By optimizing the nano-indentation characteristics and using photo-curable adhesive in the adhesive layer, combined with ultraviolet laser cutting technology, the problem of adhesive overflow when pasting optical components is solved, productivity and yield are improved, and it is especially suitable for Manufacturing of irregularly shaped image display devices.

CN114761228BActive Publication Date: 2024-10-29NITTO DENKO CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202080084725.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-06
Publication Date
2024-10-29
Estimated Expiration
2040-11-06

AI Technical Summary

Technical Problem

When pasting optical components, thick adhesive easily overflows from the chip end surface, causing foreign matter to adhere and stick. In irregular-shaped image display devices, it is difficult to align the adhesive layer, resulting in reduced productivity and yield. .

Method used

Adopt an adhesive layer with a minimum load of -0.2μN or more in the load curve and a displacement of less than 8μm in the unloading curve. By optimizing the nano-indentation characteristics, combined with photo-curable adhesive and ultraviolet laser cutting technology, the adhesive layer is ensured. The end face characteristics and the gel fraction of the adhesive reach more than 70% to prevent the adhesive from overflowing and adhesion.

Benefits of technology

It effectively prevents the adhesion and adhesion of foreign matter caused by adhesive overflow, improves operability and productivity, and ensures the stability and cutting accuracy of the adhesive layer especially in the manufacture of irregular-shaped image display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114761228B_ABST
    Figure CN114761228B_ABST
Patent Text Reader

Abstract

The optical laminate has adherends attached to the two main surfaces of the adhesive layer (21). The adherend attached to one surface of the adhesive layer (21) may be a polarizing plate, or may further include an image display unit such as an organic EL unit. The chip is obtained by cutting the optical laminate from the mother substrate. In the chip of the optical laminate, the physical properties of the end face of the adhesive layer (21) measured by nanoindentation are within a specified range. The adhesive constituting the adhesive layer (21) may be photocurable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an optical laminate to which an adherend is bonded via a pressure-sensitive adhesive layer, and a method for producing the same. Background Art

[0002] In display devices such as liquid crystal displays and organic EL displays, and display input devices such as touch panels, transparent adhesive sheets are used to adhere optical components. In addition, transparent adhesive sheets are also used when a cover window formed of a transparent resin plate, a glass plate, etc. is arranged on the visible side surface of the image display device.

[0003] A coloring layer for the purpose of decoration and light shielding is printed on the frame portion of the cover window, and a printing height difference of about 10 μm to several tens of μm is generated in the printed portion of the coloring layer. As described in Patent Document 1, in the pasting of optical components with printed height differences, a thick and soft adhesive sheet is used to prevent bubbles from being mixed into the printed height difference portion and stress concentration.

[0004] In recent years, organic EL panels using bendable substrates (flexible substrates) such as resin films have been put into practical use, and foldable displays that can be folded have also been put into practical use. In foldable displays, deformation occurs at and around the bent portion due to repeated bending at the same portion. Patent document 2 proposes the following scheme: In order to prevent damage to the device caused by concentrated deformation at the bent portion, the adhesive sheet that adheres the optical components to each other is softened to alleviate stress deformation.

[0005] Transparent adhesive sheets for bonding optical components are generally provided in the form of adhesive sheets with release films bonded to both sides, and are cut into a specified size for use according to the shape and size of the adherend. For example, in bonding the components of an image display device, an adhesive sheet cut into a single piece having a size substantially equal to the size of the screen is used. As described in Patent Documents 1 and 3, the transparent adhesive sheet can also be cut into a single piece for use in a state where it is previously bonded to an optical component such as a polarizing plate.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2014-115468

[0009] Patent Document 2: Japanese Patent Application Publication No. 2018-45213

[0010] Patent Document 3: Japanese Patent Application Publication No. 2019-179211 Summary of the invention

[0011] Problem that the invention aims to solve

[0012] If a thick adhesive or a soft adhesive is used, the adhesive exposed at the end face of the product (chip) cut into a single piece of a specified size is likely to overflow from the end face of the chip, sometimes causing foreign matter to adhere to the end face and surrounding contamination. In addition, if multiple chips are stacked and stored, the adhesive is likely to overflow from the end face, causing the adhesive sheets to stick to each other, and sometimes it is difficult to pick up the adhesive sheets one by one.

[0013] In order to suppress the undesirable situation caused by the adhesive overflowing from the end face, Patent Document 1 proposes the following scheme: cutting and processing are performed in a manner that the end face of the adhesive layer is located on the inner side compared to the end face (cut face) of the release film. The screen shape of the image display device is usually rectangular, but in the dashboard of a car, smart watch, etc., the screen shape is a shape other than a rectangle (irregular shape). In addition, in mobile devices such as smartphones, as bezel-less is being adopted, an irregular screen shape with a cutout on the periphery is adopted to configure cameras and sensors.

[0014] In order to manufacture an image display device with an irregular screen, it is necessary to process each optical component into an irregular shape. In addition, when pasting each component, it is necessary to align the positions correctly, which sometimes leads to a decrease in productivity and yield. Therefore, the following scheme is proposed: in a state where a plurality of optical components such as an organic EL unit and a polarizing plate are pasted in advance with an adhesive sheet, the optical components are cut into irregular shapes.

[0015] When chips are cut out in a state where a plurality of optical members are stacked, the end faces of the optical members and release films are aligned with the end faces of the adhesive sheet, making it difficult to process with the end face of the adhesive layer located inside the stack.

[0016] In view of the above, an object of the present invention is to provide an optical laminate in which foreign matter adhesion and blocking due to adhesive exposed on the end surface are unlikely to occur even when the end surface of the adhesive layer is aligned with the end surface of the optical member or the release film.

[0017] Solutions for solving problems

[0018] The optical laminate has a first adherend and a second adherend attached to the two main surfaces of the first adhesive layer. The thickness of the first adhesive layer can be 30 μm or more. As adherends, optical films such as polarizing plates, image display units, cover windows, release films, etc. can be listed. The optical laminate can have a polarizing plate in contact with the first adhesive layer, and the polarizing plate can also be further attached with an image display unit such as an organic EL unit.

[0019] The end surface of the first adhesive layer preferably has a minimum load of -0.2 μN or more in the load curve measured by nanoindentation and a displacement of 8 μm or less in the unloading curve. The gel fraction of the adhesive in the center of the first adhesive layer is preferably 25% or more.

[0020] The physical properties of the in-plane center portion and the end surface of the first adhesive layer may be different. For example, the minimum load of the load curve of the in-plane center portion of the first adhesive layer measured by nanoindentation may be less than 0.3 times the minimum load of the load curve of the end surface. The displacement of the unloading curve of the in-plane center portion of the first adhesive layer measured by nanoindentation may be less than 0.5 times the displacement of the unloading curve of the end surface.

[0021] The first adhesive layer may contain an ultraviolet absorber. The adhesive constituting the first adhesive layer may have photocurability.

[0022] The photocurable adhesive may contain a monomer or oligomer having a photocurable functional group in addition to a base polymer. In addition, a compound having a photocurable functional group may be bonded to the base polymer. The photocurable adhesive may contain a photopolymerization initiator. The gel fraction of the photocurable adhesive after photocuring is preferably 70% or more. The gel fraction of the photocurable adhesive after photocuring is preferably 1.2 times or more of the gel fraction before photocuring.

[0023] A monolithic optical laminate (chip) is obtained by cutting the mother substrate into a specified size. The chip can also be cut out from the mother substrate by irradiating an ultraviolet laser. The optical laminate is preferably such that when the first adhesive layer is cut by an ultraviolet laser, the minimum load of the load curve of the adhesive in the cut surface is less than 0.3 times that before the cutting process, the displacement of the unloading curve of the adhesive in the cut surface is less than 0.5 times that before the cutting process, and the indentation modulus of the adhesive in the cut surface is 1.5 to 10 times that before the cutting process.

[0024] Effects of the Invention

[0025] The optical laminate of the present invention is excellent in handling properties because foreign matter and blocking due to the adhesive exposed on the end surface are unlikely to occur even when the adhesive layer is exposed on the end surface of a chip cut out from a large-area mother substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a cross-sectional view of an optical layered body according to one embodiment.

[0027] Figure 2 This is a cross-sectional view of an optical layered body according to one embodiment.

[0028] Figure 3 This is a cross-sectional view of an optical layered body according to one embodiment.

[0029] Figure 4 This is a cross-sectional view of an optical layered body according to one embodiment.

[0030] Figure 5 This is a cross-sectional view of an optical layered body according to one embodiment.

[0031] Figure 6 This is an example of a load-displacement curve of a PSA sheet based on nanoindentation. DETAILED DESCRIPTION

[0032] [Laminated Structure Example of Optical Laminated Body]

[0033] The optical laminate of the present invention is a laminate in which adherends are bonded to the first and second principal surfaces of a transparent adhesive sheet, respectively. The adherend may be fixedly laminated on the adhesive layer or may be bonded in a releasable manner (temporary bonding).

[0034] Figure 1 The optical layered body 101 is a cross-sectional view of an embodiment. The optical layered body 101 is a pressure-sensitive adhesive sheet with release films, in which release films 41 and 43 are temporarily attached to the first main surface and the second main surface of the pressure-sensitive adhesive layer 21, respectively.

[0035] Figure 2 The optical laminate 102 shown is a polarizing plate with an adhesive in which an adhesive layer 21 is laminated on the first main surface of an optical film 10. Figure 1 The release film 43 is peeled off from the optical layered body 101 shown, and the optical film 10 is attached to the second main surface of the exposed pressure-sensitive adhesive layer 21 to form an optical layered body 102 .

[0036] Figure 3 The optical laminate 103 shown is a polarizing plate with adhesives on both sides, wherein a first adhesive layer 21 is laminated on a first main surface of an optical film 10, and a second adhesive layer 22 is laminated on a second main surface of the optical film 10. Figure 2 The second adhesive layer 22 is stacked on the second main surface of the optical film 10 of the optical laminate 102 shown, thereby forming an optical laminate 103. The first adhesive layer 21 may be stacked after the second adhesive layer 22 is stacked on the second main surface of the optical film 10, or the first adhesive layer 21 and the second adhesive layer 22 may be stacked on both main surfaces of the optical film 10 at the same time.

[0037] Figure 4 The optical laminate 104 shown is an image display panel having an optical film 10 on the surface of the image display unit 70. Figure 3The release film 42 is peeled off from the optical laminate 103 shown, and the image display unit 70 is attached to the exposed second pressure-sensitive adhesive layer 22 , thereby forming an optical laminate 104 .

[0038] Figure 5 The optical laminate 105 shown is an image display panel having a cover window 80 on the surface of the polarizing plate. Figure 4 The release film 41 is peeled off from the optical laminate 104 shown, and a cover window 80 is attached to the exposed first main surface of the first pressure-sensitive adhesive layer 21 , thereby forming an optical laminate 105 .

[0039] The optical laminate can be formed by laminating an adherend on the front and back surfaces of the adhesive layer 21, and its lamination structure is not limited to the above structure. Figure 3 As shown in the figure, the optical laminate may further include another adhesive layer 22 on the adherend (optical film 10) attached to the adhesive layer 21, or may be Figure 4 As shown in FIG. 1 , an adherend (image display unit 70) is further attached to the adhesive layer 22. Figure 5 As shown, an adherend (cover window 80) is fixedly laminated on the first adhesive layer 21. Another adherend may be laminated on the adherend bonded to the first adhesive layer 21 via another adhesive layer.

[0040] [Characteristics of optical stacked chip]

[0041] These optical laminates are usually cut into single-piece products (chips) of a specified size after forming a large-sized mother substrate. In this method, multiple sheet products can be obtained from the mother substrate, so the productivity can be improved. In the chip cut out of the optical laminate with adherends attached to both sides of the adhesive sheet, the end face of the adherend attached to the adhesive is aligned with the end face of the adhesive layer, and the adhesive layer is exposed at the end face of the laminate.

[0042] In the optical laminate of the present invention, the end face of the adhesive layer 21 has a predetermined characteristic. The characteristics of the end face of the adhesive layer can be evaluated by nanoindentation. The nanoindentation method is a method in which the indenter of the nanoindenter is pressed into the sample (loaded) to a predetermined depth, and then the indenter is lifted (unloaded) until the indenter leaves the sample, and the mechanical characteristics of the sample surface are analyzed by the relationship between the displacement and the load (load-displacement curve) at this time.

[0043] Figure 6It is an example of a load-variation curve of an adhesive sheet measured at a certain load / unload speed. If the indenter is brought close to the sample, when the indenter contacts the sample, a negative load (the force that pulls the indenter toward the sample) (point A) is applied to the indenter. The load w at this time is the minimum load of the load curve. The minimum load w of the load curve is the force of the adhesive layer pulling into the adherend, foreign matter, and other adherends (the force and adhesion of the adhesive to the adherend), which reflects the surface tension and wettability of the adhesive. The smaller the minimum load w of the load curve (the larger the absolute value of w), the greater the wettability of the adhesive, and it is easy to fit when contacting the adherend.

[0044] The indenter is pressed at a constant load speed until it reaches a predetermined depth p (point B). The load q at this time is the maximum load of the load curve. The greater the load q, the harder the adhesive.

[0045] After the indenter is pressed to a depth of p, it is lifted at a constant unloading speed. When the force of lifting the indenter and the force of the adhesive to hold the indenter (adhesion) are in balance, the test force decreases. If the two lose balance, the unloading curve shows a minimum value (point C). The load u at this time is the minimum load of the unloading curve. The higher the adhesion, the larger the absolute value of the load u becomes.

[0046] Furthermore, if the pressure head is lifted, the pressure head begins to peel off from the adhesive, and when the pressure head is completely peeled off from the adhesive, the load reaches 0 (point D). The absolute value d of the displacement at this time is the displacement of the unloading curve. The adhesive is prone to local deformation, and the greater the wire drawing caused by shrinkage or necking, the greater the displacement d of the unloading curve becomes.

[0047] The load-displacement curve of the end surface of the adhesive layer of the optical laminate was measured using a conical-spherical indenter with a tip curvature radius of 10 μm (a conical indenter with a curved tip) at a load speed / unload speed of 1000 nN / sec and an indentation depth of 3000 nm.

[0048] The minimum load w of the load curve of the end face of the adhesive layer 21 is preferably greater than -0.2μN. The minimum load w of the load curve is more preferably greater than -0.15μN, further preferably greater than -0.1μN, and particularly preferably greater than -0.07μN. The larger W is (the smaller the absolute value of w is) and the closer it is to 0, the less sticky the end face of the adhesive layer is, and there is a tendency to suppress adhesion caused by adhesion of foreign matter and contact between the end faces of the chip.

[0049] The displacement d of the unloading curve of the end face of the adhesive layer 21 is preferably 8 μm or less. The displacement of the unloading curve is preferably 7 μm or less, more preferably 6 μm or less, and further preferably 5 μm or less. As d is smaller and closer to 0, the adhesive at the end face of the adhesive layer is less likely to deform, and there is a tendency that overflow from the end face caused by the flow of the adhesive and adhesion between chips when multiple chips are stacked are suppressed.

[0050] From the viewpoint of suppressing the flow of the adhesive at the end surface, the indentation modulus of the end surface of the adhesive layer 21 is preferably 0.3 MPa or more, more preferably 0.35 MPa or more, and even more preferably 0.4 MPa or more.

[0051] As described above, for a chip of an optical stack in which the adhesive layer 21 is exposed at the end face, from the viewpoint of suppressing the adhesion of foreign matter caused by the end face of the adhesive layer and the adhesion of chips to each other, the absolute value of the minimum load w of the load curve and the displacement d of the unloading curve are preferably smaller at the end face of the adhesive layer 21.

[0052] On the other hand, the wettability and viscosity of the adhesive are important properties for bonding and holding the adherend. An adhesive sheet with a small absolute value of the minimum load w of the load curve and a small displacement d of the unloading curve sometimes has poor adhesion and retention to the adherend. Therefore, the adhesive layer 21 preferably has the above-mentioned properties locally at the end face, and in the central part of the chip surface, the absolute value of the minimum load w of the load curve and the displacement d of the unloading curve are preferably larger than the end face. In other words, the adhesive layer 21 preferably has a smaller absolute value of the minimum load w of the load curve and the displacement d of the unloading curve locally at the end face (and its vicinity). By reducing the absolute value of w and d locally at the end face, it is possible to reduce the adhesion and adhesion of foreign matter caused by the exposed end face of the adhesive layer while maintaining the bonding properties to the adherend.

[0053] In the chip of the optical laminate, the minimum load w of the load curve is preferably less than -0.2 μN, more preferably less than -0.25 μN, in the center of the plane of the adhesive layer 21. The displacement d of the unloading curve is preferably greater than 10 μm, more preferably greater than 12 μm, and further preferably greater than 14 μm, in the center of the plane of the adhesive layer 21.

[0054] The minimum load w of the load curve of the end face of the adhesive layer 21 is preferably less than 0.3 times the minimum load of the load curve of the center portion of the surface, more preferably less than 0.2 times, and further preferably less than 0.1 times. The displacement d of the unloading curve of the end face of the adhesive layer 21 is preferably less than 0.5 times the displacement of the unloading curve of the center portion of the surface, more preferably less than 0.4 times, and further preferably less than 0.3 times. The indentation modulus of the end face of the adhesive layer 21 is preferably 1.5 to 10 times the indentation modulus of the center portion of the surface, more preferably 2 to 8 times, and further preferably 2.5 to 7 times.

[0055] The chip of the optical laminate is cut in the center of the surface in such a way that the adhesive does not change in properties, and the indenter is brought into contact with the cut surface, thereby enabling nanoindentation measurement of the adhesive in the center of the surface of the adhesive layer 21 of the optical laminate. Alternatively, the adherend may be peeled off from the adhesive layer, and the indenter may be brought into contact with the main surface of the adhesive layer for measurement.

[0056] In order to reduce the absolute value of the minimum load w of the load curve of the end face and the displacement d of the unloading curve while maintaining the adhesive properties of the in-plane central portion of the adhesive layer 21, for example, it is sufficient to locally modify the adhesive on the end face and its vicinity. For example, the adhesive can be modified by locally heating the end face of the chip. When the adhesive constituting the adhesive layer 21 is curable, the adhesive on the end face and its vicinity can be selectively cured by irradiating the end face with active energy rays such as electron beams and ultraviolet rays. In addition, when the chip is cut out from the mother substrate, the adhesive on the cut surface can be modified. For example, when the adhesive constituting the adhesive layer 21 is photocurable, if ultraviolet laser is used for cutting, the cut surface (end face of the chip) and the laser irradiation area near it can be locally photocured.

[0057] [Components of the optical layered body]

[0058] As described above, the components constituting the optical laminate are optical members bonded to the pressure-sensitive adhesive layer 21 or optical members bonded via another pressure-sensitive adhesive. Specific examples thereof include optical films, image display units, and cover windows.

[0059] <Image Display Unit>

[0060] exist Figure 4 In the optical stack 104 shown, the image display unit 70 is a top emission type organic EL unit, which is provided with a metal electrode 73, an organic light emitting layer 75 and a transparent electrode 77 in sequence on a substrate 71. A sealing material 79 is stacked on the transparent electrode 77. Although not shown in the figure, the sealing material 79 is preferably provided in a manner covering the side surfaces of the electrodes 73, 77 and the organic light emitting layer 75.

[0061] As the substrate 71, a glass substrate or a plastic substrate is used. In a top-emitting organic EL unit, the substrate 71 does not need to be transparent, and a highly heat-resistant film such as a polyimide film can be used as the substrate 71. When a polyimide film is used as the substrate 71, polyimide has a large ultraviolet absorption, so the laminate 104 can be cut by irradiating an ultraviolet laser from the side of the substrate 71. Even if a material other than polyimide is used, a resin material with high ultraviolet absorption such as polyethylene naphthalate (PEN) or a material containing an ultraviolet absorber can be used as the material of the substrate 71, so that cutting can be easily performed using an ultraviolet laser.

[0062] The organic light emitting layer 75 may include an electron transport layer, a hole transport layer, etc. in addition to the organic layer that functions as a light emitting layer. The transparent electrode 77 is a metal oxide layer or a metal thin film that transmits light from the organic light emitting layer 75. A back plate (not shown) may be provided on the back side of the substrate 71 for the purpose of protecting and reinforcing the substrate.

[0063] The organic EL unit may be a bottom emission type in which a transparent electrode, an organic light-emitting layer, and a metal electrode are sequentially stacked on a substrate. In a bottom emission type organic EL unit, a transparent substrate is used, and the substrate is arranged on the visible side (the second adhesive layer 22 side). The image display unit is not limited to an organic EL unit, and may be a liquid crystal unit, an electrophoretic display unit (electronic paper), etc. A touch panel sensor (not shown) may be arranged on the visible side surface of the image display unit 70.

[0064] <Optical Film>

[0065] As the optical film 10 disposed on the visible side surface of the organic EL unit 70, a polarizing plate can be cited. The polarizing plate includes a polarizer 11, and transparent films 13 and 15 as polarizer protective films are laminated on both sides of the polarizer 11. The polarizer protective film on one or both sides of the polarizer can be omitted, and an adhesive layer can be directly provided on the polarizer 11.

[0066] The polarizer 11 includes, for example, a polarizer obtained by adsorbing dichroic substances such as iodine and dichroic dyes onto hydrophilic polymer films such as polyvinyl alcohol films, partially formalized polyvinyl alcohol films, and partially saponified films of ethylene-vinyl acetate copolymers, and then uniaxially stretching them; and polyene-based oriented films such as dehydrated products of polyvinyl alcohol and dehydrochlorinated products of polyvinyl chloride.

[0067] As the polarizer 11, a thin polarizer with a thickness of 10 μm or less may be used. As the thin polarizer, for example, polarizers described in Japanese Patent Publication No. 51-069644, Japanese Patent Publication No. 2000-338329, WO2010 / 100917, Japanese Patent No. 4691205, and Japanese Patent No. 4751481 can be cited. The thin polarizer is obtained by a method including, for example, the following steps: a step of stretching a polyvinyl alcohol-based resin layer and a stretching resin substrate in a laminated state; and a step of dyeing with a dichroic material such as iodine.

[0068] As the transparent films 13 and 15, transparent resin films such as cellulose resin, cyclic polyolefin resin, acrylic resin, phenylmaleimide resin, and polycarbonate resin are preferably used. When the transparent films 13 and 15 are provided on both sides of the polarizer 11, the transparent films 13 and 15 may be films formed of the same resin material or films formed of different resin materials.

[0069] The optical film 10 may have an optical functional film laminated by means of an appropriate adhesive layer or adhesive layer on one or both surfaces of the polarizer 11 as required. As optical functional films, phase difference plates, field angle expansion films, field angle restriction (anti-peep) films, brightening films, etc. may be listed. The optical film 10 may include a touch panel sensor as an optical functional film. The transparent films 13 and 15 in contact with the polarizer may have the functions of a polarizer protective film and an optical functional film. The transparent films 13 and 15 may have the function of an electrode substrate film as a touch panel sensor.

[0070] The metal electrode 73 of the organic EL unit 70 is light reflective. Therefore, if external light enters the interior of the organic EL unit, the light is reflected by the metal electrode 73, and the reflected light looks like a mirror from the outside. By configuring a circular polarizer as an optical film 10 on the visible side surface of the organic EL unit 70, it is possible to prevent the reflected light at the metal electrode 73 from being re-emitted to the outside, thereby improving the visibility and design of the screen of the display device.

[0071] The circular polarizer has a phase difference film on the surface of the organic EL unit 70 side of the polarizer 11. The transparent film 15 arranged adjacent to the polarizer 11 can be a phase difference film. The phase difference film has a delay of λ / 4, and when the angle between the slow axis direction of the phase difference film and the absorption axis direction of the polarizer 11 is 45°, the laminate of the polarizer and the phase difference film functions as a circular polarizer for suppressing the reflected light at the metal electrode 73 from being emitted again. The phase difference film constituting the circular polarizer can be stacked with more than two layers of film. For example, by stacking the polarizer, the λ / 2 plate and the λ / 4 plate in a manner such that their respective optical axes present a specified angle, a wide-band circular polarizer that functions as a circular polarizer in a wide band of visible light can be obtained.

[0072] <Overlay Window>

[0073] As the cover window 80, a transparent plate having appropriate mechanical strength and thickness can be used. As such a transparent plate, a transparent resin plate or a glass plate such as an acrylic resin, a polycarbonate resin, or a transparent polyimide resin can be used. The thickness of the cover window 80 is, for example, about 20 to 2000 μm. In a flexible device, as the cover window 80, a transparent resin film is preferably used, and its thickness is preferably 20 to 500 μm, more preferably 30 to 300 μm, and further preferably 50 to 200 μm. As the cover window 80, a thin glass substrate that can be bent can be used.

[0074] The cover window 80 may be integrated with the touch panel sensor. An anti-reflection layer, a hard coating layer, etc. may be provided on the visible side surface of the cover window 80 .

[0075] <Release film>

[0076] As the release films 41, 42, 43 temporarily attached to the adhesive layers 21, 22, it is preferable to use a release film having a release layer on the surface of the film substrate. As the material of the release layer, silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, fatty acid amide-based release agents, etc. can be cited. From the perspective of being able to achieve both adhesion and releasability to acrylic adhesives, silicone release agents are preferred.

[0077] As the film substrate of the release film, a transparent resin film is preferably used. As the resin material, polyester resins such as polyethylene terephthalate and polyethylene naphthalate can be listed; acetate resins, polyethersulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth) acrylic resins, polyvinyl chloride resins, polyvinylidene chloride resins, polystyrene resins, polyvinyl alcohol resins, polyarylate resins, polyphenylene sulfide resins, etc. Among these, polyester resins such as polyethylene terephthalate (PET) are particularly preferred. The thickness of the release film is preferably 10 to 200 μm, more preferably 25 to 150 μm.

[0078] <First Adhesive Layer>

[0079] The first adhesive layer 21 is an adhesive layer formed in a layered state. Figures 2 to 5 In the optical laminate shown, the first pressure-sensitive adhesive layer 21 is disposed on the visible side of the optical film 10 and is used to bond the optical film 10 to a transparent member such as a cover window 80 .

[0080] The adhesive layer 21 is preferably transparent and has low absorption of visible light. The total light transmittance of the adhesive layer 21 is preferably 85% or more, more preferably 90% or more. The haze of the adhesive layer 21 is preferably 2% or less, more preferably 1% or less. The total light transmittance and haze are measured using a haze meter in accordance with JIS K7136.

[0081] As the adhesive constituting the adhesive layer 21, an adhesive having an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyvinyl ether, a vinyl acetate / vinyl chloride copolymer, a modified polyolefin, an epoxy polymer, a fluorine polymer, a rubber polymer or the like as a base polymer can be appropriately selected and used.

[0082] As the adhesive constituting the adhesive layer 21, an acrylic adhesive having an acrylic polymer as a base polymer is preferably used, because it has excellent optical transparency, exhibits appropriate adhesive properties such as wettability, cohesiveness and adhesion, and is also excellent in weather resistance, heat resistance, etc. In the acrylic adhesive, the content of the acrylic base polymer relative to the total solid content of the adhesive composition is preferably 50% by weight or more, more preferably 70% by weight or more, and even more preferably 80% by weight or more.

[0083] As the acrylic base polymer, a polymer having a monomer unit of an alkyl (meth)acrylate as a main skeleton is preferably used. In the present specification, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid.

[0084] As the alkyl (meth)acrylate, an alkyl (meth)acrylate having an alkyl group with 1 to 20 carbon atoms is preferably used. The alkyl group in the alkyl (meth)acrylate may have a branched chain. The content of the alkyl (meth)acrylate is preferably 40% by weight or more, more preferably 50% by weight or more, and further preferably 60% by weight or more relative to the total amount of the monomer components constituting the base polymer. The acrylic base polymer may be a copolymer of multiple alkyl (meth)acrylates. The arrangement of the constituent monomer units may be random or block.

[0085] In the acrylic base polymer, as a copolymer component, an acrylic monomer unit having a crosslinkable functional group can be included. When the base polymer has a crosslinkable functional group, the gel fraction of the adhesive can be easily increased due to thermal crosslinking, photocuring, etc. of the base polymer. As acrylic monomers having a crosslinkable functional group, hydroxyl-containing monomers and carboxyl-containing monomers can be listed. Among them, as a copolymer component of the base polymer, a hydroxyl-containing monomer is preferably included. When the base polymer has a hydroxyl-containing monomer as a monomer unit, there is a tendency that the crosslinking property based on an isocyanate crosslinking agent, etc. is improved and the white turbidity of the adhesive under a high temperature and high humidity environment is suppressed, and an adhesive with high transparency can be obtained.

[0086] Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethyl)cyclohexylmethyl (meth)acrylate.

[0087] The content of the hydroxyl group-containing monomer is preferably 0.1 to 50% by weight, more preferably 1 to 40% by weight, and even more preferably 3 to 30% by weight, based on the total amount of monomer components constituting the base polymer.

[0088] In the acrylic base polymer, it is preferred that, in addition to the hydroxyl-containing monomer unit, a highly polar monomer unit such as a nitrogen-containing monomer is contained. By containing a highly polar monomer such as a nitrogen-containing monomer in addition to the hydroxyl-containing monomer, the adhesive has high adhesion and holding power, and white turbidity is suppressed in a high temperature and high humidity environment.

[0089] Examples of the nitrogen-containing monomer include vinyl monomers such as N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, (meth)acryloylmorpholine, N-vinylcarboxylic acid amides, and N-vinylcaprolactam; and cyanoacrylate monomers such as acrylonitrile and methacrylonitrile. Among them, N-vinylpyrrolidone and (meth)acryloylmorpholine are preferably used.

[0090] The content of the nitrogen-containing monomer is preferably 0.1 to 50% by weight, more preferably 1 to 40% by weight, and even more preferably 3 to 30% by weight, based on the total amount of monomer components constituting the base polymer.

[0091] The monomer components forming the acrylic polymer may include a multifunctional monomer component. The multifunctional monomer is a monomer having at least two polymerizable functional groups having unsaturated double bonds, such as (meth)acryloyl groups or vinyl groups. The multifunctional monomer may have three or more polymerizable functional groups in one molecule.

[0092] The base polymer can be prepared by known polymerization methods such as solution polymerization, UV polymerization, bulk polymerization, and emulsion polymerization. From the viewpoints of transparency, water resistance, cost, etc. of the adhesive, solution polymerization or UV polymerization is preferred. As solvents for solution polymerization, ethyl acetate, toluene, etc. are generally used. When preparing the base polymer, polymerization initiators such as photopolymerization initiators and thermal polymerization initiators can be used depending on the type of polymerization reaction. In order to adjust the molecular weight of the base polymer, a chain transfer agent can be used.

[0093] From the viewpoint of imparting appropriate adhesive holding power and flexibility to the adhesive, the weight average molecular weight of the base polymer is preferably 200,000 to 1,000,000, more preferably 250,000 to 800,000. The molecular weight of the base polymer refers to the molecular weight of the polymer before the crosslinking structure is introduced.

[0094] The base polymer may have a cross-linked structure. By introducing a cross-linked structure into the base polymer, the cohesive force of the adhesive is increased, and the adhesion to the adherend is improved. The formation of the cross-linked structure is carried out by, for example, adding a cross-linking agent after the polymerization of the base polymer. As the cross-linking agent, commonly used cross-linking agents such as isocyanate cross-linking agents, epoxy cross-linking agents, oxazoline cross-linking agents, aziridine cross-linking agents, carbodiimide cross-linking agents, and metal chelate cross-linking agents can be used. The content of the cross-linking agent is generally in the range of 0.01 to 5 parts by weight relative to 100 parts by weight of the acrylic base polymer, preferably 0.05 to 3 parts by weight, and more preferably 0.07 to 2.5 parts by weight. The more the amount of cross-linking agent added, the greater the gel fraction of the adhesive.

[0095] The adhesive constituting the adhesive layer 21 may be photocurable. For example, if a photocurable adhesive is used in the pasting of an adherend having a printed height difference caused by decorative printing or the like (e.g., a cover window), the adhesive before photocuring can have the ability to follow the height difference by pasting in a soft state, and the adhesive can be photocured by irradiating ultraviolet rays or the like after pasting, thereby improving the bonding reliability. In addition, if the adhesive is photocurable, when the optical laminate is cut by laser irradiation to cut out a chip, the cut surface (the end face of the chip) and its vicinity can be locally photocured, and the absolute value of the minimum load w of the load curve of the end face and the displacement d of the unloading curve can be reduced while maintaining the bonding characteristics of the in-plane central portion of the adhesive layer 21.

[0096] The photocurable adhesive preferably contains, for example, a photocurable compound (a monomer or oligomer having a photopolymerizable functional group) in addition to a base polymer. The base polymer may be provided with photocurability by introducing a photopolymerizable functional group into the base polymer.

[0097] As the photocurable compound, it is preferred to include a multifunctional polymerizable compound having two or more polymerizable functional groups in one molecule. As the multifunctional polymerizable compound, there can be listed compounds having two or more ethylenically unsaturated groups in one molecule; compounds having one C=C bond and polymerizable functional groups such as epoxy, aziridine, oxazoline, hydrazine, hydroxymethyl, etc. Among them, preferred are compounds having two or more ethylenically unsaturated groups in one molecule, such as multifunctional (meth)acrylates. Specific examples of the multifunctional polymerizable compound include polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, bisphenol A ethylene oxide-modified di(meth)acrylate, bisphenol A propylene oxide-modified di(meth)acrylate, alkanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, ethoxylated isocyanuric acid triacrylate, pentaerythritol tri(meth)acrylate, pentaerythritol di(meth)acrylate, Ester, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol poly(meth)acrylate, dipentaerythritol hexa(meth)acrylate, neopentyl glycol di(meth)acrylate, glycerol di(meth)acrylate, urethane (meth)acrylate, epoxy (meth)acrylate, butadiene (meth)acrylate, isoprene (meth)acrylate, and the like.

[0098] The amount of the photocurable compound used varies depending on its molecular weight, number of functional groups, etc., and is preferably 0.3 to 10 parts by weight, more preferably 0.5 to 5 parts by weight, relative to 100 parts by weight of the base polymer. The more the amount of photocurable compound added, the easier it is to cure the adhesive on the cut surface by laser irradiation, and there is a tendency for the absolute value of the minimum load w of the load curve of the end face and the displacement d of the unloading curve to become smaller.

[0099] Examples of a method for introducing a photopolymerizable functional group into a base polymer include a method of mixing a compound having a functional group capable of bonding to a functional group (hydroxyl group, carboxyl group, etc.) of the base polymer and a radical polymerizable functional group with the base polymer.

[0100] The photocurable adhesive preferably further comprises a photopolymerization initiator on the basis of a polymer having a photocurable compound and / or a photopolymerizable functional group introduced therein. As the photopolymerization initiator, benzoin ether-based photopolymerization initiators, acetophenone-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzyl-based photopolymerization initiators, benzophenone-based photopolymerization initiators, ketal-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, etc. can be listed. The amount of the photopolymerization initiator added is preferably 0.01 to 5 parts by weight, and more preferably 0.05 to 3 parts by weight relative to 100 parts by weight of the base polymer.

[0101] In addition to the above-exemplified components, the adhesive may contain additives such as a silane coupling agent, a tackifier, a plasticizer, a softener, an anti-degradation agent, a filler, a colorant, an antioxidant, a surfactant, and an antistatic agent.

[0102] The adhesive may contain an ultraviolet absorber. If the adhesive layer 21 has ultraviolet absorption, when the optical laminate is cut by irradiation with ultraviolet laser, the adhesive layer 21 absorbs the energy of the laser, so there is a tendency that the cutting processability of the optical laminate is improved, and the undesirable conditions such as poor processing or peeling of the adherend are suppressed. The light transmittance of the first adhesive layer 21 at a wavelength of 355nm can be 80% or less or 75% or less. The content of the ultraviolet absorber in the adhesive layer 21 is, for example, about 0.01 to 10% by weight.

[0103] Examples of the ultraviolet absorber include benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, triazine ultraviolet absorbers, salicylate ultraviolet absorbers, cyanoacrylate ultraviolet absorbers, etc. From the perspective of easily obtaining an acrylic pressure-sensitive adhesive sheet having high ultraviolet absorbency, excellent compatibility with acrylic polymers, and high transparency, triazine ultraviolet absorbers and benzotriazole ultraviolet absorbers are preferred, and among them, triazine ultraviolet absorbers containing a hydroxyl group and benzotriazole ultraviolet absorbers having one benzotriazole skeleton in one molecule are preferred.

[0104] The adhesive layer is formed by coating the adhesive composition in a layer on the substrate, and drying the solvent and crosslinking / curing the base polymer as needed. The thickness of the adhesive layer 21 is not particularly limited, and is usually about 5 to 1000 μm. When the adhesive layer 21 is required to have high-low tracking properties and stress relaxation properties, the thickness of the adhesive layer 21 is preferably 30 μm or more. The thickness of the adhesive layer 21 may be 40 μm or more or 50 μm or more. Considering the viewpoint of lightweight / thinning of the display device, the ease of forming the adhesive layer, the operability, etc., the thickness of the adhesive layer 21 is preferably 500 μm or less, more preferably 300 μm or less, and further preferably 250 μm or less.

[0105] From the viewpoint of flexibility, the storage modulus G' of the adhesive layer 21 at 25°C is preferably 0.35 MPa or less, more preferably 0.30 MPa or less, and further preferably 0.20 MPa or less. On the other hand, when the adhesive layer 21 is too soft, foreign matter may adhere to the adhesive exposed on the end surface and the chip may stick together. Therefore, the storage modulus G' of the first adhesive layer 21 at 25°C is preferably 0.01 MPa or more, and more preferably 0.02 MPa or more. The storage modulus G' of the first adhesive layer 21 at 25°C may be 0.03 MPa or more, 0.05 MPa or more, or 0.1 MPa or more.

[0106] The gel fraction of the adhesive layer 21 is preferably 25% or more. If the gel fraction is too low, foreign matter may adhere to the adhesive exposed on the end face and the chip may stick. As described in detail later, the greater the gel fraction of the adhesive layer 21, the smaller the absolute value of the minimum load w of the load curve based on the cut surface (end face) processed by the laser and the displacement d of the unloading curve. The gel fraction of the adhesive layer 21 is preferably 30% or more, more preferably 35% or more, further preferably 40% or more, and can be 45% or more.

[0107] The gel fraction of the adhesive can be obtained as the insoluble component relative to a solvent such as ethyl acetate, and specifically, as the weight fraction (unit: weight %) of the insoluble component after the adhesive is immersed in ethyl acetate at 23°C for 7 days relative to the sample before immersion. Generally speaking, the gel fraction of a polymer is equivalent to the degree of crosslinking, and the more crosslinked parts in the polymer, the greater the gel fraction. The gel fraction (the amount of crosslinked structure introduced) can be adjusted to the desired range by the method of introducing the crosslinked structure, the type and amount of the crosslinking agent, etc.

[0108] When the adhesive is photocurable, the gel fraction of the adhesive layer 21 after photocuring is preferably 70% or more. In addition, the gel fraction of the adhesive layer 21 after photocuring is preferably 1.2 times or more of the gel fraction before photocuring, and can be 1.3 times or more, 1.4 times or more, or 1.5 times or more.

[0109] <Second Adhesive Layer>

[0110] The second adhesive layer 22 is an adhesive layer formed in a layered state. Figures 3 to 5 In the optical laminate shown, the second adhesive layer 22 is used to adhere the optical film 10 and the image display unit 70 .

[0111] The second adhesive layer is preferably transparent and has low absorption of visible light. The total light transmittance of the adhesive layer 22 is preferably 85% or more, more preferably 90% or more. The haze of the adhesive layer 22 is preferably 2% or less, more preferably 1% or less.

[0112] The adhesive constituting the adhesive layer 22 is not particularly limited, and adhesives having various polymers as base polymers can be appropriately selected and used. As described above, the adhesive constituting the second adhesive layer 22 is preferably an acrylic adhesive having an acrylic polymer as a base polymer.

[0113] The thickness of the adhesive layer 22 is not particularly limited. The second adhesive layer 22 is not required to have the same thickness and softness as the first adhesive layer 21. The thickness of the adhesive layer 22 is, for example, about 3 to 50 μm, and can be 5 to 35 μm or 10 to 25 μm. The storage modulus G' of the adhesive layer 22 at 25°C is, for example, about 0.02 to 5 MPa. If the adhesive layer 22 is thinner than the adhesive layer 22, it is not easy to cause the adhesion and adhesion of foreign matter due to the adhesive exposed on the end face. Therefore, the adhesive properties of the second adhesive layer end face of the second adhesive layer are not particularly limited.

[0114] [Cutting of optical laminate]

[0115] The constituent elements of the optical laminate are laminated by means of an adhesive layer to form a mother substrate of the optical laminate. The lamination can be either a roll-to-roll method or an intermittent method. The roll-to-roll method and the intermittent method can also be used in combination. For example, a polarizing plate with adhesive on both sides can be made by laminating adhesive layers 21, 21 (and release films 41, 42) on both sides of an optical film 10 by a roll-to-roll method, and after being cut into sheets, the adhesive layer 22 of the polarizing plate with adhesive on both sides is pasted on the image display unit 70 formed into a sheet. The lamination of the image display unit can also be implemented by a roll-to-roll method.

[0116] The chip of the optical stack is obtained by cutting a monolithic product of a specified size from the mother substrate of the optical stack. The shape of the chip is not particularly limited and can be rectangular, polygonal, rounded polygonal, circular, etc., or can have a notch (cut) on the periphery.

[0117] As described above, the chip of the optical laminate shows predetermined physical properties in the nanoindentation measurement of the end surface of the pressure-sensitive adhesive layer 21 , and therefore foreign matter is unlikely to adhere to or stick to the chip end surface, and has excellent handling properties.

[0118] The method for cutting the optical laminate is not particularly limited, and examples thereof include: a method of punching using a Thomson knife or the like; a method of using a cutter such as a round knife or a dish knife; a method using a laser or water pressure, etc. From the perspective that the adhesive on the cut surface and its vicinity can be locally cured, laser cutting is preferred. When the adhesive layer 21 is formed of a photocurable adhesive, by cutting the optical laminate using an ultraviolet laser while photocuring the end face of the adhesive layer 21, the absolute value of the minimum load w of the load curve of the end face and the displacement d of the unloading curve can be reduced.

[0119] The ultraviolet laser is not particularly limited as long as it can irradiate with a wavelength of 400 nm or less, but the third harmonic of YAG laser (wavelength 355 nm) is preferred because of its high output and excellent processability. The laser power is, for example, about 0.1 to 50 W.

[0120] The laser can be irradiated from any surface of the optical laminate. The components arranged on the laser irradiation surface preferably have laser absorptivity. For example, ultraviolet laser can be used to irradiate the optical laminate. Figure 1 When the optical laminate 101 shown is cut, it is preferred that the release films 41 and 43 disposed on the laser irradiation surface have ultraviolet absorption properties. Figure 2 When the optical laminate 102 shown is irradiated with ultraviolet laser for cutting, it is preferable that the transparent film 15 has ultraviolet absorption. Figure 4When the optical layered body 104 shown is cut by irradiating ultraviolet laser, it is preferable that the substrate 71 has ultraviolet absorption property.

[0121] In order to make the film or adhesive layer have ultraviolet absorption, it is sufficient to add an ultraviolet absorber to the resin material. Alternatively, a resin material having ultraviolet absorption, such as polyimide film or polyethylene naphthalate, can be used. Figure 4 and Figure 5 In the optical laminates 104 and 105 shown, if the substrate 71 of the image display unit 70 is a polyimide film, the polyimide film will release heat / vaporize by irradiating the image display unit 70 side with ultraviolet laser light, so that the second adhesive layer 22, optical film 10, first adhesive layer 21 and release film 41 or cover window 80 provided on the image display unit 70 and above are blown away together with the vapor, forming a through hole penetrating the optical laminate. By moving the optical laminate relative to the laser light source, a cutting line formed by connecting the through holes is formed. By forming the cutting line along the periphery of the chip shape, a chip of a specified shape is cut out.

[0122] Components other than the laser irradiation surface may also have ultraviolet absorption. For example, if the adhesive layer 21 has ultraviolet absorption, the adhesive layer 21 absorbs ultraviolet laser light, and therefore, even when the adhesive layer 21 is thick and soft, it exhibits good processability. In addition, if the adhesive layer 21 has ultraviolet absorption, the release film 41 and the cover window 80 temporarily attached to the adhesive layer 21 are also processed as the adhesive layer 21 is heated and vaporized during processing, and therefore, the peeling of the adherend around the laser irradiation area and the mixing of bubbles can be suppressed.

[0123] In the chip of the optical laminated body cut by laser, the adhesive behavior of the adhesive layer 21 is locally different in the laser irradiation area of ​​the end face and its vicinity. The adhesive layer 21 preferably has a large absolute value of the minimum load w of the load curve and a large displacement d of the unloading curve in the center of the surface, and a small absolute value of the minimum load w of the load curve and a small displacement d of the unloading curve at the end face cut by laser irradiation.

[0124] In the cut surface based on laser irradiation, plasticization occurs due to molecular breakage. On the other hand, active species such as free radicals are generated by laser irradiation, and therefore, a curing effect caused by the generation of cross-linked structures between polymer chains is also generated. When the gel fraction of the adhesive is small, a large amount of low-molecular-weight molecular chains that are not cross-linked are generated due to molecular breakage, and therefore, there is a tendency for the plasticization effect to become larger. On the other hand, even if the molecular chain breaks, low-molecular-weight components will not be generated as long as the cross-linked structure remains. Therefore, when the gel fraction (cross-linking degree) of the adhesive is large, there is a tendency for the influence of curing caused by free radical reactions, etc. to become larger than plasticization based on molecular breakage. Therefore, there is the following tendency: the larger the gel fraction of the adhesive layer 21, the smaller the absolute value of the minimum load w of the load curve of the laser-processed end face and the displacement d of the unloading curve become.

[0125] When the adhesive is photocurable, the photocuring of the adhesive by laser irradiation also affects the characteristics of the cut surface. In particular, when the adhesive layer 21 formed of a photocurable adhesive composition containing a photocurable monomer and a photopolymerization initiator is cut by irradiating an ultraviolet laser, the adhesive layer 21 is locally photocured in the laser irradiation area of ​​the end surface and its vicinity. Therefore, there is a tendency that the absolute value of the minimum load w of the load curve of the laser-processed end surface and the displacement d of the unloading curve become smaller.

[0126] As described above, in the chip of the optical laminate, at the center of the surface of the adhesive layer 21, the minimum load w of the load curve is preferably less than -0.2μN, and more preferably less than -0.25μN. At the end face of the adhesive layer 21, the minimum load of the load curve is preferably greater than -0.2μN, more preferably greater than -0.15μN, further preferably greater than -0.1μN, and particularly preferably greater than -0.07μN. The minimum load of the load curve of the end face of the adhesive layer 21 is preferably less than 0.3 times the minimum load of the load curve in the center of the surface, more preferably less than 0.2 times, and further preferably less than 0.1 times. In other words, in the optical laminate (mother substrate) before being cut into chips, it is preferred that: the minimum load of the load curve of the adhesive layer 21 is less than -0.2μN, and when cutting is performed by irradiating ultraviolet laser, the absolute value of the minimum load of the load curve of the cut surface reaches less than 0.3 times.

[0127] In the chip of the optical laminate, in the central part of the surface of the adhesive layer 21, the displacement d of the unloading curve is preferably greater than 10 μm, more preferably greater than 12 μm, and further preferably greater than 14 μm. At the end face of the adhesive layer 21, the displacement of the unloading curve is preferably less than 8 μm, more preferably less than 7 μm, further preferably less than 6 μm, and particularly preferably less than 5 μm. The displacement of the unloading curve of the end face of the adhesive layer 21 is preferably less than 0.5 times the displacement of the unloading curve in the central part of the surface, more preferably less than 0.4 times, and further preferably less than 0.3 times. In other words, in the optical laminate (mother substrate) before being cut into chips, it is preferred that: the displacement of the unloading curve of the adhesive layer 21 is greater than 10 μm, and when the cutting process is performed by irradiating ultraviolet laser, the displacement of the unloading curve of the cut surface reaches less than 0.5 times.

[0128] In the chip of the optical laminate, in the central part of the surface of the adhesive layer 21, the indentation modulus is preferably 0.05 to 0.3 MPa, and more preferably 0.1 to 0.25 MPa. The indentation modulus of the end face of the adhesive layer 21 is preferably above 0.3 MPa, more preferably above 0.35 MPa, and further preferably above 0.4 MPa. The indentation modulus of the end face of the adhesive layer 21 is preferably 1.5 to 10 times the indentation modulus of the central part of the surface, more preferably 2 to 8 times, and further preferably 2.5 to 7 times. In other words, in the optical laminate (mother substrate) before being cut into chips, it is preferred that the indentation modulus of the adhesive layer 21 is 0.05 to 0.3 MPa, and when the cutting process is performed by irradiating an ultraviolet laser, the indentation modulus of the cut surface reaches 1.5 to 10 times.

[0129] As described above, when the gel fraction of the adhesive layer 21 is high and the adhesive is photocurable, there is a tendency that the effect of curing becomes greater than the effect of plasticization caused by molecular breakage during laser processing, the absolute value of the minimum load of the load curve based on the cut surface of the laser processing and the displacement of the unloading curve become smaller, and the indentation modulus becomes larger.

[0130] [Formation of display device]

[0131] The optical laminated body processed into a chip shape can be further laminated with other components as needed. Figure 4 In the chip of the optical laminate 104 shown, the release film 41 temporarily attached to the pressure-sensitive adhesive layer 21 can be peeled off and an adherend such as a cover window 80 can be attached to form an image display device.

[0132] After the cover window 80 is pasted on the first adhesive layer 21, heating, pressurization, decompression and other treatments may be performed to remove bubbles at the pasting interface and near the printing height difference. An autoclave treatment may be performed for the purpose of suppressing delay bubbles. When the adhesive layer 21 is a photocurable adhesive, the adhesive may be photocured after the cover window 80 is pasted on the adhesive layer 21. As described above, when the adhesive layer 21 is cut using an ultraviolet laser, the adhesive on the end face is sometimes partially photocured, but the adhesive in other areas is in an uncured state. By photocuring the adhesive layer 21, its bonding reliability to the adherend such as the cover window 80 can be improved.

[0133] Example

[0134] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples.

[0135] [Preparation of adhesive sheet]

[0136] <Production example 1>

[0137] (Preparation of base polymer)

[0138] In a reaction container, 139 parts by weight of ethyl acetate, 64 parts by weight of butyl acrylate (BA), 6 parts by weight of cyclohexyl acrylate (CHA), 10 parts by weight of isostearyl acrylate (ISA), 5 parts by weight of N-vinyl pyrrolidone (NVP) and 15 parts by weight of 4-hydroxybutyl acrylate (4HBA) as monomer components, and 0.2 parts by weight of azobisisobutyronitrile (AIBN) as a thermal polymerization initiator were added, and stirred for 1 hour in a nitrogen atmosphere at 23°C, and nitrogen replacement was performed. Thereafter, it was reacted at 65°C for 5 hours, and then at 70°C for 2 hours to prepare an acrylic base polymer solution. The weight average molecular weight of the obtained polymer was 450,000.

[0139] (Preparation of adhesive composition and production of adhesive sheet)

[0140] To the base polymer solution, 0.27 parts by weight of trimethylolpropane xylylene diisocyanate ("TAKENATE D110N" manufactured by Mitsui Chemicals, Inc.) as an isocyanate crosslinking agent, 2.5 parts by weight of polypropylene glycol (#400) diacrylate ("APG400" manufactured by Shin-Nakamura Chemical Co., Ltd.) as a multifunctional acrylate, 2.2 parts by weight of a mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate ("KAYARAD DPHA" manufactured by Nippon Kayaku Co., Ltd.), 0.22 parts by weight of "Ominirad 184" manufactured by IRM Resins Co., Ltd. as a photopolymerization initiator, and 0.33 parts by weight of "KBM-403" manufactured by Shin-Etsu Chemical Co., Ltd. as a silane coupling agent were added to 100 parts by weight of the polymer and uniformly mixed to prepare an adhesive composition (solution). The adhesive composition was applied on the release-treated surface of a separator having a thickness of 75 μm in a manner to achieve a thickness of 150 μm after drying, and after drying at 130° C. for 3 minutes to remove the solvent, the release-treated surface of another separator was overlapped on the adhesive layer to obtain an adhesive sheet A with separators attached to both sides at the same time.

[0141] <Production example 2>

[0142] (Preparation of base polymer)

[0143] In a reaction container, 139 parts by weight of ethyl acetate, 60 parts by weight of BA, 6 parts by weight of CHA, 1 part by weight of ISA, 18 parts by weight of NVP, and 15 parts by weight of 4HBA as monomer components, and 0.2 parts by weight of AIBN as a thermal polymerization initiator were added, and stirred for 1 hour in a nitrogen atmosphere at 23°C, and nitrogen replacement was performed. Thereafter, the reaction was allowed to proceed at 65°C for 5 hours, and then at 70°C for 2 hours to prepare an acrylic polymer solution. The weight average molecular weight of the obtained polymer was 300,000.

[0144] (Preparation of adhesive composition and production of adhesive sheet)

[0145] In the solution of the base polymer, 0.27 parts by weight of "TAKENATE D110N" as an isocyanate crosslinking agent, 1 part by weight of "APG400" and 2.2 parts by weight of "KAYARADDPHA" as multifunctional acrylates, 0.22 parts by weight of "Ominirad 651" manufactured by IRM Resins as a photopolymerization initiator, 0.02 parts by weight of "Tinuvin 384-2" manufactured by BASF as an ultraviolet absorber, and 0.33 parts by weight of "KBM-403" manufactured by Shin-Etsu Chemical Co., Ltd. as a silane coupling agent were added to 100 parts by weight of the polymer, and uniformly mixed to prepare an adhesive composition (solution). Using this adhesive composition, an adhesive sheet B having a thickness of 150 μm was prepared in the same manner as in Preparation Example 1.

[0146] <Production example 3>

[0147] In the preparation of the adhesive composition, the amount of the isocyanate crosslinking agent (TAKENATE D110N) was changed to 0.05 parts by weight, the amount of "APG400" was changed to 3 parts by weight, and the amount of "KAYARAD DPHA" was changed to 1 part by weight. The same operation as in Preparation Example 2 was performed to prepare an adhesive sheet C having a thickness of 150 μm.

[0148] <Production example 4>

[0149] In the preparation of the adhesive composition, the amount of the isocyanate crosslinking agent (TAKENATE D110N) was changed to 0.08 parts by weight, and the polyfunctional acrylate and the photopolymerization initiator were not added. A 150 μm thick adhesive sheet D was prepared in the same manner as in Preparation Example 2 except that the amount was changed to 0.08 parts by weight.

[0150] <Production example 5>

[0151] Using ethyl acetate as a solvent, 97 parts by weight of butyl acrylate (BA) and 3 parts by weight of acrylic acid (AA) were polymerized in the presence of a thermal polymerization initiator (AIBN) to obtain a solution of a polymer having a weight average molecular weight (Mw) of 1.1 million. In this solution, 0.8 parts by weight of trimethylolpropane toluene diisocyanate ("CORONATE L" manufactured by Tosoh Corporation) and 0.1 parts of a silane coupling agent ("KBM-403" manufactured by Shin-Etsu Chemical Co., Ltd.) as an isocyanate crosslinking agent were added to 100 parts by weight of the polymer, and the mixture was uniformly mixed to prepare an adhesive composition (solution). The composition was applied to the demoulding surface of a separator having a thickness of 38 μm in a manner to achieve a thickness of 20 μm after drying, and after drying at 100 ° C for 3 minutes to remove the solvent, the demoulding surface of another separator was overlapped on the adhesive layer, and heated at 50 ° C for 48 hours for crosslinking treatment to obtain an adhesive sheet P having a thickness of 30 μm with separators attached to both sides at the same time.

[0152] [Preparation of Laminated Body A]

[0153] Using a roll laminator, an adhesive sheet A was attached to one side (on the hard coating layer) of a polarizing plate having a thickness of about 75 μm, and an adhesive sheet P was attached to the other side, thereby obtaining a long polarizing plate with adhesives on both sides. As the polarizing plate, a triacetyl cellulose film (32 μm) provided with a hard coating layer was attached to one side of a polarizer formed of a stretched polyvinyl alcohol film having a thickness of 12 μm impregnated with iodine, and a triacetyl cellulose film (31 μm) provided with a phase difference layer was attached to the other side of the polarizer.

[0154] The release film on the surface of the adhesive sheet P was peeled off, and a polyimide film ("KAPTON EN100" manufactured by Toray DuPont) with a thickness of 25 μm was adhered to the surface of the adhesive sheet P using a roll-to-roller to obtain a laminate of polyimide film (25 μm) / adhesive sheet P (30 μm) / polarizing plate (75 μm) / adhesive sheet A (150 μm)) / separator (75 μm).

[0155] [Production of laminates B to D]

[0156] An optical laminate was prepared in the same manner as the laminate A except that adhesive sheets B to D were used instead of adhesive sheet A, wherein a polyimide film was adhered to one side of a polarizing plate with the aid of an adhesive sheet P with a thickness of 30 μm, and an adhesive sheet with a thickness of 150 μm was provided on the other side of the polarizing plate, and a release film was temporarily adhered thereto.

[0157] [Cutting of optical laminate]

[0158] The optical layered body was cut into a 40 mm×60 mm rounded rectangle (radius of curvature of the corner portion: 7 mm) by two methods.

[0159] <Knife-based cutting>

[0160] The optical stack was die cut using a Thomson knife.

[0161] <Cutting by UV laser>

[0162] The optical laminate was cut out by irradiating the polyimide film side with YAG third harmonic ultraviolet laser (wavelength 355 nm, frequency 40 Hz, output 0.4 W) while moving at a scanning speed of 10 mm / sec.

[0163] [evaluate]

[0164] <Gel Fraction of Adhesive>

[0165] Take about 1g of adhesive from adhesive sheets A to D, wrap it with a porous polytetrafluoroethylene membrane ("NTF-1122" manufactured by Nitto Denko Corporation) cut into a size of 100mm×100mm and with a pore diameter of 0.2μm, and tie the wrapping mouth with a kite string. Subtract the total weight (A) of the porous polytetrafluoroethylene membrane and the kite string measured in advance from the weight of the sample to calculate the weight (B) of the adhesive sample. The adhesive sample wrapped with the porous polytetrafluoroethylene membrane is immersed in about 50mL of ethyl acetate at 23°C for 7 days to dissolve the sol component of the adhesive outside the porous polytetrafluoroethylene membrane. After immersion, take out the adhesive wrapped with the porous polytetrafluoroethylene membrane, dry it at 130°C for 2 hours, and after natural cooling for about 20 minutes, measure the dry weight (C). The gel fraction of the adhesive is calculated by the following formula.

[0166] Gel fraction (%) = 100 × (CA) / B

[0167] For adhesive sheets A to C, the cumulative amount of light irradiated to the adhesive sheets was about 3000 mJ / cm 2 The adhesive was photocured by irradiating ultraviolet rays, and the gel fraction of the obtained adhesive was also measured.

[0168] <Nanoindentation Measurement of the End Surface of the Adhesive Layer>

[0169] The laminate of the embodiment and the comparative example was cut at a position 3 mm away from the end face to prepare a sample for measurement. The sample was fixed on the stage of the nanoindentation system ("TI950 TriboIndenter" manufactured by Hysitron) in such a way that the end face of the laminate became the measurement surface. Under an environment of a temperature of 25°C and a relative humidity of 50%, a conical-spherical indenter (radius of curvature at the front end: 10 μm) was used to press to a depth of 3000 nm at a load speed of 1000 nN / s, and then lifted at an unloading speed of 1000 nN / s for testing. The minimum load of the load curve, the indentation modulus, and the displacement of the unloading curve were obtained from the obtained load-displacement curve. The indentation modulus E is calculated using the following formula based on the slope of the unloading curve, the projected contact area A of the indenter, and the circumference π.

[0170] E=(S√π) / (2√A)

[0171] <Adhesion of the end surface>

[0172] A PET film with a thickness of 50 μm and no surface treatment was cut into a size of 5 mm × 10 mm and placed on a horizontal platform. The end face (cut face) of the optical laminate was pressed against the surface of the PET film and then lifted upward. Based on the bonding state between the end face of the optical laminate and the PET film at this time, the adhesion of the end face was evaluated according to the following criteria.

[0173] ○: The end surface of the optical laminate is not bonded to the PET film, and the optical laminate can be lifted without resistance.

[0174] △: When the optical laminate is lifted, the PET film is not lifted, but the peeling resistance between the end surface of the optical laminate and the PET film is felt.

[0175] ×: The end surface of the laminate and the PET film remain in a bonded state, and the PET film is lifted

[0176] <Pickup Test>

[0177] Ten single optical laminates were stacked in such a way that the surface on the polyimide film side was on the lower side. A suction cup was placed against the upper side (the surface on the release film side) of the stacked adhesive sheets to adsorb the laminate, and the laminate stacked on the top was lifted up with the suction cup for picking up. Whether only one optical laminate could be picked up was confirmed, and the pick-up property was evaluated according to the following criteria.

[0178] ○: Only one stacked body picked up is lifted

[0179] △: The stacked body directly below the stacked body being picked up was lifted, but then separated, and only one stacked body could be picked up.

[0180] ×: Two or more stacked bodies are lifted up as a whole and cannot be picked up one by one

[0181] Table 1 shows the gel fraction (before and after photocuring) of the pressure-sensitive adhesive of each of the optical laminates obtained above, the method of dicing into chips, and the evaluation results.

[0182] [Table 1]

[0183]

[0184] When the chips of stack A and stack B were cut out by punching, there was stickiness on the cut surface, resulting in poor pickup, but when the chips were cut out by ultraviolet laser processing, there was no stickiness on the end surface, showing good pickup. In stack A and stack B, the elastic modulus of the end surface processed by laser was larger than that of the end surface processed by punching, and the absolute value of the minimum load of the load curve and the displacement of the unloading curve became smaller. Based on these results, it can be considered that in the chips of stack A and stack B, the end surface was cured by laser processing, so the stickiness of the end surface of the adhesive layer was reduced.

[0185] In the laminate C using an adhesive having a small gel fraction before photocuring, both when the chips were cut out by punching and when the chips were cut out by laser processing, there was stickiness on the cut surface, resulting in poor pickup. In addition, the laminate D using an adhesive not having photocurability also had problems with pickup.

[0186] It can be seen that although the adhesive of laminate C is photocurable, the end surface is not cured even when cut by ultraviolet laser. On the contrary, when cut by laser, a decrease in elastic modulus and an increase in the displacement of the unloading curve (stringiness) are observed, indicating that plasticization has occurred. It can be considered that in laminate C, since the gel fraction of the adhesive is small, the influence of molecular breakage due to laser irradiation (generation of low molecular weight components) becomes the dominant factor, which is the cause of the softening of the adhesive.

[0187] In laminate D, the adhesive is not photocurable, but the displacement of the unloading curve is smaller when the chip is cut out by laser processing than when the chip is cut out by punching. Comparison between laminate C and laminate D shows that in order to obtain a laminate with no stickiness on the end surface of the adhesive layer by laser processing, it is important that the adhesive not only has photocurability but also has a large gel fraction.

[0188] Description of Reference Numerals

[0189] 10 Optical film (polarizing plate)

[0190] 11 polarizer

[0191] 13, 15 Transparent film

[0192] 21, 22 Adhesive layer

[0193] 41, 42, 43 Release film

[0194] 70 Image display unit (organic EL unit)

[0195] 71 Substrate (polyimide film)

[0196] 80 Covering Window

[0197] 101, 102, 103, 104, 105 Optical laminate

Claims

1. A method for producing an optical laminate, wherein: A mother substrate for an optical laminate is prepared, wherein the optical laminate comprises: a first adhesive layer having a first main surface and a second main surface; a first adherend attached to the first main surface of the first adhesive layer; and a second adherend attached to the second main surface of the first adhesive layer, The mother substrate is cut into chips with a size smaller than that of the mother substrate. The adhesive constituting the first adhesive layer contains a base polymer and further contains a monomer or oligomer having a photocurable functional group, or a compound having a photocurable functional group is bonded to the base polymer, so that the adhesive has photocurability. When the mother substrate is cut, the mother substrate is irradiated with ultraviolet laser to cut the optical laminate, and the first adhesive layer on the cut surface is photocured. In the optical laminate after dicing, the diced surface of the first pressure-sensitive adhesive layer has a minimum load of -0.2 μN or more in a load curve measured by nanoindentation and a displacement of 8 μm or less in an unloading curve.

2. The method for producing an optical layered body according to claim 1, wherein: In the optical layered body after the slicing process, the gel fraction of the adhesive in the center portion of the in-plane of the first adhesive layer is 25% or more.

3. The method for producing an optical layered body according to claim 1, wherein: In the optical laminate after dicing, the absolute value of the minimum load in the load curve of the diced surface of the first pressure-sensitive adhesive layer measured by nanoindentation is 0.3 times or less the absolute value of the minimum load in the load curve at the center of the surface.

4. The method for producing an optical layered body according to claim 1, wherein: In the optical laminate after slicing, the displacement of the unloading curve of the slicing surface of the first pressure-sensitive adhesive layer measured by nanoindentation is 0.5 times or less the displacement of the unloading curve of the center portion of the surface.

5. The method for producing an optical layered body according to claim 1, wherein: The adhesive further contains a photopolymerization initiator.

6. The method for producing an optical layered body according to claim 1, wherein: The gel fraction of the adhesive in the center portion of the first adhesive layer after photocuring is 70% or more.

7. The method for producing an optical layered body according to claim 1, wherein: The gel fraction of the adhesive in the center portion of the first adhesive layer after photocuring is 1.2 times or more of the gel fraction before photocuring.

8. The method for producing an optical layered body according to any one of claims 1 to 7, wherein: The first adhesive layer contains an ultraviolet absorber.

9. The method for producing an optical layered body according to any one of claims 1 to 7, wherein: The first adhesive layer has a thickness of 30 μm or more.

10. The method for producing an optical layered body according to any one of claims 1 to 7, wherein: The second adherend has a polarizing plate in contact with the first pressure-sensitive adhesive layer.

11. The method for producing an optical layered body according to claim 10, wherein: The second adherend further includes an image display unit adhered to the polarizing plate via a second adhesive layer.

12. The method for producing an optical layered body according to claim 11, wherein: The image display unit is an organic EL unit.

13. The method for producing an optical layered body according to claim 11, wherein: The image display unit includes a polyimide film.

14. The method for producing an optical layered body according to any one of claims 1 to 7, wherein: The first adherend is a release film releasably attached to the first pressure-sensitive adhesive layer.

Citation Information

Patent Citations

  • Polarizing plate and its production

    JP2000338329A

  • Polarizing film with adhesive layer and image display device

    JP2019179211A

  • Highly functional thin polarizing film and process for producing same

    WO2010100917A1

  • Optical film with adhesive and production method thereof, and method for producing image display device

    CN105505243A

  • Surface protection sheet

    CN107267080A