Prepregs, laminates and integrated moldings
By using the laminated structure of prepregs in fiber-reinforced composite materials and utilizing the combination of reinforced fibers and thermoplastic resins, the bonding time and strength issues in the manufacture of complex-shaped parts are solved, achieving efficient, high-speed molding and excellent structures. performance.
Patent Information
- Application Number
- CN202080084898.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-11
- Filing Date
- 2020-11-20
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-11-20
AI Technical Summary
When manufacturing parts with complex shapes using existing fiber-reinforced composite materials, mechanical joining methods lead to extended process times and reduced material strength; adhesive joining methods require long process times and insufficient joint strength; and the heat resistance of thermosetting resins and thermoplastic resins is poor. Insufficient chemical resistance.
A prepreg containing reinforcing fiber, an epoxy resin composition and a thermoplastic resin composition is used to form a laminate through chemical or physical combination of the reinforcing fiber and the thermoplastic resin across the boundary surface of the resin area to achieve efficient welding and excellent joint strength. .
It shortens the component joining process time, improves the molding speed and cost-effectiveness of structural components, and significantly improves the compressive strength and interlayer damage toughness. It is suitable for high-demand aircraft and other fields.
Smart Images

Figure CN114761468B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a prepreg in which reinforcing fibers are impregnated with epoxy resin and thermoplastic resin, and a laminate or an integrated molded product comprising epoxy resin, thermoplastic resin and reinforcing fibers. Background Art
[0002] For the fiber-reinforced composite material using thermosetting resin or thermoplastic resin as a matrix and combined with reinforcing fibers such as carbon fiber and glass fiber, it is lightweight, and has excellent mechanical properties such as strength and rigidity, heat resistance, and corrosion resistance, so it is used in many fields such as aerospace, automobiles, railway vehicles, ships, civil engineering and sports goods. However, these fiber-reinforced composite materials are not suitable for manufacturing parts and structures with complex shapes with a single molding process. In the above-mentioned uses, it is necessary to prepare parts formed by fiber-reinforced composite materials, and then integrate with the same or different parts. As a method for integrating fiber-reinforced composite materials containing reinforcing fibers and thermosetting resins with the same or different types, mechanical joining methods such as bolts, rivets, screws, and joining methods using adhesives can be used. In the mechanical joining method, since it is necessary to pre-process the process of the joining part such as the opening, the manufacturing process time becomes longer and the manufacturing cost increases. In addition, there is a problem that the material strength is reduced due to the opening. The bonding method using an adhesive requires a bonding step including preparation of the adhesive, application of the adhesive, and a curing step, which results in a long manufacturing process and a problem that reliability in terms of bonding strength cannot be fully satisfied.
[0003] For fiber-reinforced composite materials using thermoplastic resins in the matrix, in addition to the above-mentioned mechanical joining methods and joining using adhesives, a method of joining the parts by welding can also be applied, so there is a possibility that the time required for joining the parts can be shortened. On the other hand, in the case of mechanical properties at high temperatures and excellent resistance to chemicals such as aircraft structural parts, there is a problem that the heat resistance and chemical resistance are insufficient compared to fiber-reinforced composite materials formed of thermosetting resins and reinforcing fibers.
[0004] Here, Patent Document 1 discloses a method of joining a fiber-reinforced composite material composed of a thermosetting resin and reinforcing fibers with an adhesive.
[0005] Patent Document 2 shows a method for integrating a component formed of a thermoplastic resin and a component formed of a fiber-reinforced composite material formed of a thermosetting resin. That is, a thermoplastic resin film is laminated on the surface of a prepreg sheet formed of reinforcing fibers and a thermosetting resin, and the prepreg is heated and pressurized to obtain a fiber-reinforced composite material. Thereafter, the obtained fiber-reinforced composite material is placed in a mold, and a thermoplastic resin is injection molded, and the formed thermoplastic resin component and the fiber-reinforced composite material are joined by injection molding.
[0006] Patent Document 3 describes a method for producing a laminate having a thermoplastic resin adhesive layer formed on the surface of a composite material composed of a thermosetting resin and reinforcing fibers, and describes that the laminate exhibits an adhesive effect with other members via the thermoplastic resin.
[0007] Patent Document 4 describes a prepreg and a fiber-reinforced composite material thereof, wherein particles, fibers, or films made of a thermoplastic resin are arranged on the surface layer of a prepreg made of reinforcing fibers and a thermosetting resin.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2018-161801
[0011] Patent Document 2: Japanese Patent Application Laid-Open No. 10-138354
[0012] Patent Document 3: Japanese Patent No. 3906319
[0013] Patent Document 4: Japanese Patent Application Laid-Open No. 8-259713 Summary of the invention
[0014] Problems to be solved by the invention
[0015] However, since the method disclosed in Patent Document 1 is a method of bonding fiber-reinforced composite materials formed of reinforcing fibers and thermosetting resins to each other using an adhesive, and since the thermosetting resin is a matrix resin, welding cannot be directly applied as a method of bonding fiber-reinforced composite materials. Since the curing of the adhesive takes time, there is a problem that time is required in the bonding process, and the bonding strength exhibited is insufficient.
[0016] In the method described in Patent Document 2, the bonding strength at the bonding portion between the thermosetting resin and the thermoplastic resin film in the fiber-reinforced composite material is insufficient.
[0017] The fiber-reinforced composite material disclosed in Patent Document 3 can be integrated by welding with a thermoplastic resin and exhibits excellent bonding strength at room temperature, but has insufficient bonding strength at high temperatures.
[0018] Patent Document 4 shows that the interlaminar fracture toughness value is improved by using particles, fibers or films formed of a thermoplastic resin. However, in this method, the bonding strength at the boundary between the thermosetting resin and the thermoplastic resin in the fiber-reinforced composite material is insufficient.
[0019] Therefore, the object of the present invention is to provide a prepreg blank (which provides a laminate suitable as a structural material), a laminate and an integrated molded product, wherein the molded parts have excellent dimensional accuracy, can be joined with the same or different parts by welding, and exhibit excellent joining strength, and also have excellent compressive strength and interlaminar fracture toughness values.
[0020] Means for solving problems
[0021] In order to solve the above-mentioned problems, the prepreg of the present invention has the following constitution. That is, the prepreg comprises the following constituent elements [A], [B] and [C], wherein the above-mentioned [B] further comprises [B'], the ratio of the number of moles of active hydrogen contained in [B'] to the number of moles of epoxy groups of the epoxy resin contained in [B] is 0.6 or more and 1.1 or less, [C] is present on the surface of the prepreg, and in the prepreg, there is [A] which straddles the boundary surface between the resin region containing [B] and the resin region containing [C] and is in contact with the two resin regions.
[0022] [A] Reinforcement Fiber
[0023] [B] Epoxy resin composition
[0024] [B'] Amine compound
[0025] [C] Thermoplastic resin composition
[0026] In addition, the laminate of the present invention has any of the following structures. That is, a laminate in which at least a part of the layers is constituted by the cured product of the above-mentioned prepreg, or a laminate having the following structure. That is, a laminate comprising a layer comprising the following components [A], [C] and [D], wherein in the laminate, there is a reinforcing fiber [A] that crosses the boundary surface between the resin region comprising [C] and the resin region comprising [D] and is in contact with the two resin regions.
[0027] [A] Reinforcement Fiber
[0028] [C] Thermoplastic resin composition
[0029] [D] An epoxy resin cured product obtained by curing an epoxy resin composition comprising an epoxy resin and an amine compound, wherein the ratio of the number of moles of active hydrogen in the amine compound to the number of moles of epoxy groups in the epoxy resin is 0.6 or more and 1.1 or less.
[0030] It should be noted that, in this specification, when referred to as a "laminated body", it refers to any of these laminates according to the context, unless otherwise specified. In addition, as can be seen from this specification, the laminate of the present invention is typically a fiber-reinforced resin that can be produced by using a preform containing the prepreg of the present invention, but is not particularly limited.
[0031] Effects of the Invention
[0032] The prepreg and laminate of the present invention use a thermosetting resin and a thermoplastic resin, which are firmly bonded and can be well welded with the same or different parts, so that the time required in the bonding process can be shortened compared to the fiber-reinforced composite material formed by the conventional thermosetting resin and reinforcing fiber, and the molding of the structural parts can be accelerated. In addition, by controlling the epoxy resin, amine compound and the reactive group ratio used, excellent compressive strength and bonding strength are exhibited, and the dimensional accuracy of the obtained parts is also excellent, and an excellent laminate as a structural material can be obtained, and because it is suitable for aircraft structural parts, windmill blades, automobile structural parts, IC trays, notebook computer housings and other computer uses, etc., it shows excellent performance as a structure, and the molding time and molding cost of the products involved in the above uses can be greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] [ Figure 1 ] is a schematic diagram of a prepreg or laminate according to the present invention, and is a schematic diagram showing Figure 2 The diagram relates to a cross section perpendicular to the plane of the prepreg or the plane of the laminate.
[0034] [ Figure 2 ] is a schematic diagram of a cross section perpendicular to the plane of the prepreg blank or the plane of the laminate in the present invention, and is a diagram that helps to illustrate the method of measuring the average length RSm of roughness and the average height Rc of roughness. DETAILED DESCRIPTION
[0035] As the component [A] reinforcing fiber used in the present invention, there are glass fiber, carbon fiber, metal fiber, aromatic polyamide fiber, polyaramid fiber, aluminum oxide fiber, silicon carbide fiber, boron fiber, basalt fiber, etc. The above substances can be used alone or in combination of two or more. The above reinforcing fibers can be subjected to surface treatment. As surface treatment, there are metal deposition treatment, treatment using a coupling agent, treatment using a sizing agent, and additive adhesion treatment. It should be noted that in this specification, when such a surface treatment is applied to the reinforcing fibers, the reinforcing fibers in the state after the surface treatment are included and referred to as reinforcing fibers. The above reinforcing fibers also include reinforcing fibers with conductivity. As reinforcing fibers, carbon fibers are preferably used because they have a small specific gravity and are high in strength and elastic modulus.
[0036] Commercially available products of carbon fibers include "Torayca (registered trademark)" T800G-24K, "Torayca (registered trademark)" T800S-24K, "Torayca (registered trademark)" T700G-24K, "Torayca (registered trademark)" T700S-24K, "Torayca (registered trademark)" T300-3K, and "Torayca (registered trademark)" T1100G-24K (all manufactured by Toray Co., Ltd.).
[0037] The form and arrangement of the reinforcing fibers can be appropriately selected from the form and arrangement of reinforcing fibers arranged in one direction; a laminate of objects in which reinforcing fibers are arranged in one direction; or a woven form. However, in order to obtain a lightweight laminate with a higher level of durability, in each prepreg, it is preferred that the reinforcing fibers be arranged in one direction in the form of long fibers (fiber bundles) or continuous fibers such as woven fabrics.
[0038] The reinforcing fiber bundle may be composed of multiple fibers of the same form, or may be composed of multiple fibers of different forms. The number of reinforcing fibers constituting one reinforcing fiber bundle is usually 300 to 60,000, and if the manufacture of the substrate is considered, it is preferably 300 to 48,000, and more preferably 1,000 to 24,000. It may also be a range formed by a combination of any of the upper limits and any of the lower limits.
[0039] For the reinforcing fiber of component [A], if the strand tensile strength measured according to the resin impregnation strand test method of JIS R7608 (2007) is 5.5 GPa or more, a laminate having excellent bonding strength in addition to tensile strength can be obtained, which is preferred. If the strand tensile strength is 5.8 GPa, it is further preferred. The bonding strength mentioned here refers to the tensile shear bonding strength determined according to ISO4587:1995 (JIS K6850 (1994)).
[0040] In addition, as the component [A] reinforcing fiber, it is preferable to use a fiber having a surface free energy of 10 to 50 mJ / m as measured by the Wilhelmy method. 2 By controlling the surface free energy within this range, the reinforcing fibers exhibit high affinity with [B] the epoxy resin composition or [D] the epoxy resin cured product and [C] the thermoplastic resin, and exhibit high bonding strength in the boundary surface between the resin region containing [B] or [D] and the resin region containing [C] where the reinforcing fibers exist across. In addition, the aggregation of the reinforcing fibers is suppressed, the reinforcing fibers are well dispersed in the molded product, and the fluctuation (coefficient of variation) of the bonding strength is reduced. The surface free energy of the reinforcing fibers is preferably 15 to 40 mJ / m 2 , more preferably 18 to 35 mJ / m 2 .
[0041] As a method for controlling the surface free energy of the above-mentioned reinforcing fibers, there are: a method of controlling the surface by oxidizing the surface and adjusting the amount of oxygen-containing functional groups such as carboxyl and hydroxyl groups; a method of controlling the surface by attaching a single or multiple compounds to the surface. In the case of attaching multiple compounds to the surface, compounds with high surface free energy and compounds with low surface free energy can be attached in a mixed manner. The following is an explanation of the method for calculating the surface free energy of the reinforcing fibers. The surface free energy can be calculated by the following method: After measuring the contact angles of the reinforcing fibers relative to three solvents (purified water, ethylene glycol, and tricresyl phosphate), the surface free energy is calculated using the Owens approximation. The steps are shown below, but the measuring equipment and detailed methods are not necessarily limited to this.
[0042] Using DCAT11 manufactured by DataPhysics, first, take out a single fiber from the reinforcing fiber bundle, cut it into 8 pieces with a length of 12±2mm, and then paste them in parallel on a special holder FH12 (a flat plate coated with an adhesive material) with a distance of 2 to 3mm between the single fibers. Then, cut the front end of the single fiber and set it in the holder DCAT11. During the measurement, bring the cell containing each solvent close to the lower end of the 8 single fibers at a speed of 0.2mm / s and immerse until 5mm from the front end of the single fiber. Then, lift the single fiber at a speed of 0.2mm / s. Repeat this operation more than 4 times. Use an electronic balance to measure the force F exerted on the single fiber when immersed in the liquid. Use this value and the following formula to calculate the contact angle θ.
[0043] COSθ = (force F (mN) on 8 single fibers) / ((8 (number of single fibers) × circumference of single fiber (m) × surface tension of solvent (mJ / m 2 ))
[0044] The measurement was performed on single fibers extracted from three different locations of the reinforcing fiber bundle. That is, the average value of the contact angles of a total of 24 single fibers was calculated for one reinforcing fiber bundle.
[0045] Surface free energy of reinforcing fibersγ f As the polar component of surface free energy γ p f , and the nonpolar component of the surface free energy γ d f Calculate the sum.
[0046] The polar component of surface free energy γ p f For example, the surface tension components and contact angles of each liquid are substituted into the Owens approximation shown below (a formula consisting of the polar and non-polar components of the surface tension inherent in each solvent and the contact angle θ), and then plotted on X and Y. The square of the slope a when the linear approximation is performed using the least squares method is used to obtain the non-polar component γ of the surface free energy. d f Calculated from the square of the intercept b. The surface free energy γf of the reinforcing fiber is the sum of the square of the slope a and the square of the intercept b.
[0047] Y=a·X+b
[0048] X=√(Polar component of the solvent surface tension (mJ / m 2 )) / √(Non-polar component of the solvent surface tension (mJ / m 2 )
[0049] Y = (1 + COSθ) (polar component of the surface tension of the solvent (mJ / m 2 )) / 2√(non-polar component of the solvent surface tension (mJ / m 2 )
[0050] Polar component of the surface free energy of the reinforcing fiber γ p f =a 2
[0051] Nonpolar component of the surface free energy of reinforcing fibersγ d f =b 2
[0052] Total surface free energy γ f =a 2 +b 2
[0053] The polar component and nonpolar component of the surface tension of each solvent are shown below.
[0054] Purified water
[0055] Surface tension 72.8mJ / m 2 , polar component 51.0mJ / m 2 , non-polar component 21.8 (mJ / m 2 )
[0056] Ethylene glycol
[0057] Surface tension 48.0mJ / m 2 , polar component 19.0mJ / m 2 , non-polar component 29.0 (mJ / m 2 )
[0058] Tricresyl phosphate
[0059] Surface tension 40.9mJ / m 2 , polar component 1.7mJ / m 2 , non-polar component 39.2 (mJ / m 2 )
[0060] Regarding component [B] (the "epoxy resin composition" as component [B] in this specification refers to a resin composition containing more than 50% by mass of epoxy resin and exhibiting the behavior of a thermosetting resin as a whole) used in the present invention and comprising component [B'] an amine compound, the average epoxy value of all epoxy resins contained therein is calculated as follows when the two components, epoxy resin 1 and epoxy resin 2, are included as an example.
[0061] Average epoxy value (meq. / g) = (mass fraction of epoxy resin 1 / epoxy equivalent of epoxy resin 1 + mass fraction of epoxy resin 2 / epoxy equivalent of epoxy resin 2) / (mass fraction of epoxy resin 1 + mass fraction of epoxy resin 2) × 1000
[0062] Here, epoxy equivalent refers to the value obtained by the method described in JIS K7236 (2009). By making the average epoxy value of all epoxy resins included be more than 6.0meq. / g and less than 11.0meq. / g, the calorific value during molding can be controlled, the unevenness of the degree of cure is suppressed, and thus a laminate showing excellent flatness can be obtained. In addition, as a laminate, excellent compressive strength is shown, so it is preferred. In addition, the average epoxy value of all epoxy resins included is more than 7.5meq. / g and less than 9.0meq. / g, which is a more preferred mode. It can be a range formed by a combination of any one of the above-mentioned upper limits and any one of the lower limits.
[0063] In addition, the average amine value of all the included amine compounds is calculated as follows when two components, amine compound 1 and amine compound 2, are included as an example.
[0064] Average amine value (meq. / g) = (mass fraction of amine compound 1 / active hydrogen equivalent of amine compound 1 + mass fraction of amine compound 2 / active hydrogen equivalent of amine compound 2) / (mass fraction of amine compound 1 + mass fraction of amine compound 2) × 1000
[0065] Here, the active hydrogen equivalent refers to the active hydrogen equivalent calculated by identifying the chemical structure and its ratio using liquid chromatography mass spectrometry (LC / MS method). By making the average amine value of all the amine compounds contained above 5.0 meq. / g and below 20.0 meq. / g, the heat generation during molding can be controlled, and the unevenness of the degree of cure can be suppressed, thereby being able to obtain a laminate showing excellent flatness, so it is a preferred method. Among them, in order to obtain a laminate with excellent flatness, it is also important to set the epoxy value of the above-mentioned epoxy resin to a certain value or above, or to set the amount of active hydrogen contained in [B'] to a certain value or above relative to the amount of epoxy groups contained in [B] as described below to suppress the unevenness of the degree of cure of the epoxy resin cured product.
[0066] The number of moles of epoxy groups in the epoxy resin contained in the component [B] is calculated as follows.
[0067] The number of moles of epoxy groups in epoxy resin = the mass fraction of epoxy resin / the epoxy equivalent of epoxy resin
[0068] When component [B] contains two or more epoxy resins, the molar number of the epoxy group of each component is the sum. As an example, when the epoxy resin contains two components (component 1 and component 2), it is calculated as follows.
[0069] The number of moles of epoxy groups in the epoxy resin = the mass fraction of component 1 / the epoxy equivalent of component 1 + the mass fraction of component 2 / the epoxy equivalent of component 2
[0070] The number of moles of active hydrogen in the amine compound of the component [B′] is calculated as follows.
[0071] The number of moles of active hydrogen in the amine compound = the mass fraction of the amine compound / the active hydrogen equivalent of the amine compound
[0072] In the case where the constituent element [B'] includes an amine compound of more than 2 components, the sum of the moles of active hydrogen of each component is calculated in the same manner as the moles of epoxy groups. By making the ratio of the moles of active hydrogen contained in [B'] to the moles of epoxy groups contained in [B] to be 0.6 or more and 1.1 or less, as a laminate, excellent compression strength is shown, and the calorific value during curing decreases, and the uneven degree of curing of the epoxy resin cured product decreases, so as to show excellent flatness as a laminate. In addition, the residual epoxy group interacts with the constituent element [C] thermoplastic resin, so as to show excellent bonding strength as an integrated molded product. The ratio of the moles of active hydrogen contained in [B'] to the moles of epoxy groups contained in [B] is more preferably 0.65 or more and 0.95 or less. It can be a range formed by a combination of any one of the above-mentioned upper limits and any one of the lower limits.
[0073] The component [D] epoxy resin cured product in the laminate of the present invention is typically obtained by heat curing the component [B] epoxy resin composition containing the component [B'] amine compound in the prepreg of the present invention. The above temperature conditions can be appropriately set according to the type of epoxy resin and the type and amount of the amine compound and accelerator. For example, when diaminodiphenyl sulfone is used as the amine compound, a temperature condition of 180°C for 2 hours can be appropriately used, and when dicyandiamide is used as the amine compound, a temperature condition of 135°C for 2 hours can be appropriately used.
[0074] Examples of the epoxy resin used in component [B] include bisphenol-type epoxy resins such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol AD-type epoxy resins, and bisphenol S-type epoxy resins, brominated epoxy resins such as tetrabromobisphenol A diglycidyl ether, epoxy resins having a biphenyl skeleton, epoxy resins having a naphthalene skeleton, epoxy resins having a dicyclopentadiene skeleton, phenol Novolac-type epoxy resins, cresol Novolac-type epoxy resins, and other Novolac-type epoxy resins, N,N,O-triglycidyl-m-aminophenol, N,N, Glycidylamine type epoxy resins such as O-triglycidyl p-aminophenol, N,N,O-triglycidyl-4-amino-3-methylphenol, N,N,N',N'-tetraglycidyl-4,4'-methylenedianiline, N,N,N',N'-tetraglycidyl-2,2'-diethyl-4,4'-methylenedianiline, N,N,N',N'-tetraglycidyl m-phenylenediamine, N,N-diglycidyl aniline, N,N-diglycidyl o-toluidine, resorcinol diglycidyl ether, triglycidyl isocyanurate, etc.
[0075] The component [B] of the present invention contains 40 to 100 parts by mass of a glycidylamine epoxy resin containing three or more glycidyl groups relative to 100 parts by mass of the total epoxy resin contained, so that a cured product with high heat resistance can be obtained, which is a more preferred embodiment, and it is further preferred to contain 80 to 100 parts by mass. Examples of the glycidylamine epoxy resin containing three or more glycidyl groups include N,N,O-triglycidyl-m-aminophenol, N,N,O-triglycidyl-p-aminophenol, N,N,O-triglycidyl-4-amino-3-methylphenol, N,N,N',N'-tetraglycidyl-4,4'-methylenedianiline, N,N,N',N'-tetraglycidyl-2,2'-diethyl-4,4'-methylenedianiline, and N,N,N',N'-tetraglycidyl-m-xylylenediamine.
[0076] Examples of the amine compound used in the component [B′] include dicyandiamide, aromatic amine compounds, tetramethylguanidine, and thiourea-added amines.
[0077] Among them, by using an aromatic amine compound as the [B'] amine compound, an epoxy resin having good heat resistance can be obtained. Examples of the aromatic amine compound include 3,3'-diisopropyl-4,4'-diaminodiphenyl sulfone, 3,3'-di-tert-butyl-4,4'-diaminodiphenyl sulfone, 3,3'-diethyl-5,5'-dimethyl-4,4'-diaminodiphenyl sulfone, 3,3'-diisopropyl-5,5'-dimethyl-4,4'-diaminodiphenyl sulfone, 3,3'-di-tert-butyl-5,5'-dimethyl-4,4'-diaminodiphenyl sulfone, 3,3',5,5'-tetraethyl-4,4'-diaminodiphenyl sulfone, 3,3'-diisopropyl-5,5'-diethyl-4,4'-diaminodiphenyl sulfone, 3,3'-di-tert-butyl-5,5'-diethyl-4,4'-diaminodiphenyl sulfone, 3,3',5,5'-tetraisopropyl-4,4'-diaminodiphenyl sulfone, 3,3'-di-tert-butyl-5,5'-diisopropyl-4,4'-diaminodiphenyl sulfone, 3,3',5,5'-tetra-tert-butyl-4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, etc.
[0078] In the epoxy resin composition [B] of the present invention, the amine compound [B'] is the main component of the curing agent, but other curing agents or curing accelerators may also be included. The mass of [B'] is preferably 80% or more relative to the total mass of the curing agent and the curing accelerator contained in the epoxy resin composition [B]. Examples of other curing agents include acid anhydrides, phenol Novolac compounds, etc., and examples of curing accelerators include phosphorus-based curing accelerators such as triphenylphosphine and tetraarylphosphonium tetraarylborate, cationic polymerization initiators, tertiary amines, imidazole compounds, urea compounds, etc.
[0079] In addition, the epoxy resin composition of component [B] preferably contains a thermoplastic resin component soluble in epoxy resin as a viscosity modifier in a dissolved state. The thermoplastic resin component is another thermoplastic resin component different from the thermoplastic resin contained in component [C]. Here, the so-called "soluble in epoxy resin" means that there is a temperature range in which a uniform phase is formed by heating the resin obtained by mixing the thermoplastic resin component with the epoxy resin, or heating and stirring. Here, "forming a uniform phase" means that a state in which no separation can be obtained under visual observation. Here, "dissolved state" means that the epoxy resin containing the thermoplastic resin component is placed in a certain temperature range and becomes a uniform phase. Once it becomes a uniform phase in a certain temperature range, it does not matter even if separation occurs outside the temperature range, for example at room temperature.
[0080] As a thermoplastic resin component soluble in the epoxy resin of the constituent element [B], in general, a thermoplastic resin having a bond selected from the group consisting of a carbon-carbon bond, an amide bond, an imide bond, an ester bond, an ether bond, a carbonate bond, a carbamate bond, a thioether bond, a sulfone bond and a carbonyl bond in the main chain is preferred. In addition, for the thermoplastic resin component, it is also possible to partially have a cross-linked structure, and it may be crystalline or amorphous. In particular, it is suitable to be at least one resin selected from the group consisting of polyamide, polycarbonate, polyoxymethylene, polyphenylene ether, polyphenylene sulfide, polyarylate, polyester, polyamide-imide, polyimide, polyetherimide, polyimide having a phenyltrimethylindane structure, polysulfone, polyethersulfone, polyetherketone, polyetheretherketone, polyarylamide, polyvinyl formal, polyvinyl butyral, phenoxy resin, polyether nitrile and polybenzimidazole. In order to obtain good heat resistance, the glass transition temperature is preferably 150° C. or higher, more preferably 170° C. or higher, from the viewpoint of being less likely to cause thermal deformation when used as a molded body. Polyetherimide and polyethersulfone are suitable examples.
[0081] The thermoplastic resin constituting component [C] (the "thermoplastic resin composition" as component [C] in this specification refers to a resin composition containing more than 50% by mass of a thermoplastic resin and exhibiting the behavior of a thermoplastic resin as a whole) is not particularly limited, and examples thereof include polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, polyethylene naphthalate, and liquid crystal polyesters, and polyethylene , polyolefins such as polypropylene and polybutene, styrene resins, polyurethane resins, and polyamides such as polyoxymethylene, polyamide 6, and polyamide 66, polycarbonates, polymethyl methacrylates, polyvinyl chloride, polyphenylene sulfide, polyphenylene ether, modified polyphenylene ether, polyimide, polyamide-imide, polyetherimide, polysulfone, modified polysulfone, polyethersulfone, polyketone, polyetherketone, polyetheretherketone, polyetherketoneketone, polyarylene etherketone, polyarylate, polyether nitrile, phenolic resins, phenoxy resins, etc. In addition, the above-mentioned thermoplastic resins can be copolymers, modified products, and / or resins obtained by blending two or more of the above-mentioned resins. Among these, from the viewpoint of heat resistance, it is preferred that component [C] contains 60% by mass or more of one or more of polyarylene etherketone, polyphenylene sulfide, or polyetherimide. In order to improve impact resistance, an elastomer or rubber component can be added. In addition, other fillers and additives may be appropriately contained within the range not impairing the purpose of the present invention according to the application, etc. For example, inorganic fillers, flame retardants, conductivity imparting agents, crystal nucleating agents, ultraviolet absorbers, antioxidants, vibration damping agents, antibacterial agents, insect repellents, deodorants, anti-coloring agents, heat stabilizers, mold release agents, antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, foaming agents, coupling agents, etc. may be mentioned.
[0082] The thermoplastic resin contained in component [C] is preferably a preferred embodiment because it has a functional group reactive with an epoxy group at the terminal or in the main skeleton, thereby forming a covalent bond with the remaining epoxy group by chemical reaction, thereby exhibiting excellent bonding strength as an integrated molded article. Examples of the functional group reactive with an epoxy group include a carboxyl group, an amino group, a hydroxyl group, an isocyanate group, and the like.
[0083] In the prepreg of the present invention, there is a reinforcing fiber [A] that crosses the boundary surface between the resin region containing [B] and the resin region containing [C] and is in contact with the two resin regions. By the presence of the reinforcing fiber [A] that crosses the boundary surface between the resin region containing the component [B] and the resin region containing the component [C] and is in contact with the two resin regions, [A] is chemically or / and physically bonded to [B] and [C], and the resin region containing [B] and the resin region containing [C] are not easily peeled off, thereby showing excellent bonding strength. The component [A] present on the boundary surface is chemically or / and physically bonded to the component [B] and the component [C], thereby improving the adhesion between the resin region containing the component [B] and the resin region containing the component [C].
[0084] In the prepreg of the present invention, it is preferred that the resin region containing [B] and the resin region containing [C] are each formed in a layered manner and are adjacent to each other. Figure 1 is a schematic diagram of a prepreg or laminate according to the present invention, Figure 2 yes Figure 1 The schematic diagram of the cross section perpendicular to the prepreg plane or the laminate plane shown as the cross-sectional observation plane 5 in FIG. 1 is useful for explaining the method of measuring the roughness average length RSm and the roughness average height Rc.
[0085] In the prepreg of the present invention, the term "formed in layers and adjacent to each other" means, for example, Figure 2 As shown, in the cross section cut perpendicularly to the plane direction of the prepreg, the resin region 7 containing [C] and the resin region 8 containing [B] which are continuous in the plane direction are in a state of being closely present while forming a boundary surface 10. In the case where the resin region 7 containing [C] is not in a continuous layered state but exists in a particle form, a fiber form, a nonwoven fabric form, etc., the ratio of the surface area where the epoxy resin contained in [B] is exposed increases, and the coverage of [C] on the outermost surface decreases, so there is a tendency for the weldability to decrease.
[0086] Furthermore, from the perspective of improving the bonding strength, when the prepreg is viewed from above, in a cross section perpendicular to the plane of the prepreg containing the fibers of [A] existing across the above-mentioned two resin regions, obtained from a direction that differs by 45 degrees (whether clockwise or counterclockwise) with respect to the fiber direction of any [A] that is in contact with the above-mentioned two resin regions, that is, in a cross section obtained by cutting perpendicularly with respect to the plane direction of the prepreg, it is preferred that the roughness average length RSm defined by JIS B0601 (2001) of the cross-sectional curve formed by the boundary surface of the two resins is less than 100 μm and the roughness average height Rc is greater than 3.5 μm.
[0087] When the roughness average length RSm is less than 100 μm, not only chemical and / or physical bonding forces exist, but also mechanical bonding forces such as interweaving are superimposed, and the resin region containing component [B] and the resin region containing component [C] become difficult to peel off. The lower limit is not particularly limited, but from the perspective of avoiding the reduction of mechanical bonding forces caused by stress concentration, it is preferably 15 μm or more. In addition, by making the roughness average height Rc of the cross-sectional curve greater than 3.5 μm, not only the mechanical bonding forces caused by interweaving will appear, but also the component [A] on the boundary surface is chemically or / and physically combined with the component [B] and the component [C], and the adhesion between the resin region containing component [B] and the resin region containing component [C] is improved. The preferred range of the roughness average height Rc of the cross-sectional curve is 10 μm or more (component [A] becomes easy to be included in the above two resin regions and the adhesion is further improved), and particularly preferably 20 μm or more. The upper limit is not particularly limited, but is preferably 100 μm or less from the viewpoint of avoiding a decrease in mechanical bonding strength due to stress concentration.
[0088] Here, as a method for measuring the roughness average height Rc and the roughness average length RSm of the cross-sectional curve, a known method can be used. For example, after the component [B] is solidified, a method for measuring the cross-sectional image obtained using X-ray CT, a method for measuring the element analysis distribution image using an energy dispersive X-ray spectrometer (EDS), or a method for measuring the cross-sectional observation image using an optical microscope or a scanning electron microscope (SEM) or a transmission electron microscope (TEM). During the observation, in order to adjust the contrast, the component [B] and / or the component [C] can also be stained. In the image obtained by any of the above methods, the roughness average height Rc and the roughness average length RSm of the cross-sectional curve are measured within a range of 500 μm square.
[0089] use Figure 2An example of a method for measuring the roughness average height Rc and the roughness average length RSm of a cross-sectional curve is shown below. Figure 2 In the observed image 9 shown in FIG. 1 , the resin region 7 including the component [C] and the resin region 8 including the component [B] are closely attached to each other and are shown as a boundary surface 10 in the observed image 9 . In addition, a plurality of components [A] 6 are present on the boundary surface 10 .
[0090] An example of a method for measuring the roughness average height Rc and the roughness average length RSm of a cross-sectional curve is shown (method 1 for measuring cross-sectional curve elements). The end of the rectangular observation image 9 on the side of the resin region 8 containing the component [B] is used as the reference line 11, and a vertical baseline 12 is drawn at intervals of 5 μm from the resin region 8 containing the component [B] to the resin region 7 containing the component [C]. The point where the vertical baseline 12 drawn from the reference line 11 first intersects with the component [C] is plotted, and the line connecting the plotted points is set as the cross-sectional curve 13. The obtained cross-sectional curve 13 is screened based on JIS B0601 (2001) to calculate the roughness average height Rc and the roughness average length RSm of the cross-sectional curve 13.
[0091] The thermoplastic resin component [C] in the prepreg of the present invention preferably has a weight per unit area of 10 g / m 2 If 10g / m 2 More preferably, it is 20 g / m 2 The upper limit is not particularly limited, but is preferably 500 g / m 2 This is because the amount of the thermoplastic resin does not become too much compared to the reinforcing fiber, and a laminate having excellent specific strength and specific elastic modulus can be obtained. 2 The mass (g) of the component [C] contained in the prepreg.
[0092] The prepreg of the present invention preferably has a reinforcing fiber content of 30 to 2,000 g / m2 per unit area. 2 If the amount of reinforcing fiber is 30g / m 2 If the amount of reinforcing fiber is 2,000 g / m 2 Below, the drapability of the prepreg becomes easy to improve.
[0093] The reinforcing fiber mass content of the prepreg of the present invention is preferably 30 to 90% by mass, more preferably 35 to 85% by mass, and further preferably 40 to 80% by mass. It can be a range formed by a combination of any one of the above upper limits and any one of the lower limits. When the reinforcing fiber mass content is 30% by mass or more, the amount of resin does not become too much compared to the fiber, and it is easy to obtain the advantages of a laminate with excellent specific strength and specific elastic modulus. In addition, when the laminate is formed, the heat generation during curing is not easy to become excessively high. In addition, when the reinforcing fiber mass content is 90% by mass or less, poor impregnation of the resin is not likely to occur, and the voids of the obtained laminate are easy to become less.
[0094] Another aspect of the present invention is a laminated body produced by a method of curing a preform in which at least one layer is composed of the prepreg of the present invention, i.e., a laminated body in which at least one layer is composed of a cured product of the prepreg of the present invention, the preformed body being produced by laminating a plurality of the prepregs of the present invention or laminating the prepreg of the present invention together with other prepregs other than the prepreg of the present invention. Here, as a method of applying heat and pressure, for example, a press molding method, an autoclave molding method, a bag molding method, a tape wrapping method, an internal pressure molding method, etc. can be used.
[0095] Alternatively, another aspect of the present invention is a laminate comprising a layer including components [A], [C], and [D], and having reinforcing fibers [A] that straddle a boundary surface between a resin region including [C] and a resin region including [D] and are in contact with both resin regions.
[0096] When looking down at the prepreg, the cross section perpendicular to the plane of the laminate containing [A] existing across the above two resin regions is obtained from the direction of the fiber direction of any [A] connected to the above two resin regions at a difference of 45 degrees (whether clockwise or counterclockwise), that is, the cross section obtained by cutting perpendicularly to the plane direction of the laminate, the cross-sectional curve formed by the close boundary surface of the two resin regions is defined by JIS B0601 (2001) as being less than 100 μm, and the roughness average height Rc is preferably 3.5 μm or more. The roughness average height Rc is further preferably more than 10 μm. The lower limit of RSm and the upper limit of Rc are not particularly limited. From the perspective of the possibility of reduced mechanical bonding force caused by stress concentration, RSm is preferably more than 15 μm, and Rc is preferably less than 100 μm.
[0097] The roughness average height Rc and the roughness average length RSm of the cross-sectional curve can be determined by the above-mentioned method in the same manner as the measurement method for the prepreg of the present invention.
[0098] As a method for molding the laminate of the present invention, it can be prepared by molding methods such as press molding, autoclave molding, bag mold molding, tape winding, internal pressure molding, hand lay-up molding, filament winding, pultrusion, resin injection molding, and resin transfer molding.
[0099] In the laminate of the present invention, it is preferred that the component [C] thermoplastic resin composition is present on the surface, that is, the laminate has a layer comprising [A], [C] and [D] as the outermost layer, and [C] is exposed. It is further preferred that the component [C] is present on both the surface and the inside of the laminate of the present invention, that is, the laminate also has a layer comprising [A], [C] and [D] as the inner layer. By having the component [C] thermoplastic resin on the surface of the laminate, the laminate of the present invention can be joined to the same or different parts by welding via the component [C]. On the other hand, when the component [C] thermoplastic resin is also present inside the laminate, an excellent interlaminar fracture toughness value (G IIC ).
[0100] For the laminate of the present invention, some heating means can be utilized to make other parts, i.e. parts of the same kind and / or different kinds as the parts constituting the laminate (adherends) be joined with the surface having [C], especially the constituent element [C] existing on the surface of the laminate, and be integrated (welded) with the laminate via the constituent element [C], thereby making an integrated molded product. As different kinds of parts (adherends), parts formed by thermoplastic resins and parts formed by metal materials can be cited. In the parts formed by thermoplastic resins, reinforcing fibers, fillers, etc. can be included. The integration method is not particularly limited, for example, heat welding, vibration welding, ultrasonic welding, laser welding, resistance welding, induction welding, insert injection molding, injection molding on substrate, etc. can be cited.
[0101] The strength of the joint of the integrated molded product can be evaluated based on ISO4587:1995 (JIS K6850 (1994)). The tensile shear bonding strength measured based on ISO4587:1995 is preferably 25 MPa or more, more preferably 28 MPa or more. Generally speaking, if it is 20 MPa or more, the laminate can be used as a bonding material for structural materials, and it is also high strength compared to the tensile shear bonding strength (about 10 MPa) of a conventional adhesive at a test environment temperature of 23°C. The higher the tensile shear bonding strength, the more preferred it is. There is no particular upper limit. In a conventional integrated molded product of a laminate, the tensile shear bonding strength is upper limited to 200 MPa.
[0102] The laminate of the present invention is preferably used for aircraft structural parts, wind turbine blades, automobile outer panels and IC trays, computer applications such as notebook computer housings, and sports applications such as golf clubs and tennis rackets.
[0103] Example
[0104] Hereinafter, the present invention will be described in detail using examples. However, the scope of the present invention is not limited to these examples. It should be noted that, for the unit "part" of the composition ratio, it refers to mass parts unless otherwise noted. In addition, for the measurement of various properties, unless otherwise specified, it is carried out under an environment of a temperature of 23° C. and a relative humidity of 50%.
[0105] <Materials used in Examples and Comparative Examples>
[0106] The following components [A], [B], [B'], and [C] were used. The components used in each example and comparative example are shown in Tables 1 to 3.
[0107] Component [A]: Reinforcement fiber
[0108] After obtaining a common carbon fiber bundle as a raw material by the following method, various sizing agent compounds were applied to obtain it. First, an acrylonitrile copolymer copolymerized with itaconic acid was spun and calcined to obtain a total of 24,000 filaments with a specific gravity of 1.8 g / cm 3 , a carbon fiber bundle with a bundle tensile strength of 4.9 GPa and a bundle tensile elastic modulus of 230 GPa. Then, various sizing agent compounds are mixed with acetone to obtain a solution of about 1% by mass in which the compound is uniformly dissolved. Each compound is applied to the above-mentioned carbon fiber bundle by an immersion method, and then heat-treated at 210°C for 90 seconds. The attachment amount of each compound is adjusted to 0.5 parts by mass relative to 100 parts by mass of carbon fiber to which each compound is attached. The sizing agent compounds used in each carbon fiber and the surface free energy after sizing agent coating are as follows.
[0109] CF1: polyethylene glycol diglycidyl ether ("Denacol" (registered trademark) EX-841, manufactured by Nagase ChemteX Co., Ltd.), surface free energy: 20 mJ / m 2
[0110] CF2: bisphenol A diglycidyl ether ("jER" (registered trademark) 828, manufactured by Mitsubishi Chemical Corporation), surface free energy: 9 mJ / m 2
[0111] CF3: sorbitol polyglycidyl ether ("Denacol" (registered trademark) EX-614B, manufactured by Nagase ChemteX Co., Ltd.), surface free energy: 32 mJ / m 2
[0112] Thermoplastic resin contained in component [C]
[0113] PA6: Polyamide 6 ("Amilan" (registered trademark) CM1007 (Toray Co., Ltd., melting point 225°C, terminal functional groups: amino group, carboxyl group)) with a unit weight of 120 g / m 2 membrane
[0114] PPS: polyphenylene sulfide ("Torelina" (registered trademark) A670T05 (manufactured by Toray Industries, Ltd., melting point 278°C, glass transition temperature 90°C, terminal functional group: carboxyl group)) with a unit weight of 120 g / m 2 membrane
[0115] PEKK1: Polyetherketoneketone ("KEPSTAN" (registered trademark) 6002 (produced by Arkema, melting point 300°C, glass transition temperature 160°C, terminal functional group: carboxyl group)) with a unit weight of 120 g / m 2 membrane
[0116] PEKK2: Polyetherketoneketone ("KEPSTAN" (registered trademark) 7002 (produced by Arkema, melting point 331°C, glass transition temperature 162°C, terminal functional group: carboxyl group)) with a unit weight of 120 g / m 2 membrane
[0117] ·PEEK: Polyetheretherketone (PEEK 450G (Victrex, melting point 343°C, glass transition temperature 143°C, terminal functional group: hydroxyl group)) with a unit weight of 120 g / m 2 membrane
[0118] · Semi-aromatic PA: Made of polyamide 6T (melting point 320°C, glass transition temperature 125°C, terminal functional groups: amino, carboxyl)) with a unit weight of 120 g / m 2 membrane
[0119] PES1: Polyethersulfone ("Sumikaexcel" (registered trademark) 5003P manufactured by Sumitomo Chemical Co., Ltd., glass transition temperature 225°C, terminal functional group: hydroxyl group), unit weight 120 g / m 2 membrane
[0120] PES2: Polyethersulfone ("Sumikaexcel" (registered trademark) 3600P manufactured by Sumitomo Chemical Co., Ltd., glass transition temperature 225°C, terminal functional group: chlorine group) with a unit weight of 120 g / m 2 membrane
[0121] <Method for measuring melting point of thermoplastic resin>
[0122] The melting point of the thermoplastic resin is measured using a differential scanning calorimeter (DSC) based on JIS K7121 (2012). When a plurality of melting points are observed in a mixture or the like, the highest melting point is adopted as the melting point of the thermoplastic resin.
[0123] <Method for producing and evaluating epoxy resin composition>
[0124] The epoxy resin compositions of the specific examples described in Table 1 were prepared using the following compounds.
[0125] (1) Epoxy resin contained in component [B]
[0126] Tetraglycidyldiaminodiphenylmethane ("Araldite" (registered trademark) MY721, manufactured by Huntsman Advanced Materials, epoxy equivalent: 113 (g / eq.), tetrafunctional glycidylamine type epoxy resin)
[0127] Aminophenol type epoxy resin ("Araldite" (registered trademark) MY0500, manufactured by Huntsman Advanced Materials, epoxy equivalent: 100 (g / eq.), trifunctional glycidylamine type epoxy resin)
[0128] Bisphenol A type epoxy resin ("jER" (registered trademark) 825, manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: 175 (g / eq.))
[0129] Bisphenol A type epoxy resin ("jER" (registered trademark) 1001, manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: 475 (g / eq.))
[0130] (2) Component [B']: Amine compound
[0131] ·4,4'-Diaminodiphenyl sulfone (Seikacure S, manufactured by Wakayama Seika Industries, Ltd., active hydrogen equivalent: 62 (g / eq.))
[0132] Diethyltoluenediamine ("Aradur (registered trademark)" 5200, manufactured by Huntsman Advanced Materials, active hydrogen equivalent: 45 (g / eq.))
[0133] (3) Viscosity modifier
[0134] ·Polyethersulfone ("Sumikaexcel" (registered trademark) PES5003P, manufactured by Sumitomo Chemical Co., Ltd.)
[0135] (4) Preparation method of epoxy resin composition
[0136] The epoxy resin and viscosity modifier listed in Table 1 were placed in a kneading device, and heated and kneaded to dissolve the viscosity modifier. Then, the temperature was lowered to 100° C. or lower while the kneading was continued, and an amine compound appropriately selected from the amine compounds listed in Table 1 was added and stirred to obtain epoxy resin compositions B-1 to B-12.
[0137] <Method for producing and evaluating epoxy resin cured products>
[0138] The epoxy resin composition prepared by the above method was injected into a mold, and the temperature was raised from 30°C to 180°C at a rate of 1.5°C / min in a hot air dryer, and after heat curing at 180°C for 120 minutes, the temperature was lowered to 30°C at a rate of 2.5°C / min to produce a plate-shaped resin cured product with a thickness of 2 mm. The obtained epoxy resin cured product was evaluated for each specific example described in Table 1 by the following method.
[0139] <Method for measuring glass transition temperature of cured epoxy resin>
[0140] A test piece with a width of 12.7 mm and a length of 45 mm was cut out from the resin cured plate prepared by the above method, and the test piece was dried in a vacuum oven at 60°C for 24 hours. A storage elastic modulus curve was obtained by a dynamic viscoelasticity test in accordance with JIS K 7244-7 (2007). In the storage elastic modulus curve, the temperature value at the intersection of the tangent line in the glass state and the tangent line in the transition state was taken as the glass transition temperature.
[0141] <Method for measuring the flexural modulus of epoxy resin cured products>
[0142] A test piece with a length of 60 mm and a width of 10 mm was cut out from the resin cured plate produced by the above method, and the test piece was dried in a vacuum oven at 60°C for 24 hours. A three-point bending test was carried out using a universal testing machine (manufactured by Instron Japan Co., Ltd., "Instron" (registered trademark) 5565 Model P8564) at a test speed of 2.5 mm / min and a distance between fulcrums of 32 mm, and the bending modulus was calculated in accordance with JIS K7171 (1994).
[0143] <Method for producing prepreg>
[0144] The prepregs were prepared by the following two methods. The components used in each example are shown in Tables 2 and 3, respectively.
[0145] [I] Pull out the component [A] reinforcing fiber (weight per unit area 193g / m 2 ) a reinforcing fiber sheet arranged in a continuous state in one direction, which is made to run in one direction, and the unit area weight of the component [C] is 120 g / m 2 The resin sheet is arranged on the continuous reinforcing fiber sheet, heated by an IR heater to melt the component [C], and attached to the entire surface of one side of the continuous reinforcing fiber sheet, and pressed by a nip roll whose surface temperature is maintained below the melting point of the component [C] to impregnate the reinforcing fiber sheet, and the resulting object is cooled to obtain a fiber-reinforced resin intermediate. The epoxy resin composition related to the components [B] and [B'] selected as shown in Tables 2 and 3 was coated with 100 g / m 2 The epoxy resin film is prepared by coating a resin per unit area weight on release paper, and then the epoxy resin film is overlapped on the surface of the intermediate opposite to the surface impregnated with the component [C], and the epoxy resin composition is impregnated into the intermediate by heating and pressing with a hot roller to obtain a prepreg [I].
[0146] [II] Using a knife coater, the epoxy resin compositions of the components [B] and [B'] selected as described in Tables 2 and 3 were coated at a rate of 50 g / m 2 The resin film was coated on release paper with a unit weight of 193 g / m2. The resin film was overlapped on the reinforcing fibers (unit weight 193 g / m2) of the component [A] which were paralleled in one direction. 2 ) on both sides, heat and pressurize using hot rollers and impregnate the carbon fibers with an epoxy resin composition to obtain a prepreg [II].
[0147] <Production method of laminate and evaluation of mechanical properties>
[0148] (1) Determination method of tensile shear bond strength
[0149] The prepregs [I] and [II] prepared above are cut into a specified size to obtain 2 prepregs [I] and 6 prepregs [II]. The axial direction of the reinforcing fiber is set to 0°, the axis-orthogonal direction is defined as 90°, and [0° / 90°]2s (symbol s represents mirror symmetry) is stacked to prepare a preform. At this time, the two outermost layers of each side are stacked in a manner to become prepregs [I], and the two surface layers of the preform are configured in a manner to become thermoplastic resin layers containing constituent element [C]. The preform is set in a press molding die, and a clamp and a spacer are used as needed. A pressure of 0.6MPa is applied by a press while maintaining the shape, and heated at 180°C for 120 minutes to obtain a laminate.
[0150] The obtained laminate was cut into two pieces with a width of 250 mm and a length of 92.5 mm with the 0° direction as the length direction of the test piece, and dried in a vacuum oven for 24 hours. Then, the two sheets were overlapped with a width of 25 mm × a length of 12.5 mm with the 0° direction as the length direction, and a pressure of 3 MPa was applied at a temperature 20°C higher than the melting point of the thermoplastic resin used as the component [C], and maintained for 1 minute, thereby welding the overlapped surfaces to obtain an integrated molded product. According to ISO4587:1995 (JIS K6850 (1994)), the wing sheet was bonded to the obtained integrated molded product and cut with a width of 25 mm to obtain the target test piece.
[0151] The obtained test piece was dried in a vacuum oven for 24 hours, and the tensile shear bonding strength at an ambient temperature of 23° C. was measured in accordance with ISO 4587:1995 (JIS K6850 (1994)), and the following evaluation was performed based on the measurement results. The results are shown in the table.
[0152] 28MPa and above: A
[0153] 25MPa or more, less than 28MPa: B
[0154] 20MPa or more, less than 25MPa: C
[0155] Less than 20MPa: D (unqualified)
[0156] (2) Determination method of compressive strength
[0157] The prepregs [I] and [II] prepared in the above are cut into a specified size to obtain 2 prepregs [I] and 4 prepregs [II]. The two outermost layers of each side are made into prepregs [I], and the prepregs [II] are sandwiched in the middle. A total of 6 sheets are stacked in a manner that all have the same reinforcing fiber direction to prepare a preform. At this time, the two surface layers of the preform are arranged in a manner that they become thermoplastic resin layers containing component [C]. The preform is set in a press molding die, and a clamp and a spacer are used as needed. While maintaining its shape, a pressure of 0.6MPa is applied by a press machine, and heated at 180°C for 120 minutes to obtain a laminated body.
[0158] According to SACMA-SRM 1R-94, after bonding the tab to the obtained laminate, a rectangular test piece of 80 mm in length and 15 mm in width was cut out with the axial direction of the reinforcing fiber as the length direction of the test piece. The obtained test piece was dried in a vacuum oven at 60°C for 24 hours, and the compressive strength was measured at 23°C using a material universal testing machine (Instron Japan (Strain), "Instron" (registered trademark) 5565 type P8564) according to SACMA-SRM 1R-94, and the evaluation was performed in the following manner based on the measurement results. The results are shown in the table.
[0159] 1.6GPa and above: A
[0160] 1.4GPa or more, less than 1.6GPa: B
[0161] 1.2GPa or more, less than 1.4GPa: C
[0162] Less than 1.2GPa: D (unqualified)
[0163] (3) Method for measuring flatness (dimensional accuracy)
[0164] The prepregs [I] and [II] prepared above were cut into pieces with a length of 250 mm and a width of 125 mm to obtain two prepregs [I] and six prepregs [II]. The two outermost layers of each side were made into prepregs [I], and the prepregs [II] were sandwiched in the middle. A total of eight sheets were stacked in a manner that all had the same reinforcing fiber direction to prepare a preform. At this time, the two surface layers of the preform were arranged in a manner that the thermoplastic resin layers containing the constituent element [C] were formed. The preform was placed in a press-molding die, and a clamp and a spacer were used as needed. While maintaining its shape, a pressure of 0.6 MPa was applied by a press machine, and heated at 180°C for 120 minutes to obtain a laminate.
[0165] According to JIS B7513 (1992), the flatness of the obtained laminate is evaluated. The obtained laminate is cut into a size of 250 mm in length and 125 mm in width, and 3 of the 4 ends of the laminate are grounded on a precision platform, and the height of the remaining 1 point from the table is calculated. The 4 ends of the laminate are each used as a point not grounded on the above-mentioned precision platform, and the height from each table is calculated using the above method. The highest value of the 4 heights from the table is used as the flatness of the laminate. Based on the measurement results, the evaluation is performed in the following manner. The results are shown in the table.
[0166] Less than 5mm: A
[0167] 5mm or more and less than 10mm: B
[0168] 10mm or more and less than 15mm: C
[0169] 15mm and above: D (unqualified)
[0170] (4) Interlaminar fracture toughness value (G IIC )
[0171] The prepreg [I] prepared above was cut into a predetermined size and stacked in a total of 20 sheets in such a manner that the reinforcing fibers were in the same direction. At this time, a release film for introducing precracks was sandwiched between the 10th and 11th sheets in the center to prepare a preform. The preform was placed in a press-forming mold, and a jig and a spacer were used as needed. While maintaining the shape, a pressure of 0.6 MPa was applied by a press machine, and heated at 180° C. for 120 minutes to obtain a laminate.
[0172] From the obtained laminate, a rectangular test piece with a length of 150 mm and a width of 20 mm was cut out with the reinforcing fiber axis as the length direction of the test piece, and dried in a vacuum oven at 60°C for 24 hours. The obtained test piece was evaluated for interlaminar fracture toughness value (G IIC ).
[0173] <Measurement of the mean roughness length RSm and the mean roughness height Rc of the prepreg and laminate>
[0174] Using the prepreg [I] prepared above, an optical microscope is used to take a 1000-fold image in a cross section cut perpendicular to the plane direction of the prepreg at an angle of 45 degrees when looking down at the prepreg relative to any fiber direction of [A] connected to the above two resin regions. In an arbitrary 500 μm square observation range in the obtained image, the roughness average length RSm and the roughness average height Rc of the obtained cross-sectional curve element defined by JIS B0601 (2001) are measured using the above-mentioned cross-sectional curve element measurement method 1. In the case of a laminate, the laminate described in (1) the tensile shear bonding strength measurement method is also used, and an optical microscope is used to take a 1000-fold image in an observation cross section cut perpendicular to the plane direction, and then the measurement is performed in the same manner as in the case of the above-mentioned prepreg.
[0175] <Methods for producing laminates of Examples 1 to 19 and Comparative Examples 1 and 2>
[0176] In Examples 1 to 19 and Comparative Examples 1 and 2, laminates were produced by the method described in (1) the method for measuring tensile shear bond strength, (2) the method for measuring compressive strength, and (3) the method for measuring flatness.
[0177] <Method for producing laminates of Example 20 and Comparative Examples 3 to 5>
[0178] In Comparative Example 3, a film having a unit weight of 50 g / m2 was attached to both sides of a reinforcing fiber sheet arranged in a plane in one direction. 2 A film of polyamide 6 ("Amilan" (registered trademark) CM1007 (manufactured by Toray Co., Ltd.)) was heated and pressed at 250°C to obtain a reinforced carbon fiber with a unit weight of 193 g / m 2 The obtained prepreg was cut into a predetermined size and used for evaluation of bonding strength, flatness and compressive strength at [0° / 90°] 2s The laminates were stacked in the same direction, 8 sheets were stacked in the same direction, or 6 sheets were stacked in the same direction, and then a pressure of 3 MPa was applied by a press machine and heated at 250°C for 10 minutes to obtain laminates. The bonding strength, compression strength and flatness of the obtained laminates were measured by the methods described in the examples.
[0179] In Example 20, the above-mentioned prepreg [I] was cut into a predetermined size, a total of 20 sheets were stacked in such a manner that the reinforcing fibers were oriented in the same direction, and a release film for introducing a precrack was sandwiched between the 10th and 11th sheets in the center to produce a preform.
[0180] In Comparative Example 4, the prepreg [II] (not containing the component [C]) was cut into a predetermined size and laminated in the same manner as in Example 20 with a release film interposed therebetween to obtain a preform.
[0181] In Comparative Example 5, on one side of a prepreg [II] (not including component [C]) cut into a predetermined size, the particle amount per unit area of the prepreg was 7 g / m 2 Polyamide particles (SP-500, manufactured by Toray Co., Ltd.) were uniformly dispersed in a manner, and then laminated in the same manner as in Example 20, with a release film interposed therebetween to obtain a preform.
[0182] In Example 20 and Comparative Examples 4 and 5, a pressure of 0.6 MPa was applied to the obtained preform by a press machine and heated at 180° C. for 120 minutes to obtain a laminate. Then, the interlaminar fracture toughness value (G IIC ).
[0183] [Table 1]
[0184]
[0185] [Table 2]
[0186]
[0187] [Table 3]
[0188]
[0189] Description of Reference Numerals
[0190] 1: Prepreg or laminate
[0191] 2: Constituent elements [A]
[0192] 3: Component [C] and component [B] or component [D]
[0193] 4: Axial direction of any fiber bundle
[0194] 5: Observe the cross section
[0195] 6: Constituent elements [A]
[0196] 7: Resin area including component [C]
[0197] 8: Resin region containing component [B] or component [D]
[0198] 9: Observe the image
[0199] 10: Boundary surface
[0200] 11: Baseline
[0201] 12: Vertical Baseline
Claims
1. A prepreg comprising the following components [A], [B] and [C], wherein: [B] further includes [B'], wherein the ratio of the number of moles of active hydrogen contained in [B'] to the number of moles of epoxy groups of the epoxy resin contained in [B] is 0.65 or more and 0.95 or less, The average epoxy value of all epoxy resins contained in [B] is 6.0 meq. / g or more and 9.0 meq. / g or less, 40 to 100 parts by mass of a glycidylamine-type epoxy resin containing three or more glycidyl groups is contained relative to 100 parts by mass of all epoxy resins contained in [B], The average amine value of all amine compounds contained in [B'] is 5.0 meq. / g or more and 20.0 meq. / g or less, [C] is present on the surface of the prepreg, wherein [A] is present across the boundary between the resin region containing [B] and the resin region containing [C] and in contact with both resin regions, The resin region containing [B] and the resin region containing [C] are each formed in a layered manner and are adjacent to each other, thereby forming the boundary surface. [A] Reinforcement fibers; [B] an epoxy resin composition; [B'] amine compound; [C] Thermoplastic resin composition.
2. The prepreg according to claim 1, wherein In the prepreg when viewed from above, when a cross section perpendicular to the plane of the prepreg containing [A] is obtained from a direction that differs by 45 degrees from the fiber direction of any [A] that is in contact with two resin regions [B] and [C], the cross-sectional curve formed by the closely fitting boundary surfaces of the two resin regions in the cross section has a roughness average length RSm defined by JIS B0601 (2001) of less than 100 μm and a roughness average height Rc of more than 3.5 μm.
3. A laminate comprising a layer comprising the following components [A], [C] and [D], In the laminate, there are reinforcing fibers [A] that straddle a boundary surface between a resin region containing [C] and a resin region containing [D] and are in contact with both resin regions. [A] Reinforcement fibers; [C] a thermoplastic resin composition; [D] An epoxy resin cured product obtained by curing an epoxy resin composition comprising an epoxy resin and an amine compound, wherein the ratio of the number of moles of active hydrogen of the amine compound to the number of moles of epoxy groups of the epoxy resin is 0.65 or more and 0.95 or less, The average epoxy value of all epoxy resins contained in [D] is 6.0 meq. / g or more and 9.0 meq. / g or less, 40 to 100 parts by mass of a glycidylamine-type epoxy resin containing three or more glycidyl groups is contained relative to 100 parts by mass of all epoxy resins contained in [D], The average amine value of all amine compounds contained in [D] is 5.0 meq. / g or more and 20.0 meq. / g or less, The boundary surface is formed by the resin region containing [C] and the resin region containing [D] being formed in layers and being adjacent to each other.
4. The laminate according to claim 3, wherein: In a stack viewed from above, when a cross-section perpendicular to the plane of the stack containing [A] is obtained from a direction that differs by 45 degrees from the fiber direction of any [A] that is connected to two resin regions [C] and [D], the cross-sectional curve formed by the closely fitting boundary surfaces of the two resin regions in the cross-section has a roughness average length RSm defined by JIS B0601 (2001) of less than 100 μm and a roughness average height Rc of more than 3.5 μm.
5. The laminate according to claim 3 or 4, wherein: On the surface there is a resin region containing [C].
6. The prepreg according to claim 1 or 2, or the laminate according to any one of claims 3 to 5, wherein: The thermoplastic resin contained in [C] has a functional group selected from the group consisting of a carboxyl group, an amino group, a hydroxyl group, and an isocyanate group.
7. The prepreg according to claim 1 or 2, or the laminate according to any one of claims 3 to 6, wherein: The surface free energy measured by the Wilhelmy method is 10 to 50 mJ / m 2 The reinforcing fiber is used as [A].
8. A laminate, wherein: A cured product of the prepreg according to claim 1 or 2 constitutes at least a part of the layer.
9. An integrated molded article, which is formed by integrating the laminate according to claim 5 with another member by bonding it to the surface where the resin region including [C] exists.
Citation Information
Patent Citations
Prepreg and fiber-reinforced composite material
JP1996259713A
Carbon fiber reinforced resin molded product and its manufacture
JP1998138354A
Adhesion structural member
JP2018161801A
Epoxy resin composition for carbon-fiber-reinforced composite materials, prepreg, and carbon-fiber-reinforced composite material
CA3097322A1
Epoxy resin composition, prepreg, and fiber-reinforced composite material
CN103370353A