrogel is coated on the surface of the base layer, and dried at a second temperature for a second time to obtain a prefabricated layer;

[0026] Mixing ethylene glycol, conductive carbon black, a hydrophobic agent and a dispersant to obtain a microporous layer slurry;

[0027] The microporous layer slurry is coated on the surface of the prefabricated layer and then baked to obtain the gas diffusion layer.

[0028] Optionally, the hydrogel loading on the surface of the substrate is 0.1-0.5 μg / cm 2 .

[0029] Optionally, the mass ratio of the conductive carbon black to the dispersant is 1:(10-30); the mass ratio of the conductive carbon black to ethylene glycol is (4-20):1.

[0030] Optionally, the mass ratio of the conductive carbon black to the water repellent is (3-10):1.

[0031] Optionally, the second temperature is 80° C., and the second time is 2 hours.

[0032] Optionally, in the microporous layer slurry, the mass percentage of the water repellent is 15-30%.

[0033] Optionally, the conductive carbon black includes any one or more combinations of acetylene black, Vulcan XC-72, Black pearls, and carbon nanotubes.

[0034] Optionally, the calcination temperature is 200-300° C., and the calcination time is 3 hours.

[0035] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0036] The preparation method of the hydrogel provided by the embodiment of the present invention can prepare a hydrogel with excellent mechanical properties. The hydrogel is coated on the surface of the gas diffusion layer, which can effectively improve the mechanical strength of the gas diffusion layer and reduce the possibility of damage to the gas diffusion layer due to external factors; moreover, the hydrogel can coordinate with metal ions to form a metal skeleton inside, further improving the mechanical properties while effectively enhancing the electrical conductivity of the gas diffusion layer; moreover, after the hydrogel is coordinated with the metal, the metal center maintains the connection with the ligand through the coordination bond, so that the three-dimensional network of the hydrogel can be reversibly dissociated and reorganized to achieve self-healing, thereby making the gas diffusion layer have self-repairing ability.

[0037] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0039] Figure 1is a flow chart of a method provided by an embodiment of the present invention;

[0040] Figure 2 is an enlarged view of the carbon paper in the initial state in the embodiment of the present invention;

[0041] Figure 3 It is an enlarged view of the carbon paper after standing for 1 hour in the embodiment of the present invention. DETAILED DESCRIPTION

[0042] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.

[0043] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. If there is a conflict, the present specification takes precedence. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. For example, room temperature can refer to a temperature within the range of 10 to 35°C.

[0044] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0045] The technical solution of the embodiment of the present application is to solve the above technical problems, and the overall idea is as follows:

[0046] According to a typical embodiment of the present invention, a method for preparing a hydrogel is provided, comprising the following steps:

[0047] S1. Dissolve asparagine in methanol, add concentrated sulfuric acid, stir and cool to room temperature to obtain a first mixed solution.

[0048] Wherein: the mass ratio of the asparagine to concentrated sulfuric acid is 5:3.

[0049] The reason for controlling the mass ratio of asparagine to concentrated sulfuric acid is that if the ratio is too high, asparagine in the solution cannot be well dissolved in the solution, and if the ratio is too low, the amount of asparagine in the solution is insufficient, which affects the subsequent reaction.

[0050] S2. Titrate the first mixed solution with sodium bicarbonate solution to a pH value of 7-8.5 to obtain a treated solution.

[0051] The reason for controlling the pH value to be 7-8.5 is that if the pH is too low, the acidic environment is not conducive to the formation of the first organic phase.

[0052] S3, concentrating the treated liquid under reduced pressure and extracting with ethyl acetate to obtain a first organic phase.

[0053] S4. Drying and filtering the first organic phase to obtain a first compound.

[0054] Wherein: the first drying is carried out using anhydrous sodium sulfate.

[0055] The reason for using anhydrous sodium sulfate for drying is that anhydrous sodium sulfate can remove moisture from organic liquids.

[0056] S5. Add the first compound, allyl bromide and potassium carbonate into anhydrous acetone and stir to obtain a second mixed solution.

[0057] Wherein: the mass ratio of the first compound, allyl bromide and potassium carbonate is 3:5:12.

[0058] S6. Reflux-heat the second mixed solution in an inert atmosphere, cool it, and filter it to obtain a second organic phase.

[0059] Wherein: the reflux heating temperature is 20-25°C, and the reflux heating time is 24h.

[0060] S7. Drying and concentrating the second organic phase for a second time to obtain a second compound.

[0061] Wherein: the second drying is carried out using anhydrous sodium sulfate.

[0062] S8, dissolving the second compound in tetrahydrofuran, then adding sodium hydroxide solution, stirring at a first temperature for a first time, and then filtering to obtain SPD.

[0063] Wherein: the first temperature is 50° C., and the first time is 4 hours.

[0064] S9, dissolving acrylamide in deionized water, adding the SPD, ethanol and potassium persulfate to obtain a third mixed solution.

[0065] S10, degassing the third mixed solution with an inert gas, and then adding 1,3,5-benzenetricarboxylic acid to carry out a polymerization reaction to obtain the hydrogel.

[0066] According to another typical embodiment of the present invention, a hydrogel is provided, which is prepared by any one of the above preparation methods.

[0067] According to another typical embodiment of the present invention, a method for preparing a gas diffusion layer is provided, comprising the following steps:

[0068] S11. Obtaining a basal layer.

[0069] S12, coating the hydrogel on the surface of the base layer, and drying at a second temperature for a second time to obtain a prefabricated layer.

[0070] in:

[0071] The hydrogel loading on the surface of the basal layer is 0.1-0.5 μg / cm 2 .

[0072] The reason for controlling the hydrogel loading is that if the hydrogel loading is too high, the strength of the gas diffusion layer will be too high, which is not conducive to stacking and multiple compression; if the hydrogel loading is too low, the strength will be insufficient and the conductivity will not be high.

[0073] The second temperature is 80° C., and the second time is 2 hours.

[0074] S13, mixing ethylene glycol, conductive carbon black, a hydrophobic agent and a dispersant to obtain a microporous layer slurry.

[0075] in:

[0076] In the microporous layer slurry, the mass percentage of the hydrophobic agent is 15-30%, the mass ratio of the conductive carbon black to the hydrophobic agent is (3-10):1; the mass ratio of the conductive carbon black to the dispersant is 1:(10-30); the mass ratio of the conductive carbon black to ethylene glycol is (4-20):1.

[0077] The reasons for controlling the above ratios are: if the ratio is too high, the conductivity of the gas diffusion layer will deteriorate, and if the ratio is too low, the gas diffusion layer will not be sufficiently hydrophobic.

[0078] The conductive carbon black includes any one or more combinations of acetylene black, Vulcan XC-72, Black pearls, and carbon nanotubes.

[0079] S14, coating the microporous layer slurry on the surface of the prefabricated layer and then baking to obtain the gas diffusion layer.

[0080] in:

[0081] The calcination temperature is 200-300° C., and the calcination time is 3 hours.

[0082] The mechanism of the preparation method of a gas diffusion layer provided in this embodiment is: first, the base layer is modified, and the prepared hydrogel is coated on the base layer to enhance the structure of the base layer and improve the conductivity, and then a slurry is prepared and coated on the base layer to finally obtain the gas diffusion layer.

[0083] The present application will be described in detail below with reference to embodiments, comparative examples and experimental data.

[0084] Example 1

[0085] This embodiment provides a method for preparing a hydrogel, comprising the following steps:

[0086] S1. Dissolve 3.2 g, 22 mmol, of asparagine in 50 mL of methanol, add 2 mL of concentrated sulfuric acid, stir and cool to room temperature to obtain a first mixed solution.

[0087] S2. Titrate the first mixed solution with sodium bicarbonate solution to a pH value of 7-8.5 to obtain a treated solution.

[0088] S3, concentrating the treated liquid under reduced pressure and extracting with ethyl acetate to obtain a first organic phase.

[0089] S4. Drying and filtering the first organic phase to obtain a first compound.

[0090] Wherein: the first drying is carried out using anhydrous sodium sulfate.

[0091] S5. Add 1.3 g, 5.8 mmol, of the first compound, 3.5 g, 25.2 mmol, of allyl bromide, and 15 g, 90.2 mmol, of potassium carbonate into 100 mL of anhydrous acetone and stir to obtain a second mixed solution.

[0092] S6. Reflux-heat the second mixed solution in an inert atmosphere, cool it, and filter it to obtain a second organic phase.

[0093] Wherein: the reflux heating temperature is 20°C, and the reflux heating time is 24h.

[0094] S7. Drying and concentrating the second organic phase for a second time to obtain a second compound.

[0095] Wherein: the second drying is carried out using anhydrous sodium sulfate.

[0096] S8. Dissolve 1.2 g, 5.7 mmol, of the second compound in 20 ml of tetrahydrofuran, then add 10 ml of sodium hydroxide solution (1.3 g, 50 mmol), stir at a first temperature for a first time, and then filter to obtain SPD.

[0097] Wherein: the first temperature is 50° C., and the first time is 4 hours.

[0098] S9. Dissolve 2 g of acrylamide in 20 ml of deionized water, add 1 g of the SPD, 2 ml of ethanol and 2 g of potassium persulfate to obtain a third mixed solution.

[0099] S10, degassing the third mixed solution with an inert gas, and then adding 5 ml of 1,3,5-benzenetricarboxylic acid, and performing a polymerization reaction at room temperature for 2 hours to obtain the hydrogel.

[0100] This embodiment also provides a hydrogel prepared by the above method.

[0101] This embodiment also provides a method for preparing a gas diffusion layer, comprising the following steps:

[0102] S11. Obtaining a basal layer.

[0103] S11.1. Immerse the base layer in a PTFE solution with a mass fraction of 15%. After immersion for 30 minutes, put it into an oven and dry it at 60°C for 1 hour. Repeat this step to make the PETF content in the base layer 5.5%.

[0104] S12, coating the hydrogel on the surface of the base layer, and drying at a second temperature for a second time to obtain a prefabricated layer.

[0105] in:

[0106] The hydrogel loading on the surface of the basal layer is 0.1 μg / cm 2 .

[0107] The second temperature is 80° C., and the second time is 2 hours.

[0108] S13. Mix 2.2 g of ethylene glycol, 25 g of conductive carbon black, 8.2 g of a water repellent and 50 ml of a dispersant to obtain a microporous layer slurry.

[0109] in:

[0110] The conductive carbon black is Vulcan XC-72.

[0111] S14, coating the microporous layer slurry on the surface of the prefabricated layer and then calcining to obtain the gas diffusion layer.

[0112] Wherein: the calcination temperature is 280° C., and the calcination time is 3 h.

[0113] Example 2

[0114] The difference between this embodiment and embodiment 1 is only that:

[0115] In step S12: the hydrogel loading on the surface of the basal layer is 0.3 μg / cm 2 .

[0116] Example 3

[0117] The difference between this embodiment and embodiment 1 is only that:

[0118] In step S12: the hydrogel loading on the surface of the basal layer is 0.6 μg / cm 2 .

[0119] Comparative Example 1

[0120] The only difference between this comparative example and Example 3 is that step S12 is not included.

[0121] Experimental example

[0122] The mechanical strength, electrical conductivity and gas permeability of the gas diffusion layers provided in Example 1-N and Comparative Example 1-N were tested respectively. The test results are shown in the following table:

[0123]

[0124] It can be seen from the above table that the various properties of the gas diffusion layers provided by Examples 1-3 of the present invention are significantly better than those of the catalyst layer membrane electrode of Comparative Example 1.

[0125] Explanation of the attached figure:

[0126] Depend on Figure 2 and Figure 3 It can be seen that Figure 2 is the carbon paper in the initial state in the embodiment, Figure 3 This is the carbon paper after standing for 1 hour in the embodiment. After standing for 1 hour, the scratch width is reduced by 9.2%, indicating that it has a certain self-repairing ability.

[0127] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.

[0128] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0129] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a gas diffusion layer, characterized in that: The steps include: Get the basal layer; The hydrogel is coated on the surface of the base layer and dried at 80° C. for 2 h to obtain a prefabricated layer; Mixing ethylene glycol, conductive carbon black, a hydrophobic agent and a dispersant to obtain a microporous layer slurry; The microporous layer slurry is coated on the surface of the prefabricated layer and then baked to obtain the gas diffusion layer; The hydrogel loading on the surface of the basal layer is 0.1-0.5 μg / cm 2 ; The mass ratio of the conductive carbon black to the dispersant is 1:(10-30); the mass ratio of the conductive carbon black to ethylene glycol is (4-20):1; The mass ratio of the conductive carbon black to the hydrophobic agent is (3-10):1; In the microporous layer slurry, the mass percentage of the water repellent is 15-30%; The preparation method of the hydrogel comprises the following steps: Dissolving asparagine in methanol, adding concentrated sulfuric acid, stirring and cooling to room temperature to obtain a first mixed solution; titrating the first mixed solution with a sodium bicarbonate solution to a pH value of 7-8.5 to obtain a treated solution; The treated liquid is concentrated under reduced pressure and extracted with ethyl acetate to obtain a first organic phase; The first organic phase is dried and filtered to obtain a first compound; adding the first compound, allyl bromide and potassium carbonate into anhydrous acetone and stirring to obtain a second mixed solution; The second mixed solution is refluxed in an inert atmosphere, cooled and filtered to obtain a second organic phase; The second organic phase is dried and concentrated for a second time to obtain a second compound; The second compound is dissolved in tetrahydrofuran, and then a sodium hydroxide solution is added, and the mixture is stirred at a first temperature for a first time and then filtered to obtain SPD; Dissolving acrylamide in deionized water, adding the SPD, ethanol and potassium persulfate to obtain a third mixed solution; The third mixed solution is degassed with an inert gas, and then 1,3,5-benzenetricarboxylic acid is added to carry out a polymerization reaction to obtain the hydrogel. The mass ratio of asparagine to concentrated sulfuric acid is 5:3, the mass ratio of the first compound, allyl bromide and potassium carbonate is 3:5:12, the reflux heating temperature is 20-25°C, the reflux heating time is 24h, the first temperature is 50°C, and the first time is 4h.

2. The preparation method according to claim 1, characterized in that: The conductive carbon black includes any one or more combinations of acetylene black, Vulcan XC-72, Black pearls, and carbon nanotubes.

3. The preparation method according to claim 1, characterized in that: The calcination temperature is 200-300° C., and the calcination time is 3 hours.