A modified pigment and its preparation method and application

By adding amide coating agents and nitrogen-containing heterocyclic compounds to alkyl alcohol solvents, the problem of poor dispersion of heterocyclic pigments is solved, and good dispersion in plastics, rubber and other products is achieved, as well as inks, Stability of oil-based paints.

CN114773677BActive Publication Date: 2024-10-15JIAHUA CHEM TECH DEV SHANGHAI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210547813.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-18
Publication Date
2024-10-15
Estimated Expiration
2042-05-18

AI Technical Summary

Technical Problem

It is difficult to significantly improve the dispersion of heterocyclic pigments in plastics, rubber, coatings and other products with existing technology, especially the dispersion of dioxazine pigments is poor.

Method used

Using a modified pigment preparation method, add amide coating agents and nitrogen-containing heterocyclic compounds to alkyl alcohol solvents, control the temperature and stirring speed, cool down after forming a solution, and dry by filter press to ensure that the coating agent is wrapped in the pigment On the particle surface, it blocks particle aggregation and improves dispersion.

Benefits of technology

Significantly improves the dispersion of heterocyclic pigments in plastics, rubber, coatings and other products, reduces extrusion pressure and color difference, improves the stability of color pastes in inks and oil-based coatings, and avoids the problem of large residual amounts of coating agents. question.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114773677B_ABST
    Figure CN114773677B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of pigment preparation, and specifically relates to a modified pigment and its preparation method and application. The preparation method comprises: (1) adding a coating agent to an alkyl alcohol solvent at 90-100°C to dissolve, and obtaining a solution A; (2) adding a nitrogen-containing heterocyclic compound to the solution A, and obtaining a mixed solution B after uniform dispersion; then cooling the mixed solution B to room temperature at a rate not higher than 10°C / h, filtering by pressure, and drying; wherein the mass concentration of the coating agent in the solution A is not higher than 10wt% and the mass concentration of the nitrogen-containing heterocyclic compound in the mixed solution B is 40wt%-70wt%; or, the mass ratio of the nitrogen-containing heterocyclic compound to the coating agent is (10-50):1. The modified pigment obtained by the preparation method has good dispersibility in products such as plastics, rubbers, coatings, and inks, and has good dispersibility in plastic substrates even for pigments with poor dispersibility such as permanent violet and phthalocyanine blue.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pigment preparation, and specifically relates to a modified pigment and a preparation method and application thereof. Background Art

[0002] Pigments play an important role as colorants in inks and coatings. Since the 1990s, organic pigments have been mixed or extruded with thermoplastic polymers such as polypropylene, polyethylene, polyamide, nylon, etc. through twin-screw extruders to directly obtain colored plastic products without the need for subsequent coloring by brushing. However, compared with traditional coating liquid systems, it is more difficult to disperse pigments in systems such as thermoplastic polymers. At present, when improving the dispersion performance of pigments, surface treatment of the pigment itself is often used to achieve the purpose of improving dispersibility. In recent years, with the in-depth research in the field of pigment technology, its dispersibility has made significant progress.

[0003] In order to improve the dispersibility of pigments in thermoplastic polymers, the prior art generally uses three aspects of pigment refinement, wetting and surface treatment to treat the pigments. Among them, the most effective treatment method is the use of dispersants. Dispersants mainly wet the pigments to make the pigments evenly dispersed in the resin and not easy to agglomerate during the processing. Dispersants are a very important component in the preparation of color plastics and are widely used in thermoplastic polymers such as polyolefins, polyesters, and polyurethanes. However, for heterocyclic pigments, especially dioxazine pigments, since their molecular structure is mainly composed of non-polar cyclic groups, no dispersant that matches them well has been found. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects in the prior art that the dispersibility of heterocyclic pigments in products such as plastics, rubbers, and coatings is difficult to be significantly improved, thereby providing a pigment and a preparation method and application thereof.

[0005] To this end, the present invention provides the following technical solutions.

[0006] The present invention provides a method for preparing a modified pigment, comprising the following steps:

[0007] (1) adding the encapsulating agent to an alkyl alcohol solvent at 90-100° C. to dissolve the encapsulating agent to obtain a solution A;

[0008] (2) adding a nitrogen-containing heterocyclic compound to the solution A and dispersing the mixture uniformly to obtain a mixed solution B; then cooling the mixed solution B to room temperature at a rate not higher than 10° C. / h, filtering by pressure, and drying;

[0009] The encapsulating agent is an amide alkyl compound having the following structural formula:

[0010]

[0011] The value range of n is 10-26, and the value range of m is 2-12;

[0012] Wherein, the mass concentration of the encapsulating agent in the solution A is not higher than 10wt% and the mass concentration of the nitrogen-containing heterocyclic compound in the mixed solution B is 40wt%-70wt%; or,

[0013] The mass ratio of the nitrogen-containing heterocyclic compound to the encapsulating agent is (10-50):1.

[0014] The saturated solubility of the encapsulating agent in an alkyl alcohol solvent at 90-100° C. is greater than 30%; and

[0015] The saturated solubility of the encapsulating agent in an alkyl alcohol solvent at 10-30° C. is less than 1%.

[0016] The alkyl alcohol solvent is at least one of isopropanol, n-butanol, pentanol, hexanol, cyclohexane and n-heptane.

[0017] The alkyl alcohol solvent used in the present invention has the following characteristics: it has good solubility for amide alkyl compounds at 90-100°C; when the temperature drops to room temperature (10-30°C), the solubility of amide alkyl compounds in alkyl alcohol solvents is poor and they will precipitate, so that the amide alkyl compounds are wrapped on the surface of the pigment particles.

[0018] The nitrogen-containing heterocyclic compound is at least one of a dioxazine compound and an indole compound.

[0019] The mass concentration of the encapsulating agent in the solution A is 4wt%-6wt%.

[0020] The mass ratio of the nitrogen-containing heterocyclic compound to the encapsulating agent is (20-30):1.

[0021] When preparing the modified pigment, the stirring speed when adding solution A to the nitrogen-containing heterocyclic compound is 50-300 rpm, which can be but not limited to 50 rpm, 80 rpm, 100 rpm, 200 rpm, 260 rpm, etc.

[0022] The preparation method of the amide alkyl compound comprises the following steps:

[0023] Mix the various raw materials of the amide alkyl compound at 90-100°C, heat to 130-150°C and stir for 3-5h after they are completely dissolved, heat to 160-180°C and react for 1-3h, and cool.

[0024] Among them, the type and dosage ratio of the raw materials can be determined according to the structural formula of the amide alkyl compound.

[0025] The present invention also provides a modified pigment prepared by the above preparation method.

[0026] The present invention also provides an application of the modified pigment prepared by the preparation method in plastics, rubber, coatings, inks, cosmetics or textiles.

[0027] The technical solution of the present invention has the following advantages:

[0028] 1. A method for preparing a modified pigment provided by the present invention, the method comprising: (1) adding an encapsulating agent to an alkyl alcohol solvent at 90-100° C. to dissolve the encapsulating agent to obtain a solution A; (2) adding a nitrogen-containing heterocyclic compound to the solution A and dispersing the nitrogen-containing heterocyclic compound to obtain a mixed solution B; then cooling the mixed solution B to room temperature at a rate not higher than 10° C. / h, filtering the mixed solution B, and drying the mixed solution B; wherein the mass concentration of the encapsulating agent in the solution A is not higher than 10wt% and the mass concentration of the nitrogen-containing heterocyclic compound in the mixed solution B is 40wt%-70wt%; or, the mass ratio of the nitrogen-containing heterocyclic compound to the encapsulating agent is (10-50):1. The modified pigment prepared by the preparation method has good dispersibility in products such as plastics, rubbers, coatings, and inks, and even has good dispersibility in plastic matrices for pigments with poor dispersibility such as permanent violet and phthalocyanine blue. When the pigment is used in products such as plastics, the extrusion pressure is small and the color difference of the product is small. At the same time, the surface of the pigment prepared by the method has good lipophilicity due to being modified by the encapsulating agent. When the pigment is used in inks and oily coatings, the obtained color paste has good stability.

[0029] The preparation method adds an encapsulating agent to the nitrogen-containing heterocyclic compound in the synthesis stage, so that the nitrogen-containing heterocyclic compound particles are in the primary particle state with a small particle size. The encapsulating agent is dissolved in an alkyl alcohol solvent at a specific temperature. By using a specific amount of the nitrogen-containing heterocyclic compound, the encapsulating agent and the alkyl alcohol solvent, and at a certain cooling rate, the encapsulating agent is encapsulated on the surface of the primary particles of the nitrogen-containing heterocyclic compound through recrystallization, so as to play a barrier role, and prevent the occurrence of large-scale aggregation between the particles of the heterocyclic compound when the modified pigment is used in plastics and rubber products, forming agglomerates, increasing the particle size, reducing the dispersibility of the pigment, and the like; at the same time, the specific encapsulating agent used in the present invention is compatible with the matrix of products such as plastics and rubbers, and can improve the solubility of the nitrogen-containing heterocyclic compound particles in the matrix of the product, and further improve the dispersibility of the pigment in the matrix of the product.

[0030] Furthermore, molecules of nitrogen-containing heterocyclic compounds lack polar groups such as amine, hydroxyl, and carboxyl groups, and ordinary dispersants are difficult to wet their surfaces. The present invention adopts a specific method to form a bond between the nitrogen-containing heterocyclic compounds and the encapsulating agent. The encapsulating agent is wrapped on the surface of the primary particles of the nitrogen-containing heterocyclic compounds to play a barrier role, prevent problems such as particle aggregation, and thereby improve the dispersibility of the pigment.

[0031] In addition, by controlling the amount of nitrogen-containing heterocyclic compounds and encapsulating agents, almost all of the encapsulating agents can completely encapsulate the nitrogen-containing heterocyclic compound particles during the recrystallization process, and the residual amount of the encapsulating agent in the alkyl alcohol solvent is less than 0.5wt%, thereby improving the utilization rate of the encapsulating agent, making the pigment have better dispersibility, and eliminating the problem of subsequent residual chemical solution treatment. By controlling various parameters in the preparation method, the pigment can have excellent dispersibility, even in nitrogen-containing heterocyclic compounds with poor dispersibility such as permanent violet and phthalocyanine blue.

[0032] Compared with the traditional soaking process, the preparation method of the present invention is more efficient and avoids the problem of large amount of residual encapsulating agent.

[0033] 2. The preparation method of the modified pigment provided by the present invention adopts an alkyl alcohol solvent with a specific solubility, so that the encapsulating agent can encapsulate the primary pigment particles, thereby improving the dispersibility of the pigment. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0035] Figure 1 is an infrared spectrum of ethylene bisstearamide prepared in Example 1 of the present invention;

[0036] Figure 2 It is the DSC spectrum of ethylene bisstearamide prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0037] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0038] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0039] Example 1

[0040] This embodiment provides a method for preparing a modified pigment, comprising the following steps:

[0041] 100 g of isopropanol was placed in a flask, heated to 90° C., 5 g of ethylene bisstearamide (EBS) was added and maintained at 90° C., and stirred until completely dissolved to obtain solution A;

[0042] And add 80g of permanent violet RL (carbazole dioxazine) to solution A at 90°C, stir to disperse it evenly to form a suspension, and obtain mixed solution B, then cool it to room temperature (25°C) at a rate of 10°C / h, stop stirring, filter the isopropanol solution with a positive pressure filter at 2-3bar, and then dry it under reduced pressure at 60°C and 20-50mbar to constant weight to obtain modified pigment A.

[0043] Wherein, the preparation method of ethylene bisstearamide in this embodiment is as follows:

[0044] Mix 285g of stearic acid and 30g of ethylenediamine at 90°C under a nitrogen atmosphere. After they are completely dissolved, heat to 140°C and stir for 4h. Heat to 170°C and react for 2h. After cooling, ethylene bisstearamide is obtained.

[0045] Figure 1 is the infrared spectrum of ethylene bisstearamide obtained in this example, Figure 2 is the DSC spectrum of ethylene bis stearamide obtained in this example; Figure 1 and Figure 2 It can be explained that the encapsulating agent prepared in this embodiment is a crystalline compound, and the encapsulating agent with crystallinity can be encapsulated on the surface of the permanent purple RL particles.

[0046] Example 2

[0047] This embodiment provides a method for preparing a modified pigment, comprising the following steps:

[0048] Place 100 g of isopropanol in a flask, heat to 90°C, add 5 g of ethylenebisbehenamide, maintain the temperature at 90°C, and stir until completely dissolved to obtain solution A;

[0049] Add 80g of permanent violet RL (carbazole dioxazine) to solution A at 90°C, stir to disperse it evenly to form a suspension, and then cool it to room temperature (25°C) at a rate of 10°C / h, stop stirring, filter the isopropanol solution with a positive pressure filter at 2-3bar, and then dry it under reduced pressure at 60°C and 20-50mbar to constant weight to obtain modified pigment B.

[0050] Wherein, the preparation method of ethylene bisbehenamide in this embodiment is as follows:

[0051] Mix 341 g of behenic acid and 30 g of ethylenediamine at 90° C. under a nitrogen atmosphere. After they are completely dissolved, heat to 140° C. and stir for 4 h. Heat to 170° C. and react for 2 h. After cooling, ethylene bisstearamide is obtained.

[0052] Example 3

[0053] This embodiment provides a method for preparing a modified pigment, comprising the following steps:

[0054] Place 100 g of isopropanol in a flask, heat to 90°C, add 5 g of ethylene bislauramide, maintain the temperature at 90°C, and stir until completely dissolved to obtain solution A;

[0055] 80 g of Permanent Purple RL (carbazole dioxazine) was added to the solution A at 90° C. and stirred to disperse it evenly to form a suspension to obtain a mixed solution B, which was then cooled to room temperature (25° C.) at a rate of 10° C. / h. The stirring was stopped, and the isopropanol solution was filtered using a positive pressure filter at 2-3 bar, and then dried under reduced pressure at 60° C. and 20-50 mbar to constant weight to obtain a modified pigment C.

[0056] Wherein, the preparation method of ethylene bislauramide in this embodiment is as follows:

[0057] Mix 200 g of lauric acid and 30 g of ethylenediamine at 90° C. under a nitrogen atmosphere. After they are completely dissolved, heat to 140° C. and stir for 4 h. Heat to 170° C. and react for 2 h. After cooling, ethylene bislauramide is obtained.

[0058] Example 4

[0059] This embodiment provides a method for preparing a modified pigment, comprising the following steps:

[0060] Place 100 g of isopropanol in a flask, heat to 90° C., add 5 g of hexamethylene bisstearamide, maintain the temperature at 90° C., and stir until completely dissolved to obtain solution A;

[0061] And add 80g of permanent violet RL (carbazole dioxazine) to solution A at 90°C, stir to disperse it evenly to form a suspension, and obtain mixed solution B, then cool it to room temperature (25°C) at a rate of 10°C / h, stop stirring, filter the isopropanol solution with a positive pressure filter at 2-3bar, and then dry it under reduced pressure at 60°C and 20-50mbar to constant weight to obtain modified pigment D.

[0062] Wherein, the preparation method of hexamethylene bisstearamide in this embodiment is as follows:

[0063] Mix 285g of stearic acid and 58g of hexamethylenediamine at 90°C under a nitrogen atmosphere. After they are completely dissolved, heat to 140°C and stir for 4h. Heat to 170°C and react for 2h. After cooling, obtain hexamethylenebisstearamide.

[0064] Example 5

[0065] This embodiment provides a method for preparing a modified pigment, comprising the following steps:

[0066] Place 100 g of isopropanol in a flask, heat to 90° C., add 5 g of hexamethylenebisbehenamide, maintain the temperature at 90° C., and stir until it is completely dissolved to obtain solution A;

[0067] 80 g of permanent violet RL (carbazole dioxazine) was added to solution A at 90° C. and stirred to disperse it evenly to form a suspension to obtain a mixed solution B, which was then cooled to room temperature (25° C.) at a rate of 10° C. / h. The stirring was stopped, and the isopropanol solution was filtered using a positive pressure filter at 2-3 bar, and then dried under reduced pressure at 60° C. and 20-50 mbar to constant weight to obtain a modified pigment E.

[0068] Wherein, the preparation method of hexamethylene bisbehenamide in this embodiment is as follows:

[0069] 341 g of behenic acid and 58 g of hexamethylenediamine were mixed at 90° C. under a nitrogen atmosphere. After they were completely dissolved, the mixture was heated to 140° C. and stirred for 4 h. The mixture was then heated to 170° C. and reacted for 2 h. After cooling, hexamethylenebisbehenamide was obtained.

[0070] Example 6

[0071] This embodiment provides a method for preparing a modified pigment, comprising the following steps:

[0072] Place 100 g of isopropanol in a flask, heat to 90°C, add 5 g of hexamethylene bislauramide, maintain the temperature at 90°C, and stir until it is completely dissolved to obtain solution A;

[0073] 80 g of permanent violet RL (carbazole dioxazine) was added to solution A at 90°C and stirred to disperse it evenly to form a suspension to obtain a mixed solution B, which was then cooled to room temperature (25°C) at a rate of 10°C / h. The stirring was stopped, and the isopropanol solution was filtered using a positive pressure filter at 2-3 bar, and then dried under reduced pressure at 60°C and 20-50 mbar to constant weight to obtain a modified pigment F.

[0074] Wherein, the preparation method of hexamethylene bislauric amide in this embodiment is as follows:

[0075] Mix 200 g of lauric acid and 58 g of hexamethylenediamine at 90° C. under a nitrogen atmosphere. After they are completely dissolved, heat to 140° C. and stir for 4 h. Heat to 170° C. and react for 2 h. After cooling, obtain hexamethylenebislauramide.

[0076] Example 7

[0077] This embodiment provides a method for preparing a modified pigment, comprising the following steps:

[0078] Place 100 g of isopropanol in a flask, heat to 90°C, add 5 g of dodecyl bisstearamide, maintain the temperature at 90°C, and stir until completely dissolved to obtain solution A;

[0079] And add 80g of permanent violet RL (carbazole dioxazine) to solution A at 90°C, stir to disperse it evenly to form a suspension, and then reduce the temperature to room temperature (25°C) at a rate of 10°C / h, stop stirring, filter the isopropanol solution with a positive pressure filter at 2-3bar, and then reduce the pressure and dry it to constant weight at 60°C and 20-50mbar to obtain modified pigment G.

[0080] Wherein, the preparation method of dodecyl bisstearamide in this embodiment is as follows:

[0081] Mix 285 g of stearic acid and 100 g of dodecanediamine at 90° C. under a nitrogen atmosphere. After they are completely dissolved, heat to 140° C. and stir for 4 h. Heat to 170° C. and react for 2 h. After cooling, obtain dodecyl bisstearamide.

[0082] Example 8

[0083] This embodiment provides a method for preparing a modified pigment, comprising the following steps:

[0084] Place 100 g of isopropanol in a flask, heat to 90° C., add 5 g of dodecyl bisbehenamide, maintain the temperature at 90° C., and stir until it is completely dissolved to obtain solution A;

[0085] 80 g of permanent violet RL (carbazole dioxazine) was added to solution A at 90° C. and stirred to disperse it evenly to form a suspension to obtain a mixed solution B, which was then cooled to room temperature (25° C.) at a rate of 10° C. / h. Stirring was stopped, and the isopropanol solution was filtered using a positive pressure filter at 2-3 bar, and then dried under reduced pressure at 60° C. and 20-50 mbar to constant weight to obtain a modified pigment H.

[0086] Wherein, the preparation method of dodecyl bisbehenamide in this embodiment is as follows:

[0087] 341 g of behenic acid and 100 g of dodecanediamine were mixed at 90° C. under a nitrogen atmosphere. After complete dissolution, the mixture was heated to 140° C. and stirred for 4 h. The mixture was then heated to 170° C. and reacted for 2 h. Dodecylbisbehenamide was obtained after cooling.

[0088] Example 9

[0089] This embodiment provides a method for preparing a modified pigment, comprising the following steps:

[0090] Place 100 g of isopropanol in a flask, heat to 90°C, add 5 g of dodecyl dilauramide, maintain the temperature at 90°C, and stir until completely dissolved to obtain solution A;

[0091] 80 g of permanent violet RL (carbazole dioxazine) was added to solution A at 90° C. and stirred to disperse it evenly to form a suspension to obtain a mixed solution B, which was then cooled to room temperature (25° C.) at a rate of 10° C. / h. The stirring was stopped, and the isopropanol solution was filtered using a positive pressure filter at 2-3 bar, and then dried under reduced pressure at 60° C. and 20-50 mbar to constant weight to obtain modified pigment I.

[0092] Wherein, the preparation method of dodecyl bislauramide in this embodiment is as follows:

[0093] Mix 200 g of lauric acid and 100 g of dodecanediamine at 90° C. under a nitrogen atmosphere. After complete dissolution, heat to 140° C. and stir for 4 h. Heat to 170° C. and react for 2 h. After cooling, obtain dodecyl dilauramide.

[0094] Example 10

[0095] This embodiment provides a method for preparing a modified pigment, comprising the following steps:

[0096] 100 g of cyclohexane was placed in a flask, heated to 95°C, 10 g of ethylene bisstearamide (EBS) was added and maintained at 95°C, and stirred until completely dissolved to obtain solution A;

[0097] And add 100g of permanent violet RL (carbazole dioxazine) to solution A at 90°C, stir to disperse it evenly to form a suspension, and then obtain mixed solution B, and then cool it to room temperature (25°C) at a rate of 10°C / h, stop stirring, filter the isopropanol solution with a positive pressure filter at 2-3bar, and then reduce the pressure and dry it to constant weight at 60°C and 20-50mbar to obtain modified pigment J.

[0098] Wherein, the preparation method of ethylene bisstearamide in this embodiment is as follows:

[0099] Mix 285g of stearic acid and 30g of ethylenediamine at 90°C under a nitrogen atmosphere. After they are completely dissolved, heat to 140°C and stir for 4h. Heat to 170°C and react for 2h. After cooling, ethylene bisstearamide is obtained.

[0100] Embodiment 11

[0101] This embodiment provides a method for preparing a modified pigment, comprising the following steps:

[0102] 100 g of isopropanol was placed in a flask, heated to 98° C., 5 g of ethylene bisstearamide (EBS) was added and maintained at 98° C., and stirred until completely dissolved to obtain solution A;

[0103] 80 g of phthalocyanine blue was added to solution A at 90° C. and stirred to disperse it evenly to form a suspension to obtain a mixed solution B, which was then cooled to room temperature (25° C.) at a rate of 2° C. / h. Stirring was stopped, and the isopropanol solution was filtered using a positive pressure filter at 2-3 bar, and then dried under reduced pressure at 60° C. and 2-50 mbar to constant weight to obtain a modified pigment K.

[0104] Wherein, the preparation method of ethylene bisstearamide in this embodiment is as follows:

[0105] Mix 285g of stearic acid and 30g of ethylenediamine at 90°C under a nitrogen atmosphere. After they are completely dissolved, heat to 140°C and stir for 4h. Heat to 170°C and react for 2h. After cooling, ethylene bisstearamide is obtained.

[0106] Comparative Example 1

[0107] This comparative example provides a method for preparing a pigment, which is different from Example 1 in that the cooling rate of 10°C / h is changed to 20°C / h, and the rest is the same as Example 1.

[0108] Comparative Example 2

[0109] This comparative example provides a method for preparing a pigment, which differs from Example 1 in that the temperature of the isopropanol in step (1) is changed. Step (1) is specifically as follows, and the rest is the same as Example 1.

[0110] 100 g of isopropanol was placed in a flask, heated to 105° C., 5 g of ethylene bisstearamide (EBS) was added and maintained at 105° C., and stirred until completely dissolved to obtain solution A.

[0111] Comparative Example 3

[0112] This comparative example provides a method for preparing a pigment. The difference from Example 1 is that the amounts of ethylene bisstearamide and Permanent Purple RL are changed. The other aspects are the same as Example 1. In this comparative example, the amount of ethylene bisstearamide is 10 g, and the amount of Permanent Purple RL is 50 g.

[0113] Test Example 1

[0114] This test example provides the dispersibility performance test and results of the pigments prepared in various embodiments and comparative examples.

[0115] Take 4kg of modified pigment (prepared from each embodiment and comparative example) and 6kg of low-density polyethylene (manufacturer: Shanghai Saike Petrochemical Co., Ltd.; model: LL0209) and mix them in a high-speed mixer for 15min, then extrude them using a twin-screw extruder (temperature is 115°C), granulate, and dry to obtain masterbatch. A 400-mesh filter screen is installed at the head of the twin-screw extruder and the pressure when the material passes through the filter screen is recorded, which is the maximum filter pressure. Take the untreated permanent purple RL as a comparative example, and use the above method to obtain the maximum filter pressure. The pressure is recorded in bar, and the larger the value, the greater the applied force and the worse the dispersibility. The results are shown in Table 1. The color difference of the masterbatch prepared in each embodiment and comparative example is tested. The color difference test method is: take 5 masterbatch per group of samples, and test the color difference of each pair of masterbatch in the 5 masterbatch by a colorimeter, a total of 10 groups of samples, take the average value, and the results are shown in Table 1.

[0116] Table 1

[0117]

[0118]

[0119] The experimental results in Table 1 show that the maximum filter pressure value and color difference value of the modified pigment prepared in the present invention in products such as plastics are relatively small, indicating that the modified pigment prepared in the present invention has good dispersibility in matrices such as resins.

[0120] Test Example 2

[0121] This test example provides the residual amount of encapsulating agent in the isopropanol solution filtered through a positive pressure filter when preparing the pigment in the embodiment, and the residual amount of dispersant in the glacial acetic acid solution collected after filtration when preparing the pigment in the prior art. The method for preparing the pigment in the prior art includes the following steps:

[0122] (1) A glacial acetic acid aqueous solution with a mass fraction of 2.0% and a temperature of 45±2°C was stirred at a stirring rate of 2000 rpm, and a dispersant CH-15C (Shanghai Sanzheng Polymer Materials Co., Ltd.) at 60°C was slowly added to the glacial acetic acid aqueous solution to prepare a CH-15C ultra-dispersed emulsion with a mass fraction of 20%.

[0123] (2) Azo toluidine red and CH-15C ultra-dispersed emulsion were mixed in a mass ratio of 1:4, stirred at room temperature for 4 hours, stopped stirring, filtered, and dried to obtain toluidine red pigment; and the filtered glacial acetic acid solution was collected.

[0124] Test method for residual amount of encapsulant or dispersant in solvent: In the process of preparing pigments in various embodiments and prior art, take the alkyl alcohol solution filtered by positive pressure filter or the filtered glacial acetic acid solution W1, the weighing amount of W1 is 2-2.5g, and place it in a blast oven, dry it to constant weight at 130±5℃, weigh it, record it as W2, calculate the residual amount of encapsulant in alkyl alcohol solvent or the residual amount of dispersant in glacial acetic acid solution, the formula is as follows,

[0125] Encapsulating agent or dispersing agent in solvent

[0126] Among them, the weighing results and calculation results are accurate to 0.1g, and the results are shown in Table 2.

[0127] Table 2

[0128] sample Residual amount of encapsulating agent or dispersing agent (%) Pigment A 0.3% Pigment B 0.3% Pigment C 0.3% Pigment D 0.3% Pigment E 0.3% Pigment F 0.3% Pigment G 0.3% Pigment H 0.4% Pigment I 0.4% Pigment J 0.4% Pigment K 0.3% Prior art 18.5%

[0129] According to the results in Table 2, the residual amount of encapsulating agent in the filtrate produced by the pigment preparation of the present invention is small, and the residual amount of dispersant in the filtrate produced by the pigment preparation of the prior art is large, which means that, compared with the prior art, the method provided by the present invention can allow more encapsulating agent to be wrapped on the particle surface of the nitrogen-containing heterocyclic compound.

[0130] Test Example 3

[0131] This test example provides the test method and results of the stability of the pigments prepared in each embodiment and comparative example.

[0132] Preparation of color paste: The organic pigment color paste was prepared by ball milling. Specifically, 10 g of nitrocellulose resin was weighed and placed in a sand mill. 7.5 g of butyl acetate, 7.5 g of n-propyl acetate, 22.5 g of isopropyl alcohol and 22.5 g of ethanol were added for homogenization to make the nitrocellulose resin uniformly dissolved in the solvent. 30 g of pigment (prepared from each embodiment and comparative example) was added to the above solvent at a speed of 50 rpm, and then the speed was increased to 1×10 3 rpm, stir for 10 min, and after stirring evenly, add 200 g of zirconium beads and3 The pigment paste was sand-milled at rpm for 2 hours to obtain the pigment paste. The stability of the modified pigment prepared by the present invention was characterized by the centrifugal stability and high temperature stability of the paste.

[0133] (1) The centrifugal stability test method is as follows: 50 ml of the pigment paste sample is placed in a 50 ml centrifuge tube, and the pigment paste is heated at 6 × 10 3 The centrifugal speed was 100 rpm and the centrifugation was carried out at room temperature for 30 minutes. The absorbance of the pigment paste at the maximum absorption wavelength before and after centrifugation was tested, marked as A0 and A1 respectively, and the relative absorbance (R) was calculated using the following formula. R was used to characterize the centrifugal stability of the pigment paste. The results are shown in

[0134] Table 3;

[0135]

[0136] Wherein, A0 is the absorbance of the pigment paste at the maximum absorption wavelength before centrifugation; A1 is the absorbance of the pigment paste at the maximum absorption wavelength after centrifugation.

[0137] Table 3

[0138]

[0139]

[0140] Note: The larger the R, the better the centrifugal stability.

[0141] (2) Test method for high temperature stability: The pigment paste was placed under high temperature conditions (50°C) for 5 days, and the changes in the particle size and color of the paste were observed to characterize the high temperature stability of the paste. The change in particle size was characterized by ΔD, and the change in color was characterized by ΔE. The results are shown in Table 4. The particle size of the paste was tested by a particle size analyzer. The particle size before high temperature placement was represented by D0, and the particle size after high temperature placement was represented by D1. The calculation method of ΔD is as follows;

[0142]

[0143] The color difference ΔE of the color paste is obtained by testing with a colorimeter, and the calculation formula is as follows:

[0144] ΔE=[(a1-a0) 2 +(b1-b0) 2 +(l1-l0)] 1 / 2 ,

[0145] Among them, a1, b1 and l1 are the parameters of the color after high-temperature placement, and a0, b0 and l0 are the parameters of the color before high-temperature placement.

[0146] Table 4

[0147]

[0148]

[0149] The experimental results in Table 4 show that the modified pigment prepared by the present invention has good stability.

[0150] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A method for preparing a modified pigment, characterized in that: The following steps are included: (1) The encapsulating agent is added to a solvent at 90-100°C to dissolve to obtain solution A; (2) adding a nitrogen-containing heterocyclic compound to the solution A and dispersing the mixture uniformly to obtain a mixed solution B; then cooling the mixed solution B to room temperature at a rate not higher than 10°C / h, filtering and drying the mixed solution; The encapsulating agent is an amide alkyl compound having the following structural formula: The value range of n is 10-26, and the value range of m is 2-12; Wherein, the mass concentration of the encapsulating agent in the solution A is not higher than 10wt% and the mass concentration of the nitrogen-containing heterocyclic compound in the mixed solution B is 40wt%-70wt%; The mass ratio of the nitrogen-containing heterocyclic compound to the encapsulating agent is (10-50): 1; The solvent is at least one of isopropanol or cyclohexane; The saturated solubility of the encapsulating agent in a solvent at 90-100° C. is greater than 30%; and The saturated solubility of the encapsulating agent in a solvent at 10-30° C. is less than 1%.

2. The preparation method according to claim 1, characterized in that: The nitrogen-containing heterocyclic compound is at least one of a dioxazine compound and an indole compound.

3. The preparation method according to claim 1 or 2, characterized in that: The mass concentration of the encapsulating agent in the solution A is 4wt%-6wt%.

4. The preparation method according to claim 2, characterized in that: The mass ratio of the nitrogen-containing heterocyclic compound to the encapsulating agent is (20-30):

1.

5. The preparation method according to claim 1 or 2, characterized in that: The preparation method of the amide alkyl compound comprises the following steps: Mix the various raw materials of the amide alkyl compound at 90-100°C, heat to 130-150°C and stir for 3-5h after they are completely dissolved, heat to 160-180°C and react for 1-3h, and cool.

6. The modified pigment obtained by the preparation method according to any one of claims 1 to 5.