Sebacic acid-blocked copolycarbonate and its preparation method and application
By introducing sebacic acid blocks into the polycarbonate backbone to form block copolymers, the problem of insufficient flow toughness of polycarbonate is solved, the mechanical properties and melt index are significantly improved, the application scope is expanded, and simple is achieved Easy-to-control preparation process.
Patent Information
- Application Number
- CN202210344925.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-03-31
AI Technical Summary
The lack of flow toughness of existing polycarbonates limits their widespread use in certain application areas.
Sebacic acid blocks are introduced into the backbone of the polycarbonate, and block copolymers are formed through specific structural units and capping structures, and specific preparation methods are adopted, including bisphenol A, alkali metal hydroxide, water, The reaction of the catalyst and triclosan blocking agent followed by polymerization with phosgene and eugenol blocked polysebaic acid, control reaction conditions and purification treatment to obtain copolycarbonate with excellent mechanical properties.
The flow toughness and elongation of break of copolycarbonate are significantly improved, and the melting index reaches 30-50g/10min, which expands its application range, and the preparation method is simple and easy to control, suitable for large-scale production.
Smart Images

Figure CN114752052B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, in particular to a sebacic acid-block copolycarbonate and a preparation method and application thereof. Background Art
[0002] Polycarbonate resins are mainly prepared by the polycondensation reaction of aromatic diols such as bisphenol A and carbonate precursors such as phosgene. Polycarbonate has excellent impact strength, dimensional stability, heat resistance and transparency, making it widely used in applications such as exterior materials for electronic and electrical products, automotive parts, building materials and optical elements.
[0003] In order to further expand the application field of polycarbonate resin, the existing technology is to introduce different structural units into the main chain of polycarbonate by using aromatic diol copolymers with different structures to obtain polycarbonate with corresponding properties. However, there are few reports on the improvement of polycarbonate flow toughness.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The object of the present invention is to provide a sebacic acid block copolycarbonate to solve the technical problems of insufficient flow toughness of polycarbonate in the prior art.
[0006] Another object of the present invention is to provide a method for preparing the sebacic acid-blocked copolycarbonate.
[0007] Another object of the present invention is to provide the use of the sebacic acid-blocked copolycarbonate in the preparation of corresponding compositions.
[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0009] A sebacic acid-block copolycarbonate comprising a block copolymer formed by a structural unit (A) and a structural unit (B), and the end-capping structure is a structure (C);
[0010] The structures of structural unit (A), structural unit (B) and structural unit (C) are as follows:
[0011]
[0012] In a specific embodiment of the present invention, m is an integer between 90 and 200; n is an integer between 10 and 70.
[0013] In a specific embodiment of the present invention, m is an integer between 150 and 200; n is an integer between 50 and 60.
[0014] In a specific embodiment of the present invention, in the copolycarbonate, the weight percentage of the structural unit B is 5% to 20%.
[0015] In a specific embodiment of the present invention, in the copolycarbonate, the weight percentage of the structural unit A is 80% to 90%.
[0016] In a specific embodiment of the present invention, the weight average molecular weight of the copolycarbonate is 30,000 to 60,000, and the polydispersity index is 1.1 to 2.4.
[0017] In a specific embodiment of the present invention, the copolycarbonate has an Izod notched impact strength of 850 to 900 J / m at room temperature and pressure. 2 The measured value is based on the standard test method for Izod impact properties of plastics in ASTM D256-1997.
[0018] In a specific embodiment of the present invention, the elongation at break of the copolycarbonate at room temperature and pressure is 100% to 150%, which is measured according to the plastic tensile property test method specified in ASTM D638-2003.
[0019] In a specific embodiment of the present invention, the melt index of the copolycarbonate is 30-50 g / 10 min, and the test conditions are 260° C. / 1.2 kg.
[0020] The present invention also provides a method for preparing a sebacic acid-blocked copolycarbonate, comprising the following steps:
[0021] (A) combining bisphenol A, alkali metal hydroxide, water, a catalyst and a triclosan blocking agent to obtain an aqueous phase;
[0022] (B) mixing phosgene with an inert organic solvent to obtain an oil phase;
[0023] (C) adding the oil phase and the eugenol-terminated polysebacic acid to the aqueous phase for polymerization reaction, adding an alkali metal hydroxide aqueous solution until the pH of the reaction system is 10.5 to 11.5, reacting at 45 to 50° C. for 2 to 4 hours, to obtain an emulsion of a sebacic acid-blocked copolycarbonate;
[0024] (D) Purifying the emulsion of the sebacic acid-block copolycarbonate and removing the organic solvent to obtain the sebacic acid-block copolycarbonate.
[0025] In a specific embodiment of the present invention, in step (A), the molar ratio of the bisphenol A, the alkali metal hydroxide and the water is 1: (2.5-4.0): (80-140).
[0026] In a specific embodiment of the present invention, the catalyst includes one or more of tetrabutylammonium bromide, triethylamine and tetrabutylammonium chloride.
[0027] In a specific embodiment of the present invention, in step (B), the molar ratio of the phosgene to the bisphenol A is (1.3-1.5):1.
[0028] In a specific embodiment of the present invention, in step (B), the mass ratio of the phosgene to the inert organic solvent is 1:(45-65).
[0029] In a specific embodiment of the present invention, in step (C), the mass ratio of the eugenol-capped polysebacic acid to the bisphenol A is 1:(4-9).
[0030] The present invention also provides the use of any one of the above-mentioned sebacic acid-blocked copolycarbonates in the preparation of a resin composition.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) The present invention introduces a certain amount of sebacic acid into the main chain of polycarbonate, so that the obtained copolycarbonate has excellent mechanical properties, especially ultra-high flow toughness, and the elongation at break is significantly improved compared with ordinary polycarbonate, and the melt index can reach 30 to 50 g / 10 min, thereby expanding its application range;
[0033] (2) The method for preparing the copolycarbonate of the present invention is simple and easy to control, can be produced on a large scale and has a high product yield. DETAILED DESCRIPTION
[0034] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0035] A sebacic acid-block copolycarbonate comprising a block copolymer formed by a structural unit (A) and a structural unit (B), and the end-capping structure is a structure (C);
[0036] The structures of structural unit (A), structural unit (B) and structural unit (C) are as follows:
[0037]
[0038] In a specific embodiment of the present invention, m is an integer between 90 and 200; n is an integer between 10 and 70; preferably, m is an integer between 150 and 200; n is an integer between 50 and 60.
[0039] For example, in different embodiments, m may be 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, etc.; n may be 10, 20, 30, 40, 50, 60, 70, etc.
[0040] In a specific embodiment of the present invention, in the copolycarbonate, the weight percentage of the structural unit B is 5% to 20%; preferably, the weight percentage of the structural unit B is 10% to 20%.
[0041] In a specific embodiment of the present invention, in the copolycarbonate, the weight percentage of the structural unit A is 80% to 90%.
[0042] For example, in different embodiments, in the copolycarbonate, the weight percentage of the structural unit B can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20% and the like; the weight percentage of the structural unit A can be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90% and the like.
[0043] In a specific embodiment of the present invention, the weight average molecular weight of the copolycarbonate is 30,000 to 60,000, and the polydispersity index is 1.1 to 2.4.
[0044] For example, in different embodiments, the weight average molecular weight of the copolycarbonate can be 30,000, 35,000, 40,000, 45,000, 50,000, 55,000, 60,000, and the like; the polydispersity index can be 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, and the like.
[0045] In a specific embodiment of the present invention, the copolycarbonate has an Izod notched impact strength of 850 to 900 J / m at room temperature and pressure. 2 The measured value is based on the standard test method for Izod impact properties of plastics in ASTM D256-1997.
[0046] In a specific embodiment of the present invention, the elongation at break of the copolycarbonate at room temperature and pressure is 100% to 150%, which is measured according to the plastic tensile property test method specified in ASTM D638-2003.
[0047] In a specific embodiment of the present invention, the melt index of the copolycarbonate is 30-50 g / 10 min, and the test conditions are 260° C. / 1.2 kg.
[0048] The present invention also provides a method for preparing a sebacic acid-blocked copolycarbonate, comprising the following steps:
[0049] (A) combining bisphenol A, alkali metal hydroxide, water, a catalyst and a triclosan blocking agent to obtain an aqueous phase;
[0050] (B) mixing phosgene with an inert organic solvent to obtain an oil phase;
[0051] (C) adding the oil phase and the eugenol-terminated polysebacic acid to the aqueous phase for polymerization reaction, adding an alkali metal hydroxide aqueous solution until the pH of the reaction system is 10.5 to 11.5, reacting at 45 to 50° C. for 2 to 4 hours, to obtain an emulsion of a sebacic acid-blocked copolycarbonate;
[0052] (D) Purifying the emulsion of the sebacic acid-block copolycarbonate and removing the organic solvent to obtain the sebacic acid-block copolycarbonate.
[0053] In a specific embodiment of the present invention, in step (A), the molar ratio of the bisphenol A, the alkali metal hydroxide and the water is 1: (2.5-4.0): (80-140).
[0054] In a specific embodiment of the present invention, in step (A), the catalyst includes one or more of tetrabutylammonium bromide, triethylamine and tetrabutylammonium chloride.
[0055] In a specific embodiment of the present invention, in step (A), the molar ratio of the catalyst to the bisphenol A is 0.001-0.0015:1.
[0056] In a specific embodiment of the present invention, in step (A), the mass percentage of triclosan in the aqueous phase is 0.1% to 0.3%.
[0057] In a specific embodiment of the present invention, in step (B), the molar ratio of the phosgene to the bisphenol A is (1.3-1.5):1.
[0058] In a specific embodiment of the present invention, in step (B), the mass ratio of the phosgene to the inert organic solvent is 1:(45-65).
[0059] In a specific embodiment of the present invention, in step (B), the inert organic solvent includes one or more of aromatics, aromatic hydrocarbons and aliphatic chlorinated hydrocarbons; preferably, the inert organic solvent includes one or more of dichloromethane, dichloroethane, trichloroethylene, 1,1,1-trichloroethane, 1,1,2-trichloroethane, carbon tetrachloride, benzene, toluene, p-xylene, m-xylene, o-xylene and chlorobenzene.
[0060] In a specific embodiment of the present invention, in step (C), the dropping rate of the oil phase is 100-200 g / min.
[0061] In a specific embodiment of the present invention, in step (C), the dripping rate of the eugenol-capped polysebacic acid is 150-200 g / min.
[0062] In a specific embodiment of the present invention, in step (C), the weight average molecular weight of the eugenol-capped polysebacic acid is 3500-4200, and the polydispersity index is less than 3.5.
[0063] In a specific embodiment of the present invention, in step (C), the method for preparing eugenol-capped polysebacic acid comprises the following steps:
[0064] Sebacic acid and clay catalyst Filtrol 20 are mixed, stirred at 45-55° C. for 2-3 hours, then heated to 100-120° C. for reaction for 5-7 hours to obtain a reaction solution, the reaction solution is filtered to remove the clay catalyst, eugenol and karstedt platinum catalyst are added, and the mixture is reacted at 75-85° C. for 12-15 hours to obtain eugenol-terminated polysebacic acid.
[0065] In a specific embodiment of the present invention, the mass ratio of the sebacic acid to the eugenol is 1:0.1-0.3.
[0066] In a specific embodiment of the present invention, the mass ratio of the sebacic acid to the clay catalyst Filtrol 20 is 1:0.01-0.02.
[0067] In a specific embodiment of the present invention, in step (D), the purification treatment includes centrifuging the emulsion of the sebacic acid-blocked copolycarbonate; multiple centrifugations can remove impurities in the emulsion.
[0068] The present invention also provides the use of any one of the above-mentioned sebacic acid-blocked copolycarbonates in the preparation of a resin composition.
[0069] Example 1
[0070] The preparation method of the sebacic acid-blocked copolycarbonate provided in this embodiment comprises the following steps:
[0071] (A) adding 230 kg of bisphenol A, 105 kg of NaOH and 1610 kg of water into a mixer and mixing, after the bisphenol A is completely dissolved, adding 325 g of tetrabutylammonium bromide and 2.5 kg of triclosan capping agent to obtain an aqueous phase;
[0072] (B) adding 130 kg of liquid phosgene and 4855 L of dichloromethane into another mixer to obtain an oil phase;
[0073] (C) placing the aqueous phase in step (A) into a polymerization reactor, adding the oil phase and 26.5 kg of eugenol-terminated polysebacic acid at a stirring rate of 800 rpm at a rate of 100 g / min and 150 g / min, respectively, into the polymerization reactor, and simultaneously adding a 10 wt % sodium hydroxide aqueous solution into the reaction system to keep the pH value of the reaction system at 10.5, and maintaining the temperature of the reaction system at 45° C.; after reacting for 2.5 hours, an emulsion of a copolycarbonate blocked with sebacic acid was obtained;
[0074] (D) The emulsion of the sebacic acid-blocked copolycarbonate is centrifuged and dichloromethane is removed to obtain the sebacic acid-blocked copolycarbonate.
[0075] The preparation method of eugenol-terminated polysebacic acid in this embodiment comprises the following steps:
[0076] Sebacic acid (146 kg) and clay catalyst Filtrol 20 (2.5 kg) were added to a reactor equipped with a stirrer and a thermometer and stirred for 30 min to make the material mixture uniform, then the reaction system was heated to 50 ° C at a rate of 2 ° C / min and stirred at this temperature for 2.5 h, then the temperature of the reaction system was further heated to 110 ° C at a rate of 5 ° C / min and stirred vigorously at this temperature for 6 h, and then filtered to remove the clay catalyst. Then the material after removing the clay catalyst was placed in a reactor equipped with a stirrer and a thermometer and a mixed solution of eugenol (29 kg) and karstedt platinum catalyst (70 g) was added dropwise at a rate of 25 g / min under stirring, and then stirred at a temperature of 80 ° C for 13 h. Subsequently, the unreacted raw materials were distilled off at 200 ° C under reduced pressure to 0.2 kPa to obtain eugenol-terminated polysiloxane with a yield of 99%. The product was analyzed by GPC, and its weight average molecular weight was 3905 and the polydispersity index was 2.8.
[0077] Example 2
[0078] The preparation method of the sebacic acid-blocked copolycarbonate provided in this embodiment comprises the following steps:
[0079] (A) adding 230 kg of bisphenol A, 130 kg of NaOH and 1900 kg of water into a mixer and mixing, and after the bisphenol A is completely dissolved, adding 370 kg of tetrabutylammonium bromide and 4.0 kg of triclosan blocking agent to obtain an aqueous phase;
[0080] (B) adding 130 kg of liquid phosgene and 5420 kg of dichloromethane into another mixer to obtain an oil phase;
[0081] (C) placing the aqueous phase in step (A) into a polymerization reactor, adding the oil phase and 40 kg of eugenol-terminated polysebacic acid at a stirring rate of 800 rpm at a rate of 120 g / min and 170 g / min, respectively, into the polymerization reactor, and simultaneously adding a 10 wt % sodium hydroxide aqueous solution into the reaction system to keep the pH value of the reaction system at 10.9, and maintaining the temperature of the reaction system at 47° C.; after reacting for 2.5 hours, an emulsion of a copolycarbonate blocked with sebacic acid was obtained;
[0082] (D) The emulsion of the sebacic acid-blocked copolycarbonate is centrifuged and dichloromethane is removed to obtain the sebacic acid-blocked copolycarbonate.
[0083] The preparation method of the eugenol-terminated polysebacic acid in this example is the same as that in Example 1.
[0084] Comparative Example 1
[0085] The preparation method of the sebacic acid-blocked copolycarbonate provided in this embodiment comprises the following steps:
[0086] (A) adding 230 kg of bisphenol A, 105 kg of NaOH and 1610 kg of water into a mixer and mixing, after the bisphenol A is completely dissolved, adding 325 g of tetrabutylammonium bromide and 2.5 kg of triclosan capping agent to obtain an aqueous phase;
[0087] (B) adding 130 kg of liquid phosgene and 4855 L of dichloromethane into another mixer to obtain an oil phase;
[0088] (C) placing the aqueous phase in step (A) into a polymerization reactor, adding the oil phase and 20 kg of eugenol-terminated polysebacic acid at a stirring rate of 800 rpm at a rate of 120 g / min and 170 g / min, respectively, into the polymerization reactor, and simultaneously adding a 10 wt % sodium hydroxide aqueous solution into the reaction system to keep the pH value of the reaction system at 11.6, and maintaining the temperature of the reaction system at 55° C.; after reacting for 2.5 hours, an emulsion of sebacic acid-blocked copolycarbonate was obtained;
[0089] (D) The emulsion of the sebacic acid-blocked copolycarbonate is centrifuged and dichloromethane is removed to obtain the sebacic acid-blocked copolycarbonate.
[0090] The preparation method of the eugenol-terminated polysebacic acid in this comparative example is the same as that in Example 1.
[0091] Experimental Example 1
[0092] In order to compare and illustrate the properties of the copolycarbonates with sebacic acid blocks prepared in different embodiments and comparative examples, the performance of the copolycarbonates with sebacic acid blocks prepared in various embodiments and comparative examples were tested. The test results are shown in Table 1.
[0093] Wherein, the product is analyzed by GPC to obtain the weight average molecular weight and polydispersity index of the product;
[0094] The test conditions of melt index MI are 260℃ / 1.2kg, refer to ISO 1133-1;
[0095] The test of elongation at break refers to ASTM D638-2003;
[0096] The test of Izod notched impact strength refers to ASTM D256-1997.
[0097] Table 1 Test results of copolycarbonates with different sebacic acid blocks
[0098] Test items Example 1 Example 2 Comparative Example 1 GPC weight average molecular weight 32304 31050 22560 Polydispersity Index 1.9 2.1 3.2 Melt index MI (g / 10min) 40 42 30 Elongation at break (%) 125 130 70 Izod notched impact strength (J / m) 860 880 550
[0099] From the above test results, it can be seen that the present invention introduces a certain amount of sebacic acid into the main chain of polycarbonate, so that the obtained copolycarbonate has excellent mechanical properties, especially ultra-high flow toughness, and the elongation at break is significantly improved compared with ordinary polycarbonate. The melt index can reach 30-50g / 10min, which expands its application range.
[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A sebacic acid-blocked copolycarbonate, characterized in that: A block copolymer comprising a structural unit (A) and a structural unit (B), wherein the end-capping structure is a structure (C); The structures of structural unit (A), structural unit (B) and structural unit (C) are as follows: The copolycarbonate has an Izod notched impact strength of 850 to 900 J / m at room temperature and pressure. 2 ; And / or, the elongation at break of the copolycarbonate at normal temperature and pressure is 100% to 150%; And / or, the melt index of the copolycarbonate is 30-50 g / 10 min, and the test conditions are 260° C. / 1.2 kg.
2. The sebacic acid-blocked copolycarbonate according to claim 1, characterized in that: m is an integer between 90 and 200; n is an integer between 10 and 70.
3. The sebacic acid-blocked copolycarbonate according to claim 1, characterized in that: m is an integer between 150 and 200; n is an integer between 50 and 60.
4. The sebacic acid-blocked copolycarbonate according to claim 1, characterized in that: In the copolycarbonate, the mass percentage of the structural unit B is 5% to 20%; And / or, the mass percentage of the structural unit A is 80% to 90%.
5. The sebacic acid-blocked copolycarbonate according to claim 1, characterized in that: The weight average molecular weight of the copolycarbonate is 30,000 to 60,000, and the polydispersity index is 1.1 to 2.
4.
6. The method for preparing the sebacic acid-blocked copolycarbonate according to any one of claims 1 to 5, characterized in that: The steps include: (A) combining bisphenol A, alkali metal hydroxide, water, a catalyst and a triclosan blocking agent to obtain an aqueous phase; (B) mixing phosgene with an inert organic solvent to obtain an oil phase; (C) adding the oil phase and the eugenol-terminated polysebacic acid to the aqueous phase for polymerization reaction, adding an alkali metal hydroxide aqueous solution until the pH of the reaction system is 10.5 to 11.5, reacting at 45 to 50° C. for 2 to 4 hours, to obtain an emulsion of a sebacic acid-blocked copolycarbonate; (D) Purifying the emulsion of the sebacic acid-block copolycarbonate and removing the organic solvent to obtain the sebacic acid-block copolycarbonate.
7. The method for preparing the sebacic acid-blocked copolycarbonate according to claim 6, characterized in that: In step (A), the molar ratio of the bisphenol A, the alkali metal hydroxide and the water is 1:(2.5-4.0):(80-140).
8. The method for preparing the sebacic acid-blocked copolycarbonate according to claim 6, characterized in that: In step (A), the catalyst includes one or more of tetrabutylammonium bromide, triethylamine and tetrabutylammonium chloride.
9. The method for preparing the sebacic acid-blocked copolycarbonate according to claim 6, characterized in that: In step (B), the molar ratio of the phosgene to the bisphenol A is (1.3-1.5):
1.
10. The method for preparing the sebacic acid-blocked copolycarbonate according to claim 6, characterized in that: In step (B), the mass ratio of the phosgene to the inert organic solvent is 1:(45-65).
11. The method for preparing the sebacic acid-blocked copolycarbonate according to claim 6, characterized in that: In step (C), the mass ratio of the eugenol-capped polysebacic acid to the bisphenol A is 1:(4-9).
12. Use of the sebacic acid-blocked copolycarbonate according to any one of claims 1 to 5 in the preparation of a resin composition.