Back silver paste for crystalline silicon solar cell and preparation method thereof
By using a combination of silver powder, organic binder, glass powder and organic additives in crystalline silicon solar cells, the problem of insufficient sintering density and silver aluminum contact caused by the reduction of silver content of back silver paste is solved, and high density is achieved It is formed with a silver layer with low resistance, which enhances the aging performance of the battery.
Patent Information
- Application Number
- CN202210252893.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-03-15
AI Technical Summary
The silver content of the silver back paste of existing crystalline silicon solar cells is reduced, resulting in insufficient sintering density, and defects are prone to occur at the contacts of silver aluminum, resulting in increased resistance of the cell and non-conductivity problems.
Using a combination of silver powder, organic binder, glass powder and organic additives, by controlling the mass ratio and viscosity of silver paste, use sheet, needle or plate silver powder to match with spherical silver powder, and through specific melting and ball milling The glass powder is prepared by process to form a back silver paste with good conductivity and denseness.
It effectively improves the density of the silver layer after sintering, reduces the contact resistance between silver electrode and silver aluminum, prevents aluminum thorns and cracks, and enhances anti-aging performance and adhesion.
Smart Images

Figure CN114758812B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a back silver paste for a crystalline silicon solar cell and a preparation method thereof, belonging to the technical field of conductive pastes. Background Art
[0002] Crystalline silicon solar cells are battery devices that use the photoelectric effect of semiconductor silicon to convert solar energy into electrical energy. The internal current generated under light conditions outputs electrical energy through the positive and back electrodes. In recent years, battery cells have been continuously upgraded and the paste has been continuously iterated. Silver-aluminum contact is becoming a key point in the back silver paste for crystalline silicon solar cells, especially at low solid content. However, there are few related invention patents on the market.
[0003] As the requirements for solar cells to paste continue to increase, the silver content of the back silver paste is decreasing year by year, resulting in insufficient sintering density, defects at the silver-aluminum joints, increased resistance of the cell, and even non-conductive cells, resulting in major problems such as black EL tests. Summary of the invention
[0004] The first object of the present invention is to provide a new back silver paste for crystalline silicon solar cells.
[0005] In order to achieve the above-mentioned first purpose of the present invention, the back silver paste for crystalline silicon solar cells includes: silver powder, organic binder, solvent A, glass powder, and organic additives; the mass ratio of the silver powder, organic binder, glass powder, and organic additives is: 35-75:25-45:0.1-5:0.5-5; the organic additive is tetrabutyl titanate; the addition amount of the solvent A is based on controlling the viscosity of the silver paste to 30-60 Pa.s.
[0006] In a specific embodiment, the silver powder is silver powder A and silver powder B, the silver powder A is flaky, needle-shaped or plate-shaped silver powder with an average particle size of 1 to 1.5 μm; the silver powder B is spherical silver powder with an average particle size of 0.5 to 2 μm; the mass ratio of the silver powder A to the silver powder B is preferably 1 to 6:6 to 12.
[0007] In a specific embodiment, the specific surface area of the silver powder A is 0.5 to 2 m 2 / g; the specific surface area of the silver powder B is 1 to 5m 2 / g.
[0008] In a specific embodiment, the organic binder includes a resin and a solvent B, the resin is composed of one or more organic resins with different decomposition temperatures, and the resin preferably includes one or more of rosin, cellulose acetate, ethyl cellulose, epoxy resin, and acrylic resin;
[0009] The solvent A or solvent B is one or more of ethyl acetate, terpineol, alcohol ester dodecahydrate, ethylene glycol butyl ether, ethylene glycol butyl ether acetate, diethylene glycol butyl ether, diethylene glycol butyl ether acetate, and DBE.
[0010] In a specific embodiment, the mass ratio of the resin to the solvent B is 5-40:60-95.
[0011] In a specific embodiment, the method of preparing the organic binder is as follows: the resin and solvent B are mixed and dissolved at 50 to 100° C. for 1 to 3 hours to obtain an organic binder.
[0012] The obtained organic binder is transparent and uniform.
[0013] In a specific embodiment, the glass powder is formed by melting Bi2O3, PbO, B2O3, SiO2, CuO, MnO2, ZnO, ZrO2, Al2O3, As2O3, CaCO3, K2CO3, Li2CO3, Rb2CO3, GeO2, Ga2O3, Cr2O3, Co3O4, and NiO in the following mass ratio: 3-10:6-12:6-12:20-35:20-30:3-10:0-8:0-8:5-15:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5; the average particle size of the glass powder is preferably 1-3 μm.
[0014] In a specific embodiment, the silver paste has a fineness of less than 10 microns.
[0015] The second object of the present invention is to provide a method for preparing the above-mentioned back silver paste for crystalline silicon solar cells.
[0016] To achieve the above purpose, the preparation method of the back silver paste for crystalline silicon solar cells comprises: mixing silver powder, organic binder, solvent A, glass powder, and organic additives, wherein the mass ratio of silver powder, organic binder, glass powder, and organic additives is 35-75:25-45:0.1-5:0.5-5, and then grinding and rolling the slurry 3-10 times to obtain a silver paste with a fineness of less than 10 microns and an amount of solvent A added to control the viscosity to 30-60 Pa.s.
[0017] In a specific embodiment, the method further comprises preparing an organic binder: mixing the resin and solvent B and dissolving them at 50 to 100° C. for 1 to 3 hours to obtain an organic binder;
[0018] Preferably, it also includes the preparation of glass powder: the Bi2O3, PbO, B2O3, SiO2, CuO, MnO2, ZnO, ZrO2, Al2O3, As2O3, CaCO3, K2CO3, Li2CO3, Rb2CO3, GeO2, Ga2O3, Cr2O3, Co3O4 and NiO are mixed in proportion and melted at 1100-1400°C for 4-7 hours, and then the molten glass material is introduced into deionized water for water quenching and then ball milled and dried to obtain glass powder with an average particle size of 1-3 μm.
[0019] Beneficial effects:
[0020] 1. The present invention perfectly solves the problem of back silver-silver-aluminum contact, reduces the generation of silver-aluminum alloy, thereby preventing aluminum thorns generated during the sintering process and silver-aluminum contact cracks and voids caused by different expansion coefficients.
[0021] 2. The back silver paste for crystalline silicon solar cells with good silver-aluminum contact of the present invention is mainly composed of four parts: conductive functional phase, organic carrier, inorganic binder and other additives. It is printed on silicon wafers and forms a dense contact with aluminum paste during sintering to collect current. Good contact between the back electrode and the aluminum paste is the key to the back silver paste for crystalline silicon solar cells.
[0022] 3. The present invention uses a combination of flaky, needle-shaped or plate-shaped silver powder and spherical silver powder, which effectively improves the compactness of the silver layer after sintering and reduces the silver electrode line resistance and the silver-aluminum contact resistance.
[0023] 4. The homemade glass powder can well infiltrate the silver powder during sintering, making the silver electrode dense and reducing the resistance of the silver electrode. At the same time, the glass powder can effectively slow down the corrosion of the solder on the silver after welding, increase the anti-aging performance and provide aging adhesion. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 PL test diagrams of Example 1 and Comparative Example 1, where Figure 1 The light-colored squares in the lower left and upper right of the middle are experimental example 1, and the dark-colored squares in the lower right and upper left are comparative example 1;
[0025] Figure 2 This is the morphology of the electrode under microscope of Example 1;
[0026] Figure 3 The morphology of the electrode of comparative example 3 under microscope. DETAILED DESCRIPTION
[0027] In order to achieve the above-mentioned first purpose of the present invention, the back silver paste for crystalline silicon solar cells includes: silver powder, organic binder, solvent A, glass powder, and organic additives; the mass ratio of the silver powder, organic binder, glass powder, and organic additives is: 35-75:25-45:0.1-5:0.5-5; the organic additive is tetrabutyl titanate; the addition amount of the solvent A is based on controlling the viscosity of the silver paste to 30-60 Pa.s.
[0028] In a specific embodiment, the silver powder is silver powder A and silver powder B, the silver powder A is flaky, needle-shaped or plate-shaped silver powder with an average particle size of 1 to 1.5 μm; the silver powder B is spherical silver powder with an average particle size of 0.5 to 2 μm; the mass ratio of the silver powder A to the silver powder B is preferably 1 to 6:6 to 12.
[0029] In a specific embodiment, the specific surface area of the silver powder A is 0.5 to 2 m 2 / g; the specific surface area of the silver powder B is 1 to 5m 2 / g.
[0030] In a specific embodiment, the organic binder includes a resin and a solvent B, the resin is composed of one or more organic resins with different decomposition temperatures, and the resin preferably includes one or more of rosin, cellulose acetate, ethyl cellulose, epoxy resin, and acrylic resin;
[0031] The solvent A or solvent B is one or more of ethyl acetate, terpineol, alcohol ester dodecahydrate, ethylene glycol butyl ether, ethylene glycol butyl ether acetate, diethylene glycol butyl ether, diethylene glycol butyl ether acetate, and DBE.
[0032] In a specific embodiment, the mass ratio of the resin to the solvent is 5-40:60-95.
[0033] In a specific embodiment, the method of preparing the organic binder is as follows: the resin and solvent B are mixed and dissolved at 50 to 100° C. for 1 to 3 hours to obtain an organic binder.
[0034] The obtained organic binder is transparent and uniform.
[0035] In a specific embodiment, the glass powder is a Bi-Pb-B-Si-Al system, and the glass powder is preferably formed by melting Bi2O3, PbO, B2O3, SiO2, CuO, MnO2, ZnO, ZrO2, Al2O3, As2O3, CaCO3, K2CO3, Li2CO3, Rb2CO3, GeO2, Ga2O3, Cr2O3, Co3O4, and NiO in the following mass ratio: 3-10:6-12:6-12:20-35:20-30:3-10:0-8:0-8:5-15:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5:0-5; the average particle size of the glass powder is preferably 1-3 μm.
[0036] In a specific embodiment, the silver paste has a fineness of less than 10 microns.
[0037] To achieve the above-mentioned second purpose, the preparation method of the back silver paste for crystalline silicon solar cells comprises: mixing silver powder, organic binder, solvent A, glass powder, and organic additives, wherein the mass ratio of silver powder, organic binder, glass powder, and organic additives is 35-75:25-45:0.1-5:0.5-5, and then grinding and rolling the slurry for 3-10 times to obtain a silver paste with a fineness of less than 10 microns and an amount of solvent A added to control the viscosity to 30-60 Pa.s.
[0038] In a specific embodiment, the method further comprises preparing an organic binder: mixing the resin and solvent B and dissolving them at 50 to 100° C. for 1 to 3 hours to obtain an organic binder;
[0039] Preferably, it also includes the preparation of glass powder: the Bi2O3, PbO, B2O3, SiO2, CuO, MnO2, ZnO, ZrO2, Al2O3, As2O3, CaCO3, K2CO3, Li2CO3, Rb2CO3, GeO2, Ga2O3, Cr2O3, Co3O4 and NiO are mixed in proportion and melted at 1100-1400°C for 4-7 hours, and then the molten glass material is introduced into deionized water for water quenching and then ball milled and dried to obtain glass powder with an average particle size of 1-3 μm.
[0040] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.
[0041] Example 1
[0042] The viscosity of the present invention is measured by using an Anton Paar rheometer under the conditions of a shear rate of 15 / s, a gap of 0.1 mm, and a temperature of 25°C.
[0043] Preparation of organic binder: according to the formula ratio, weigh 8% of ethyl cellulose by mass; weigh 92% of terpineol by mass; then dissolve at 80° C. for 3 hours to obtain a transparent and uniform organic binder;
[0044] Preparation of glass powder: according to the formula, 6 parts of Bi2O3, 10 parts of PbO, 10 parts of B2O3, 27 parts of SiO2, 24 parts of CuO, 5 parts of MnO2, 2 parts of ZnO, 3 parts of ZrO2, 10 parts of Al2O3, and 3 parts of Cr2O3 are weighed and mixed to prepare glass material, and melted at 1250°C for 6 hours, and then the molten glass material is introduced into deionized water for water quenching and ball milling, and dried to obtain a glass powder product with an average particle size of 1.73 microns;
[0045] According to the above formula ratio, the weight portions are as follows: one with an average particle size of 1.21 μm and an average specific surface area of 1.21 m 2 / g of flaky, needle-shaped or plate-shaped silver powder 15 parts, another average particle size of 0.91μm, average specific surface area of 1.41m 2 / g spherical silver powder 44.8 parts; glass powder 1.2 parts; organic binder 30 parts; solvent pineol 7 parts, tetrabutyl titanate 1 part, after mixing evenly, use a three-roll grinder to roll the slurry 8 times, and make the fineness less than 10 microns and the viscosity 31.36Pa.s to prepare a back silver paste for crystalline silicon solar cells with good silver-aluminum contact.
[0046] Example 2
[0047] Preparation of organic binder: according to the formula ratio, weigh 8% of ethyl cellulose by mass; weigh 92% of terpineol by mass; then dissolve at 80° C. for 3 hours to obtain a transparent and uniform organic binder;
[0048] Preparation of glass powder: according to the formula, 6 parts of Bi2O3, 10 parts of PbO, 10 parts of B2O3, 27 parts of SiO2, 24 parts of CuO, 5 parts of MnO2, 2 parts of ZnO, 3 parts of ZrO2, 10 parts of Al2O3, and 3 parts of Cr2O3 are weighed and mixed to prepare glass material, and melted at 1250°C for 6 hours, and then the molten glass material is introduced into deionized water for water quenching and ball milling, and dried to obtain a glass powder product with an average particle size of 1.73 microns;
[0049] According to the above formula ratio, the weight portions are as follows: one with an average particle size of 1.21 μm and an average specific surface area of 1.21 m 2 / g of flaky, needle-shaped or plate-shaped silver powder 15 parts, another average particle size of 0.91μm, average specific surface area of 1.41m 2 / g spherical silver powder 44.8 parts; glass powder 1.2 parts; organic binder 28 parts; solvent pineol 7 parts, tetrabutyl titanate 3 parts, after mixing evenly, use a three-roll grinder to roll the slurry 8 times, and make the fineness less than 10 microns and the viscosity 30.76Pa.s to prepare a back silver paste for crystalline silicon solar cells with good silver-aluminum contact.
[0050] Example 3
[0051] Preparation of organic binder: according to the formula ratio, weigh 8% of ethyl cellulose by mass; weigh 92% of terpineol by mass; then dissolve at 80° C. for 3 hours to obtain a transparent and uniform organic binder;
[0052] Preparation of glass powder: according to the formula, 6 parts of Bi2O3, 12 parts of PbO, 10 parts of B2O3, 25 parts of SiO2, 21 parts of CuO, 8 parts of MnO2, 4 parts of ZnO, 3 parts of ZrO2, 8 parts of Al2O3, and 3 parts of Cr2O3 are weighed and mixed to prepare glass material, and melted at 1250°C for 6 hours, and then the molten glass material is introduced into deionized water for water quenching and ball milling, and dried to obtain a glass powder product with an average particle size of 1.53 microns;
[0053] According to the above formula ratio, the weight portions are as follows: one with an average particle size of 1.21 μm and a specific surface area of 1.21 m 2 / g of flaky, needle-shaped or plate-shaped silver powder 15 parts, another average particle size of 0.91μm, specific surface area of 1.41m 2 / g spherical silver powder 44.8 parts; glass powder 1.2 parts; organic binder 30 parts; solvent pineol 7 parts, tetrabutyl titanate 1 part, after mixing evenly, use a three-roll grinder to roll the slurry 8 times, and make the fineness less than 10 microns and the viscosity 31.59Pa.s to prepare a back silver paste for crystalline silicon solar cells with good silver-aluminum contact.
[0054] Comparative Example 1
[0055] Preparation of organic binder: according to the formula ratio, weigh 8% of ethyl cellulose by mass; weigh 92% of terpineol by mass; then dissolve at 80° C. for 3 hours to obtain a transparent and uniform organic binder;
[0056] Preparation of glass powder: according to the formula, 6 parts of Bi2O3, 10 parts of PbO, 10 parts of B2O3, 27 parts of SiO2, 24 parts of CuO, 5 parts of MnO2, 2 parts of ZnO, 3 parts of ZrO2, 10 parts of Al2O3, and 3 parts of Cr2O3 are weighed and mixed to prepare glass material, and melted at 1250°C for 6 hours, and then the molten glass material is introduced into deionized water for water quenching and ball milling, and dried to obtain a glass powder product with an average particle size of 1.73 microns;
[0057] According to the above formula ratio, the weight portions are as follows: one with an average particle size of 1.21 μm and a specific surface area of 1.21 m 2 / g of flaky, needle-shaped or plate-shaped silver powder 15 parts, another average particle size of 0.91μm, specific surface area of 1.41m 2 / g spherical silver powder 44.8 parts; glass powder 1.2 parts; organic binder 30 parts; solvent pine alcohol 8 parts, after mixing evenly, use a three-roll grinder to roll the slurry 8 times, and make the fineness less than 10 microns and the viscosity 28.65Pa.s to prepare a back silver paste for crystalline silicon solar cells with good silver-aluminum contact.
[0058] Comparative Example 2
[0059] The most common PERC back silver paste on the market is RX63600A7-5-8 from Guangzhou Ruxing Technology Co., Ltd.
[0060] Comparative Example 3
[0061] Common low solid content PERC back silver paste on the market, Changsha New Materials Industry Research Institute Co., Ltd. HT3612
[0062] The specific test method is as follows:
[0063] Tensile force: Print a fixed pattern (rectangular pattern with a length of 20 cm and a width of 0.8 mm) and test the welding tensile force at 350°C.
[0064] Tensile force during high temperature welding: Print a fixed pattern (rectangular pattern with a length of 20 cm and a width of 0.8 mm) and test the welding tensile force at 450°C.
[0065] Oven aging tensile strength: Print a fixed pattern (a rectangular pattern with a length of 20 cm and a width of 0.8 mm), weld it at 350°C, put it in an oven at 150°C, and take it out after 1 hour to test the tensile strength.
[0066] PL (photoluminescence) test: Print fixed block diagram as follows Figure 1 In the experimental example and the comparative example, a common aluminum paste on the market was printed on the same cell to test its PL. The brighter the PL, the higher the minority carrier lifetime of the cell and the less the slurry etches the passivation layer.
[0067] Electrical properties: The above PERC back silver paste is printed on the solar PERC cell, dried, and co-fired with PERC aluminum paste and PERC front silver at a peak temperature of 750-830°C to form a back electrode.
[0068] Electrode morphology: Observe the electrode silver-aluminum contact morphology under a microscope, such as Figure 2 and 3 shown.
[0069] The specific data of the embodiments and comparative examples are as follows:
[0070] Table 1 Test results of Examples 1-3 and Comparative Examples 1-3
[0071]
[0072] Figure 1 The PL test results of Example 1 and Comparative Example 1 show that Example 1 is obviously brighter. This is because the method of the present invention forms a film on the electrode surface during the sintering process, preventing the aluminum paste from penetrating into the silver electrode. It also reduces the etching of the cell passivation layer by the paste, thereby increasing the minority carrier lifetime.
[0073] Figure 2 This is the electrode morphology of Example 1, where the silver-aluminum contact has a regular shape and no defects at the contact. Figure 3 This is the electrode morphology of comparative example 3. There are many black spots at the silver-aluminum contact. This is because the different expansion coefficients of the components at the silver-aluminum interface during the sintering process lead to depressions and defects during the heating and cooling processes.
Claims
1. A back silver paste for a crystalline silicon solar cell, characterized in that: The back silver paste for crystalline silicon solar cells is composed of silver powder, organic binder, solvent A, glass powder, and organic additives; the mass ratio of the silver powder, organic binder, glass powder, and organic additives is 35-75:25-45:0.1-5:0.5-5; the organic additive is tetrabutyl titanate; the amount of solvent A added is based on controlling the viscosity of the silver paste to 30-60 Pa.s; the preparation method of the back silver paste for crystalline silicon solar cells comprises: mixing the silver powder, organic binder, solvent A, glass powder, and organic additives, and then grinding and rolling the paste for 3-10 times to obtain a silver paste with a fineness of less than 10 microns, and the amount of solvent A added is based on controlling the viscosity to 30-60 Pa.s; The glass powder is a Bi-Pb-B-Si-Al system, and is formed by melting Bi2O3, PbO, B2O3, SiO2, CuO, MnO2, ZnO, ZrO2, Al2O3, As2O3, CaCO3, K2CO3, Li2CO3, Rb2CO3, GeO2, Ga2O3, Cr2O3, Co3O4, and NiO in the following mass ratios: 3-10: 6-12: 6-12: 20-35: 20-30: 3-10: 0-8: 0-8: 5-15: 0-5: 0-5: 0-5: 0-5: 0-5: 0-5: 0-5: 0-5: 0-5: 0-5: 0-5: 0-5; the average particle size of the glass powder is 1-3 μm.
2. The back silver paste for crystalline silicon solar cells according to claim 1, characterized in that: The silver powders are silver powder A and silver powder B. The silver powder A is flaky, needle-shaped or plate-shaped silver powder with an average particle size of 1 to 1.5 μm; the silver powder B is spherical silver powder with an average particle size of 0.5 to 2 μm.
3. The back silver paste for crystalline silicon solar cells according to claim 2, characterized in that: The mass ratio of the silver powder A to the silver powder B is 1-6:6-12.
4. The back silver paste for crystalline silicon solar cells according to claim 1 or 2, characterized in that: The specific surface area of the silver powder A is 0.5 to 2 m 2 / g; the specific surface area of the silver powder B is 1 to 5m 2 / g.
5. The back silver paste for crystalline silicon solar cells according to claim 1 or 2, characterized in that: The organic binder includes a resin and a solvent B, wherein the resin is composed of one or more organic resins with different decomposition temperatures; The solvent A or solvent B is one or more of ethyl acetate, terpineol, alcohol ester dodecahydrate, ethylene glycol butyl ether, ethylene glycol butyl ether acetate, diethylene glycol butyl ether, diethylene glycol butyl ether acetate, and DBE.
6. The back silver paste for crystalline silicon solar cells according to claim 5, characterized in that: The resin includes one or more of rosin, cellulose acetate, ethyl cellulose, epoxy resin, and acrylic resin.
7. The back silver paste for crystalline silicon solar cells according to claim 5, characterized in that: The mass ratio of the resin to the solvent B is 5-40:60-95.
8. The back silver paste for crystalline silicon solar cells according to claim 5, characterized in that: The method of preparing the organic binder is as follows: the resin and solvent B are mixed and dissolved at 50-100° C. for 1-3 hours to obtain the organic binder.
9. The back silver paste for crystalline silicon solar cells according to claim 1 or 2, characterized in that: The silver paste has a fineness of less than 10 microns.
10. The method for preparing a back silver paste for a crystalline silicon solar cell according to any one of claims 5 to 8, characterized in that: The method comprises the preparation of an organic binder: the resin and a solvent B are mixed and dissolved at 50 to 100° C. for 1 to 3 hours to obtain the organic binder.
11. The method for preparing back silver paste for crystalline silicon solar cells according to claim 10, characterized in that: The method also includes the preparation of glass powder: the Bi2O3, PbO, B2O3, SiO2, CuO, MnO2, ZnO, ZrO2, Al2O3, As2O3, CaCO3, K2CO3, Li2CO3, Rb2CO3, GeO2, Ga2O3, Cr2O3, Co3O4 and NiO are mixed in proportion and melted at 1100-1400°C for 4-7 hours, and then the molten glass material is introduced into deionized water for water quenching and then ball milled and dried to obtain glass powder with an average particle size of 1-3 μm.