A carbon-supported metal nanocluster catalyst and its preparation method and application
By mixing the metal salt solution of metal chelate and nitrogen source with carbon material and performing electrochemical redox treatment in the electrolyte, a carbon-supported metal nanocluster catalyst was prepared, which solved the problem of poor dispersion and agglomeration of the catalyst. Improves catalytic performance and is suitable for biosensor applications.
Patent Information
- Application Number
- CN202210316852.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-03-29
AI Technical Summary
Existing metal nanocluster catalysts have poor dispersion and agglomeration, resulting in low catalytic performance and difficult to effectively apply in the field of biosensing.
By mixing a metal salt solution containing a metal chelate and a nitrogen source with a carbon material, lyophilized and calcined to form a precatalyst, and cyclic voltammetry electrochemical redox treatment is performed in an electrolyte containing a guide agent, the preparation is prepared The uniformly distributed carbon-supported metal nanocluster catalyst improves its catalytic performance.
It has achieved uniform distribution and catalytic performance improvement of metal nanoclusters, and is suitable for the preparation of biosensors, especially in detecting the concentration of biomolecules such as H2O2, blood sugar, galactose, cholesterol, etc., reducing the amount and cost of precious metals.
Smart Images

Figure CN114797843B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalysts, and in particular to a carbon-supported metal nanocluster catalyst and a preparation method and application thereof. Background Art
[0002] Metal nanoclusters (MNCs) are a new type of functional nanomaterials, which are composed of several to hundreds of atoms of the same or different species, with a size of less than 2nm, and have properties that single atoms or bulk materials do not have. On the one hand, the ultra-small size of metal nanoclusters increases the proportion of surface atoms, showing excellent surface structure and abundant active sites; on the other hand, metal clusters are close to the de Broglie wavelength, and their continuous electronic energy bands can evolve into discrete energy levels, thus showing properties similar to metal complexes. In turn, they show unique catalytic properties, which can improve catalytic activity. However, current metal nanocluster catalysts usually have the disadvantages of poor dispersion of metal nanoclusters and easy agglomeration, which leads to low catalytic performance of the catalyst.
[0003] Therefore, it is necessary to develop a method for preparing metal nanocluster catalysts, which makes the metal nanoclusters evenly distributed without agglomeration and improves the catalytic performance. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a carbon-supported metal nanocluster catalyst, which firstly forms a precatalyst by mixing a metal salt solution containing a metal chelate and a nitrogen source with a carbon material and freeze-drying and calcining, then combines the precatalyst with a working electrode and places it in an electrolyte containing a guiding agent, and electrochemically redox-treats the precatalyst by cyclic voltammetry to obtain a stable metal nanocluster catalyst. By treating the precatalyst by cyclic voltammetry, the supported metal nanoclusters can be distributed more evenly and agglomeration can be reduced. In addition, during the electrochemical redox treatment, the guiding agent can guide the supported metal to reconstruct the exposed crystal plane, increase the exposure ratio of the crystal plane with catalytic activity, and thus improve the catalytic performance.
[0005] Another object of the present invention is to provide a carbon-supported metal nanocluster catalyst obtained by the preparation method, which has a large specific surface area and a large number of active sites, and thus has excellent catalytic performance.
[0006] Since the metal nanocluster catalyst of the present invention has an ultra-small size and good biocompatibility, it is conducive to being safely discharged by the organism, and thus has good application prospects in the field of biosensing. Therefore, another object of the present invention is to provide a biosensor using the carbon-supported metal nanocluster catalyst.
[0007] Another object of the present invention is to provide a use of the biosensor for detecting the concentration of H2O2 or the concentration of biomolecules such as blood glucose, galactose, cholesterol, amino acids, alcohols, lactic acid or uric acid.
[0008] In order to achieve the above objectives, the present invention provides the following technical solutions.
[0009] A method for preparing a carbon-supported metal nanocluster catalyst comprises:
[0010] preparing a metal salt solution, wherein the metal salt solution comprises a metal salt, a metal chelate, a nitrogen source and a solvent;
[0011] mixing the metal salt solution with the carbon material and freeze-drying the mixture to obtain a freeze-dried sample;
[0012] calcining the freeze-dried sample under an inert atmosphere to obtain a carbon-supported metal nanocluster precatalyst; and
[0013] The metal nanocluster precatalyst is combined with a working electrode and placed in an electrolyte containing a guiding agent, and the metal nanocluster precatalyst is subjected to electrochemical oxidation-reduction treatment by cyclic voltammetry to obtain a stable metal nanocluster catalyst, wherein the guiding agent is a target product of a reaction that can be catalyzed by the metal nanocluster catalyst.
[0014] Preferably, the metal salt may be one or more of a Pt salt, an Au salt, an Ag salt, an Ir salt, a Pd salt and a Rh salt. More preferably, the metal salt may be one or more of H2PtCl6·xH2O, AuCl, AgNO3, IrCl3·3H2O, PdCl2, and RhCl3·3H2O.
[0015] Preferably, the metal chelate is a sugar, such as glucose. The metal chelate of the present invention can play a role in physically separating metal ions, so that the metal nanoclusters in the catalyst are evenly distributed on the surface of the carbon carrier without agglomeration, thereby maintaining the high dispersibility of the metal nanoclusters. The metal chelate can also be combined with the oxygen-rich carbon carrier through the interaction of oxygen-containing functional groups. In addition, it can be decomposed after roasting, and will not remain, so it will not affect the catalytic performance of the catalyst.
[0016] Preferably, the nitrogen source is one or more of melamine, dicyandiamide and urea. The nitrogen source of the present invention can play an anchoring role, and the uniformly distributed metal nanoclusters can be anchored on the surface of the carbon carrier through the combination of the N atoms modified on the surface of the carbon carrier and the metal ions in the metal salt at high temperature, so that the metal nanoclusters do not move or agglomerate during use, thereby maintaining the high dispersibility of the metal nanoclusters.
[0017] Preferably, the solvent is water, or a mixture of water and alcohols. More preferably, the solvent is a mixture of water and alcohols. Alcohols can eliminate the surface tension of the carbon material, so that the carbon material can be uniformly dispersed in the solvent together with other substances. Of course, the solvent of the present invention can also be any other solvent that can dissolve metal salts, metal chelates and nitrogen sources.
[0018] Preferably, the molar ratio of the metal salt, the metal chelate and the nitrogen source calculated by the molar amount of the metal atoms is 1: (1-5): (5-30), preferably 1: (1-5): (10-20). If the metal salt accounts for too little, the active sites are too few, the catalytic performance is not obvious, and the overall performance is the performance of the carbon material. If the metal salt accounts for too much, the size of the metal particles is greater than 2nm, and it is no longer a cluster. Relatively speaking, the atomic utilization rate is reduced, and the catalytic active sites are also reduced. Although the dosage increases, the catalytic performance will not increase accordingly, but will decrease, and cause unnecessary waste of precious metals.
[0019] Preferably, the method for preparing the metal salt solution comprises: respectively preparing the metal chelate and the nitrogen source into a metal chelate aqueous solution and a nitrogen source aqueous solution; adding the metal salt to the metal chelate aqueous solution at 20-30°C; after stirring, adding the nitrogen source aqueous solution and continuing to stir, thereby obtaining a metal salt solution. The method for preparing the metal salt solution of the present invention is conducive to the dispersion of the metal, while mixing and stirring all the components together will result in the following situation: the metal salt solution is unevenly dispersed, and even local complexation may occur, which is not conducive to the dispersion of the metal.
[0020] Preferably, the carbon material is one or more of carbon nanoparticles, conductive carbon black, lamp black carbon, carbon fiber, single-walled carbon nanotube, multi-walled carbon nanotube, graphene fiber, two-dimensional graphene paper, three-dimensional carbon foam and three-dimensional graphene aerogel. Preferably, the carbon material is one or more of single-walled carbon nanotube and multi-walled carbon nanotube. Carbon nanotube can pass through the protein wrapped outside the enzyme, directly contact with the active center prosthetic group of the enzyme, that is, no electron mediator is needed, which is conducive to the enzymatic reaction, so that the reaction is not limited by dissolved oxygen in the solution, and can also reduce the required potential of the sensor to a certain extent (after the working potential is reduced, the anti-interference ability of the sensor is enhanced). Preferably, the carbon material is modified by N atoms or S atoms. The modified carbon material can make the metal nanoclusters more stably dispersed on the carbon material. The carbon material of the present invention has the advantages of low cost, high conductivity, easy modification, etc., using carbon material as a carrier of metal nanoclusters, not only can reduce costs, but also can capture and surround the enzyme to a certain extent, thereby strengthening the fixation of the enzyme in the sensor that needs to combine the catalyst with the enzyme, and improving the stability of the product. In addition, carbon materials can also play the role of anti-interference layer and "mediator-free" electron transfer layer to a certain extent.
[0021] Preferably, after the metal salt solution is mixed with the carbon material and before freeze drying, ultrasound is performed. The ultrasound time is preferably 1-3 hours. The ultrasound power is preferably 60-150 W. After freeze drying, the solvent is completely removed.
[0022] Preferably, the inert atmosphere may be argon, nitrogen, helium or a mixture thereof.
[0023] Preferably, the calcination temperature may be 400°C-800°C, preferably 500-600°C. If the calcination temperature is too high, it will lead to the formation of larger metal particles, which will reduce the proportion of surface atoms and the reaction active sites, thereby reducing the catalytic performance of the catalyst; in addition, if the calcination temperature is too high, the nitrogen source will be directly sublimated, resulting in a reduction in the amount of nitrogen source in the catalyst. In addition, the sublimated nitrogen source will condense at the end of the pipeline and block the pipeline, which will bring danger to the experiment. If the calcination temperature is too low, the required calcination time will be too long, increasing the time cost. In addition, too low a temperature will also cause glucose or nitrogen source to not be completely pyrolyzed. If glucose remains, it will affect the detection results of the glucose sensor in the later stage. If the nitrogen source is not completely pyrolyzed, it will affect the anchoring effect of the metal.
[0024] Preferably, the heating rate can be 1-5°C / min, preferably 1-3°C / min. Heating too fast will cause temperature runaway, which will bring safety hazards to the experiment and will also cause metal sintering. Heating too slowly will take too long, increasing time costs. In addition, being at high temperature for a long time will cause the metal particles to grow.
[0025] Preferably, the calcination time may be 2-6 h, preferably 3-5 h.
[0026] Preferably, the guiding agent may be O2, H2, CO, CH4, H2O2, sodium nitrite, formic acid or acetic acid, etc. The guiding agent of the present invention is not limited to these, and any target product of the reaction that can be catalyzed by the metal nanocluster catalyst can be used. The guiding agent used can be determined according to the catalytic target of the metal nanocluster catalyst. For example, when the metal nanocluster catalyst is used to catalyze an oxidation reaction involving hydrogen peroxide, O2 can be used as a guiding agent to perform electrochemical redox treatment on the prepared precatalyst, and the catalyst prepared thereby has excellent catalytic performance for the oxidation reaction involving hydrogen peroxide.
[0027] In the present invention, the expression "reaction that can be catalyzed by the metal nanocluster catalyst" should be understood to refer to a chemical reaction carried out under the action of the metal nanocluster catalyst. The target product of the chemical reaction may be a gas, a liquid or a solid. The target product is a guiding agent used in the electrochemical redox treatment of the present invention. For example, when the concentration of hydrogen peroxide is detected under the action of the metal nanocluster catalyst, the oxidation product of the electrocatalytic hydrogen peroxide is O2, so in the electrochemical redox treatment process, O2 is used as a guiding agent. In the electrochemical redox treatment process, the guiding agent can guide the supported metal to reconstruct the exposed crystal face, increase the exposure ratio of the crystal face with catalytic activity, and thus improve the catalytic performance. However, the metal nanocluster pre-catalyst that has not been electrochemically redox treated has a disordered arrangement of its crystal faces, so that the proportion of exposed crystal faces with catalytic activity is relatively small, and the catalytic activity is relatively low.
[0028] Preferably, when the introducing agent is a gas (such as O2), the gas introducing agent is first introduced into the electrolyte to saturate the electrolyte. Preferably, the ventilation time may be 30-60 min; then, the electrochemical oxidation-reduction treatment is performed while continuously introducing the gas introducing agent. Preferably, the rate of introducing the gas introducing agent may be 1 ml / min to 200 ml / min, preferably 10 to 100 ml / min. The gas introducing agent of the present invention is in a saturated state in the electrolyte. On the one hand, it maximizes the amount of gas components dissolved. On the other hand, it facilitates the control of the amount of gas dissolved in the electrolyte to be constant, thereby making it possible to repeatedly prepare the catalyst.
[0029] Preferably, when the directing agent is liquid or solid, its concentration in the electrolyte may be 20 mM to 1 M, preferably 50 mM to 0.2 M.
[0030] Preferably, the scanning speed of the electrochemical redox treatment is 10 to 200 mV / s, preferably 50 to 100 mV / s. Preferably, the scanning potential window is -5 V to 5 V, preferably -4 to 4 V. Preferably, the number of scans is 1 to 500 times, preferably 50 to 200 times.
[0031] In the present invention, the metal nanocluster catalyst obtained after the electrochemical redox treatment can be directly used to detect the concentration of H2O2 or the concentration of biomolecules because it has been loaded on the working electrode.
[0032] Alternatively, the resulting metal nanocluster catalyst can be removed from the working electrode for use in catalytic reactions.
[0033] The present invention also provides a carbon-supported metal nanocluster catalyst obtained by the preparation method. The metal nanoclusters in the catalyst of the present invention are uniformly distributed on the carbon support, and the particle size can be 0.5-2nm, preferably 0.9-1.9nm. Preferably, based on the total mass of the metal nanocluster catalyst, the content of the metal element is 0.5-15% by weight, preferably 0.5-10% by weight.
[0034] The metal nanocluster catalyst of the present invention can reduce the overpotential required for the hydrogen peroxide oxidation reaction.
[0035] Since the metal nanoclusters of the present invention can be evenly and stably distributed on the carbon carrier, the surface atoms account for a large proportion and there are more reactive sites, so the amount of catalyst used can be reduced, and the amount of metal elements used can be reduced accordingly, thereby greatly reducing costs.
[0036] The present invention also provides a biosensor using the carbon-supported metal nanocluster catalyst.
[0037] In a first preferred embodiment of the present invention, the biosensor comprises:
[0038] basal layer;
[0039] A working electrode is disposed on the surface of the substrate layer; and
[0040] The electrocatalytic layer is arranged on the surface of the working electrode and includes the carbon-supported metal nanocluster catalyst.
[0041] Preferably, the base layer may be polyimide, polytetrafluoroethylene, polyethylene, polyvinyl chloride, polypropylene, polycarbonate, polyimide, polyethylene terephthalate, acrylonitrile-butadiene-styrene polymer or polymethyl methacrylate.
[0042] Preferably, the electrocatalytic layer is formed by a Nafion solution dispersion method, a screen printing method, an embedding method or a covalent bonding method.
[0043] The biosensor of the first preferred embodiment can be used to detect H2O2 concentration.
[0044] In organisms, H2O2 can act as a reactive oxygen species, involved in various physiological and pathological processes of cell proliferation, differentiation and migration; it can act as one of the most important signals of oxidative stress, such as the concentration of H2O2 in urine can be used as an indicator of systemic oxidative stress, for regulating renal function and diagnosing a variety of diseases. In addition, H2O2 is a key byproduct of a variety of enzymatic reactions in the body, such as enzymatic reactions involving glucose oxidase, cholesterol oxidase or lactate oxidase. Therefore, the sensitive detection of H2O2 in the nM and μM range is very important for biomedical fields such as health monitoring and disease diagnosis. The biosensor of the present invention uses the carbon-supported metal nanocluster catalyst, so that the sensitivity, detection limit and linear response range of the biosensor are significantly improved.
[0045] In addition, the existing catalysts for H2O2 catalysis usually contain high-loaded precious metal materials. Since the precious metal materials are expensive, their application in biosensors will bring heavy economic burdens to patients. The metal nanocluster catalyst of the present invention only contains low-loaded precious metals, and its main component is low-cost carbon material, thus greatly reducing the production cost of biosensors. In addition, the carbon material carrying metal nanoclusters in the present invention can not only serve as a carrier of metal nanoclusters, but also has certain catalytic activity for H2O2.
[0046] In a second preferred embodiment of the present invention, the biosensor comprises:
[0047] basal layer;
[0048] A working electrode is arranged on the surface of the substrate layer;
[0049] an electrocatalytic layer, disposed on the surface of the working electrode and comprising the carbon-supported metal nanocluster catalyst; and
[0050] The biocatalytic layer is arranged on the surface of the electrocatalytic layer and includes a bioenzyme.
[0051] Preferably, the biological enzyme is glucose oxidase, galactose oxidase, cholesterol oxidase, amino acid oxidase, alcohol oxidase, lactate oxidase or uricase.
[0052] Preferably, the biocatalytic layer is formed by an embedding method, an adsorption method, a covalent bonding method or a cross-linking method.
[0053] Preferably, the biosensor further comprises: a polymer layer disposed on the surface of the biocatalytic layer.
[0054] Preferably, the polymer layer can be polydimethylsiloxane, polyurethane, cellulose acetate, polycarbonate, polyurea cellulose acetate, Nafion, polyester sulfonic acid, polyvinyl alcohol, polyethylene glycol, polyimide, polytetrafluoroethylene or polyvinyl chloride, etc. The polymer layer has the following advantages: it can prevent larger molecules such as proteins from diffusing into the catalytic layer, thereby reducing interference with the electrode; regulate the ratio of glucose and oxygen entering the biocatalytic layer; prevent the loss of enzymes in the biocatalytic layer; and improve the biocompatibility of the sensor.
[0055] Since the biosensor according to the second preferred embodiment includes a biocatalytic layer, it can be used to detect the concentration of biomolecules such as blood glucose, galactose, cholesterol, amino acids, alcohols, lactic acid, or uric acid.
[0056] The carbon material of the present invention can be used not only as a carrier of metal nanoclusters, but also as a carrier of biological enzymes, which helps to enhance the fixation of enzymes, increase the loading capacity of biological enzymes, and increase the contact between enzymes and metal cluster catalysts, thereby extending the effective period of enzyme activity and thus extending the service life of biosensors.
[0057] Compared with the prior art, the present invention has the following beneficial effects:
[0058] 1. The present invention provides a method for preparing a carbon-supported metal nanocluster catalyst, which first forms a precatalyst by mixing a metal salt solution containing a metal chelate and a nitrogen source with a carbon material and freeze-drying and calcining, then combining the precatalyst with a working electrode and placing it in an electrolyte containing a guiding agent, and electrochemically redox treating the precatalyst by cyclic voltammetry to obtain a stable metal nanocluster catalyst. Treating the precatalyst by cyclic voltammetry can make the supported metal nanoclusters more evenly distributed and reduce agglomeration. In addition, during the electrochemical redox treatment, the guiding agent can guide the supported metal to reconstruct the exposed crystal plane, increase the exposure ratio of the crystal plane with catalytic activity, and thus improve the catalytic performance.
[0059] In addition, the electrochemical redox treatment of the present invention can stabilize the catalytic performance of the electrode, providing a guarantee for the subsequent commercial application of the electrode.
[0060] In addition, the preparation method of the metal nanocluster catalyst of the present invention is simple and repeatable.
[0061] 2. The metal nanocluster catalyst of the present invention has a large specific surface area and multiple active sites, and thus has excellent catalytic performance. It can be used not only to prepare hydrogen peroxide sensors, but also to prepare blood glucose sensors, etc., and has a wide range of applications.
[0062] 3. The preparation process of the biosensor of the present invention is repeatable, the equipment and raw materials are easy to obtain, the consistency of the catalytic performance of the sensor is easy to achieve, and it is also conducive to mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0063] Figure 1 This is a high-angle annular dark-field scanning transmission electron microscope (TEM) image of the Pt NCs2 sample prepared in Example 2.
[0064] Figure 2 This is a graph showing the change in current density over time obtained using the hydrogen peroxide biosensor of Example 5.
[0065] Figure 3 4 is a graph showing the relationship between the hydrogen peroxide concentration and the response current density obtained using the hydrogen peroxide biosensor of Example 5. DETAILED DESCRIPTION
[0066] In order to make the content of the present invention easier to understand, the technical scheme of the present invention is further described below in conjunction with specific embodiments, but the present invention is not limited thereto. All technologies realized based on the above content of the present invention are included in the scope that the present invention is intended to protect. Unless otherwise specified, the raw materials and reagents used in the examples are all commercially available products. The reagents, instruments or operating procedures not recorded herein are all contents that can be routinely determined by a person of ordinary skill in the art.
[0067] Example 1: Preparation of Pt nanocluster catalyst Pt NCs1
[0068] Weigh 1g of conductive carbon black material, 26.5mg of chloroplatinic acid hexahydrate (H2PtCl6·6H2O), 9.3mg of glucose and 10.77mg of melamine (the molar ratio of chloroplatinic acid hexahydrate, glucose and melamine calculated by the molar amount of nitrogen atoms is 1:1:10). Dissolve glucose in 30mL of deionized water to prepare a glucose aqueous solution, and dissolve melamine in 30mL of deionized water to prepare a melamine aqueous solution. Add chloroplatinic acid hexahydrate to the glucose aqueous solution and react for 0.5h, then add the melamine aqueous solution and continue to react for 0.5h. Then add conductive carbon black to the solution and ultrasonicate at 100W for 1h. Then freeze-dry until the deionized water is completely removed. Finally, put the sample into a tube furnace and heat it to 500℃ at a rate of 2℃ / min in a N2 atmosphere with a flow rate of 100mL / min, and keep it for 5h to obtain a precatalyst. Combine the prepared precatalyst with the working electrode and then connect them using a three-electrode system. Pass O2 into the electrolyte (phosphate buffer solution with pH = 7.4 and a concentration of 30mM) at a rate of 100ml / min for 30min to saturate the electrolyte with O2 (the oxidation product of electrocatalytic hydrogen peroxide is O2, so O2 is used as the treatment atmosphere for this precatalyst). Then, perform cyclic voltammetry of the electrode while continuing to ventilate at a rate of 50ml / min, with a scan rate of 50mV / s, 100 scans, and a scan range of -2V to 2V. After completion, Pt NCs1 is obtained.
[0069] TEM characterization showed that the particle size of the Pt nanoclusters supported on the conductive carbon black was 0.9 nm, and inductively coupled plasma (ICP) analysis results showed that the Pt content in the sample was 0.89 wt %.
[0070] Example 2: Preparation of Pt nanocluster catalyst Pt NCs2
[0071] Weigh 1g activated carbon nanoparticles, 0.13g chloroplatinic acid hexahydrate, 0.23g glucose and 80.81mg dicyandiamide (the molar ratio of chloroplatinic acid hexahydrate, glucose and dicyandiamide calculated by the molar amount of nitrogen atoms is 1:5:15). Glucose was dissolved in 40mL deionized water to prepare a glucose aqueous solution, and dicyandiamide was dissolved in 30mL deionized water to prepare a dicyandiamide aqueous solution. Chloroplatinic acid hexahydrate was added to the glucose aqueous solution, reacted for 1h, and then the dicyandiamide aqueous solution was added and the reaction continued for 1h. Then the activated carbon nanoparticles were added to the solution, and ultrasonicated at 150W for 1h. Then freeze-dried until the deionized water was completely removed. Then the sample was placed in a tubular furnace, heated to 600℃ at a rate of 2℃ / min in a N2 atmosphere with a flow rate of 200mL / min, and maintained for 3h to obtain a precatalyst. The prepared precatalyst was combined with a working electrode and then connected using a three-electrode system. O2 was introduced into the electrolyte (phosphate buffer solution with pH = 7.4 and a concentration of 30 mM) at a rate of 100 ml / min for 30 min to saturate the electrolyte with O2. Then, the electrode was subjected to cyclic voltammetry treatment with continuous aeration at a rate of 10 ml / min, a scan rate of 10 mV / s, a scan number of 50 times, and a scan range of -2 V to 2 V. After completion, Pt NCs2 was obtained.
[0072] Figure 1 The transmission electron microscope image of the obtained Pt NCs2 sample shows that Pt is a nanocluster particle evenly distributed on the activated carbon. After TEM data analysis, the size of the Pt nanocluster particles supported on the activated carbon is about 1.7nm. The ICP results show that the Pt content in the sample is 4.01% by weight.
[0073] Example 3: Preparation of Au nanocluster catalyst Au NCs1
[0074] Weigh 1g S-doped carbon nanotube material, 82.60mg gold chloride (AuCl), 64.03mg glucose and 213.44mg urea (the molar ratio of gold chloride, glucose and urea calculated by the molar amount of nitrogen atoms is 1:1:20). Dissolve glucose in 30mL deionized water to prepare a glucose aqueous solution, and dissolve urea in 20mL deionized water to prepare a urea aqueous solution. Add gold chloride to the glucose aqueous solution, react for 2h, then add the urea aqueous solution and continue to react for 2h. Then add the S-doped carbon nanotube material to the solution, ultrasonic 60W, 1h. Then freeze-dry until the deionized water is completely removed. Then put the sample into a tube furnace, heat it to 400℃ at a rate of 1℃ / min in a He atmosphere with a flow rate of 100mL / min, and keep it for 6h to obtain a precatalyst. Combine the prepared precatalyst with the working electrode and then connect it using a three-electrode system. O2 was introduced into the electrolyte (phosphate buffer solution with pH = 7.4 and a concentration of 30 mM) at a rate of 100 ml / min for 30 min to saturate the electrolyte with O2. Then, the electrode was subjected to cyclic voltammetry treatment with continuous aeration at a rate of 200 ml / min, a scan rate of 50 mV / s, a scan number of 200 times, and a scan range of -3 V to 3 V. After completion, Au NCs1 was obtained.
[0075] TEM characterization showed that the size of the Au nanocluster particles supported on the carbon nanotubes was 1.8 nm, and ICP results showed that the Au content in the sample was 6.12 wt %.
[0076] Example 4: Preparation of Ir nanocluster catalyst Ir NCs1
[0077] Weigh 1g of graphene material, 0.28g of iridium chloride trihydrate (IrCl3·3H2O), 0.28g of glucose and 0.33g of melamine (the molar ratio of iridium chloride trihydrate, glucose and melamine calculated by the molar amount of nitrogen atoms is 1:2:20). Dissolve glucose in 50mL of deionized water to prepare a glucose aqueous solution, and dissolve melamine in 50mL of deionized water to prepare a melamine aqueous solution. Add iridium chloride trihydrate to the glucose aqueous solution, react for 1h, then add the melamine aqueous solution and continue to react for 1h. Then add the graphene material to the solution, ultrasonicate at 100W for 1h. Then freeze-dry until the deionized water is completely removed. Then put the sample into a tube furnace, heat it to 800℃ at a rate of 3℃ / min in an Ar atmosphere with a flow rate of 150mL / min, and keep it for 2h to obtain a precatalyst. Combine the prepared precatalyst with the working electrode and then connect it using a three-electrode system. O2 was introduced into the electrolyte (phosphate buffer solution with pH = 7.4 and a concentration of 30 mM) at a rate of 100 ml / min for 30 min to saturate the electrolyte with O2. Then, the electrode was subjected to cyclic voltammetry treatment with continuous aeration at a rate of 200 ml / min, a scan rate of 10 mV / s, a scan number of 50 times, and a scan range of -2 V to 2 V. After completion, Ir NCs1 was obtained.
[0078] TEM characterization showed that the size of the Ir nanocluster particles supported on graphene was 1.9 nm, and ICP results showed that the Ir content in the sample was 9.09 wt%.
[0079] Example 5: Construction of hydrogen peroxide biosensor
[0080] The working electrode was modified by the Nafion solution dispersion method. A 0.5% nafion aqueous solution was prepared. 20 mg of the precatalyst of Example 2, i.e., the Pt nanocluster catalyst, was weighed and added to 1 mL of the nafion aqueous solution, and then ultrasonicated for 30 min to make it evenly distributed. 1 μL of the prepared slurry was taken with a pipette and applied to the surface of the working electrode in the three-electrode system. Then the three-electrode system was used for connection. O2 was introduced into the electrolyte (phosphate buffer solution with pH = 7.4, concentration of 30 mM) at a rate of 100 ml / min for 30 min to saturate the electrolyte with O2. Then, the electrode was subjected to cyclic voltammetry treatment while continuously aerating at a rate of 10 ml / min, with a scan rate of 10 mV / s, a scan number of 50 times, and a scan range of -2 V to 2 V. After completion, it was rinsed with deionized water and dried at 40°C for standby use.
[0081] Test the response performance of the constructed electrode to hydrogen peroxide. The test process is to assemble a three-electrode system with Pt as the counter electrode, Ag / AgCl as the reference electrode, and the modified electrode as the working electrode. The three-electrode system is placed in an electrolyte (30mM phosphate buffer solution, pH=7.4), and a working potential of 0.55V vs Ag / AgCl is applied. A certain concentration of hydrogen peroxide is added every 5 minutes, so that the concentration of hydrogen peroxide in the final solution increases with a gradient of 30μM. The chronoamperometry is used to record the change in current density as hydrogen peroxide is continuously added, such as Figure 2 shown.
[0082] use Figure 2 The data plotted Figure 3 The relationship curve between hydrogen peroxide concentration and response current density. It can be seen from the figure that at low substrate concentration, that is, 0-180 μM, the curve satisfies the linear relationship. The detection limit is 15.82 μM (signal-to-noise ratio S / N=3), and the detection range is 5 μM-3600 μM.
[0083] According to the same method, the metal cluster catalysts prepared in Examples 1-4 were used to modify the working electrodes respectively to prepare hydrogen peroxide sensors, and the hydrogen peroxide detection performance thereof is shown in Table 1 below.
[0084] Table 1
[0085]
[0086] Example 6: Construction of blood glucose sensor
[0087] The working electrode was modified by the Nafion solution dispersion method. A 0.5% nafion phosphate buffer solution was prepared. 20 mg of the precatalyst of Example 2, i.e., the Pt nanocluster catalyst, was weighed and added to 1 mL of the nafion phosphate buffer solution, and then ultrasonicated for 30 minutes to make it evenly distributed. 1 μL of the prepared slurry was taken with a pipette, applied to the surface of the working electrode in the three-electrode system, and then connected using the three-electrode system. O2 was introduced into the electrolyte at a rate of 100 ml / min for 30 minutes to saturate the electrolyte with O2. The electrode was then subjected to cyclic voltammetry treatment while continuing to ventilate at a rate of 10 ml / min, with a scan rate of 10 mV / s, 50 scans, and a scan range of -2 V to 2 V. After completion, it was rinsed with deionized water and dried at 40°C for use. At 4°C, the Pt NCs2-modified electrode was immersed in 5 mg mL -1 The cells were incubated in PBS buffer solution of glucose oxidase for 48 h, washed with PBS solution, and stored at 4°C for future use.
[0088] The metal cluster catalysts prepared in Examples 1-4 were used to modify the working electrodes respectively to prepare blood glucose sensors, and the glucose detection performance thereof is shown in Table 2 below.
[0089] Table 2
[0090]
[0091] Comparative Example 1: Preparation of Pt nanocluster catalyst Pt NCs1-A
[0092] Weigh 1g of conductive carbon black material, 26.5mg of chloroplatinic acid hexahydrate and 10.77mg of melamine (the molar ratio of chloroplatinic acid hexahydrate calculated by molar amount of platinum atoms to melamine calculated by molar amount of nitrogen atoms is 1:10). Melamine was dissolved in 60mL of deionized water to prepare a melamine aqueous solution. Chloroplatinic acid hexahydrate was added to the melamine aqueous solution and reacted for 0.5h. Then the conductive carbon black was added to the solution and ultrasonicated at 100W for 1h. Then freeze-dried until the deionized water was completely removed. Finally, the sample was placed in a tubular furnace and heated to 500℃ at a rate of 2℃ / min in a N2 atmosphere with a flow rate of 100mL / min, and maintained for 5h to obtain a precatalyst. The prepared precatalyst was combined with the working electrode and then connected using a three-electrode system. O2 was introduced into the electrolyte (phosphate buffer solution with pH = 7.4 and a concentration of 30 mM) at a rate of 100 ml / min for 30 min to saturate the electrolyte with O2 (the oxidation product of electrocatalytic hydrogen peroxide is O2, so O2 is used as the treatment atmosphere of the pre-catalyst). Then, the electrode was subjected to cyclic voltammetry treatment at a rate of 50 ml / min while continuous ventilation was performed, with a scan rate of 50 mV / s, 100 scans, and a scan range of -2 V to 2 V. After completion, Pt NCs1-A was obtained.
[0093] TEM characterization showed that the particle size of the Pt nanoclusters supported on the conductive carbon black was 3.4 nm, and ICP analysis results showed that the Pt content in the sample was 0.87 wt %.
[0094] Comparative Example 2: Preparation of Pt nanocluster catalyst Pt NCs1-B
[0095] Weigh 1g of conductive carbon black material, 26.5mg of chloroplatinic acid hexahydrate and 9.3mg of glucose (the molar ratio of chloroplatinic acid hexahydrate and glucose calculated by the molar amount of platinum atoms is 1:1). Dissolve glucose in 60mL of deionized water to prepare a glucose aqueous solution. Add chloroplatinic acid hexahydrate to the glucose aqueous solution and react for 0.5h. Then add conductive carbon black to the solution and ultrasonicate at 100W for 1h. Then freeze-dry until the deionized water is completely removed. Finally, place the sample in a tubular furnace, heat it to 500℃ at a rate of 2℃ / min in a N2 atmosphere with a flow rate of 100mL / min, and keep it for 5h to obtain a precatalyst. Combine the prepared precatalyst with the working electrode and then connect it using a three-electrode system. O2 was introduced into the electrolyte (phosphate buffer solution with pH = 7.4 and a concentration of 30 mM) at a rate of 100 ml / min for 30 min to saturate the electrolyte with O2 (the oxidation product of electrocatalytic hydrogen peroxide is O2, so O2 is used as the treatment atmosphere of this pre-catalyst). Then, the electrode was subjected to cyclic voltammetry treatment while continuously aerating at a rate of 50 ml / min, with a scan rate of 50 mV / s, 100 scans, and a scan range of -2 V to 2 V. After completion, Pt NCs1-B was obtained.
[0096] TEM characterization showed that the particle size of the Pt nanoclusters supported on the conductive carbon black was 5.1 nm, and ICP analysis results showed that the Pt content in the sample was 0.91 wt %.
[0097] Comparative Example 3: Preparation of Pt Nanocluster Catalyst Pt NCs1-C
[0098] Weigh 1g of conductive carbon black material and 26.5mg of chloroplatinic acid hexahydrate. Add chloroplatinic acid hexahydrate to 60mL of deionized water. Then add conductive carbon black to the solution and ultrasonicate at 100W for 1h. Then freeze-dry until the deionized water is completely removed. Finally, place the sample in a tubular furnace, heat it to 500℃ at a rate of 2℃ / min in a N2 atmosphere with a flow rate of 100mL / min, and keep it for 5h to obtain a precatalyst. Combine the prepared precatalyst with the working electrode and then connect it using a three-electrode system. Pass O2 into the electrolyte (phosphate buffer solution with pH=7.4, concentration of 30mM) at a rate of 100ml / min for 30min to saturate the electrolyte with O2 (the oxidation product of electrocatalytic hydrogen peroxide is O2, so O2 is used as the treatment atmosphere of this precatalyst). Then, the electrode was subjected to cyclic voltammetry treatment under continuous ventilation at a speed of 50 ml / min, with a scan rate of 50 mV / s, a scan number of 100 times, and a scan range of -2 V to 2 V. After completion, Pt NCs1-C was obtained.
[0099] TEM characterization showed that the particle size of the Pt nanoclusters supported on the conductive carbon black was 6.4 nm, and ICP analysis results showed that the Pt content in the sample was 0.83 wt %.
[0100] Comparative Example 4: Preparation of Pt nanocluster catalyst Pt NCs1-D
[0101] Weigh 1g of conductive carbon black material, 26.5mg of chloroplatinic acid hexahydrate, 9.3mg of glucose and 1.1mg of melamine (the molar ratio of chloroplatinic acid hexahydrate, glucose and melamine calculated by the molar amount of nitrogen atoms is 1:1:1). Glucose was dissolved in 30mL of deionized water to prepare a glucose aqueous solution, and melamine was dissolved in 30mL of deionized water to prepare a melamine aqueous solution. Chloroplatinic acid hexahydrate was added to the glucose aqueous solution and reacted for 0.5h, then the melamine aqueous solution was added and the reaction continued for 0.5h. Then the conductive carbon black was added to the solution and ultrasonicated at 100W for 1h. Then freeze-dried until the deionized water was completely removed. Finally, the sample was placed in a tubular furnace and heated to 500℃ at a rate of 2℃ / min in a N2 atmosphere with a flow rate of 100mL / min, and maintained for 5h to obtain a precatalyst. The prepared precatalyst was combined with the working electrode and then connected using a three-electrode system. O2 was introduced into the electrolyte (phosphate buffer solution with pH = 7.4 and a concentration of 30 mM) at a rate of 100 ml / min for 30 min to saturate the electrolyte with O2 (the oxidation product of electrocatalytic hydrogen peroxide is O2, so O2 is used as the treatment atmosphere of this pre-catalyst). Then, the electrode was subjected to cyclic voltammetry treatment at a rate of 50 ml / min while continuous ventilation was performed, with a scan rate of 50 mV / s, 100 scans, and a scan range of -2 V to 2 V. After completion, Pt NCs1-D was obtained.
[0102] TEM characterization showed that the particle size of the Pt nanoclusters supported on the conductive carbon black was 6.1 nm, and inductively coupled plasma (ICP) analysis results showed that the Pt content in the sample was 0.91 wt %.
[0103] Comparative Example 5: Preparation of Pt nanocluster catalyst Pt NCs1-E
[0104] Weigh 1g of conductive carbon black material, 26.5mg of chloroplatinic acid hexahydrate, 55.4mg of glucose and 43.1mg of melamine (the molar ratio of chloroplatinic acid hexahydrate, glucose and melamine calculated by the molar amount of nitrogen atoms is 1:6:40). Glucose was dissolved in 30mL of deionized water to prepare a glucose aqueous solution, and melamine was dissolved in 30mL of deionized water to prepare a melamine aqueous solution. Chloroplatinic acid hexahydrate was added to the glucose aqueous solution and reacted for 0.5h, then the melamine aqueous solution was added and the reaction continued for 0.5h. Then the conductive carbon black was added to the solution and ultrasonicated at 100W for 1h. Then freeze-dried until the deionized water was completely removed. Finally, the sample was placed in a tubular furnace and heated to 500℃ at a rate of 2℃ / min in a N2 atmosphere with a flow rate of 100mL / min, and maintained for 5h to obtain a precatalyst. The prepared precatalyst was combined with a working electrode and then connected using a three-electrode system. O2 was introduced into the electrolyte (phosphate buffer solution with pH = 7.4 and a concentration of 30 mM) at a rate of 100 ml / min for 30 min to saturate the electrolyte with O2 (the oxidation product of electrocatalytic hydrogen peroxide is O2, so O2 is used as the treatment atmosphere of this pre-catalyst). Then, the electrode was subjected to cyclic voltammetry treatment at a rate of 50 ml / min while continuous ventilation was performed, with a scan rate of 50 mV / s, 100 scans, and a scan range of -2 V to 2 V. After completion, Pt NCs1-E was obtained.
[0105] TEM characterization showed that the particle size of the Pt nanoclusters supported on the conductive carbon black was 5.3 nm, and inductively coupled plasma (ICP) analysis results showed that the Pt content in the sample was 0.81 wt %.
[0106] Comparative Example 6: Preparation of Pt nanocluster catalyst Pt NCs2-F
[0107] Weigh 1g of conductive carbon black material, 26.5mg of chloroplatinic acid hexahydrate (H2PtCl6·6H2O), 9.3mg of glucose and 10.77mg of melamine (the molar ratio of chloroplatinic acid hexahydrate, glucose and melamine calculated by the molar amount of nitrogen atoms is 1:1:10). Dissolve glucose in 30mL of deionized water to prepare a glucose aqueous solution, and dissolve melamine in 30mL of deionized water to prepare a melamine aqueous solution. Add chloroplatinic acid hexahydrate to the glucose aqueous solution and react for 0.5h, then add the melamine aqueous solution and continue to react for 0.5h. Then add conductive carbon black to the solution and ultrasonicate at 100W for 1h. Then freeze-dry until the deionized water is completely removed. Finally, place the sample in a tube furnace and heat it to 500℃ at a rate of 2℃ / min in a N2 atmosphere with a flow rate of 100mL / min, and keep it for 5h to obtain Pt NCs2-F.
[0108] TEM characterization showed that the particle size of the Pt nanoclusters supported on the conductive carbon black was 1.6 nm, and inductively coupled plasma (ICP) analysis results showed that the Pt content in the sample was 3.99 wt %.
[0109] Comparative Example 7: Construction of Hydrogen Peroxide Biosensor
[0110] According to the method of Example 5, the working electrodes were modified respectively with the metal cluster catalysts prepared in Comparative Examples 1-6 to prepare a hydrogen peroxide sensor, and its hydrogen peroxide detection performance is shown in Table 3 below.
[0111] Table 3
[0112]
[0113] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. A biosensor, characterized in that: A carbon-supported metal nanocluster catalyst is used; the particle size of the metal nanocluster is 0.5-2 nm; the content of the metal element is 0.5-15 wt % based on the total mass of the metal nanocluster catalyst; The preparation method of the carbon-supported metal nanocluster catalyst comprises: preparing a metal salt solution, wherein the metal salt solution comprises a metal salt, a metal chelate, a nitrogen source and a solvent; mixing the metal salt solution with the carbon material and freeze-drying the mixture to obtain a freeze-dried sample; calcining the freeze-dried sample under an inert atmosphere to obtain a carbon-supported metal nanocluster precatalyst; and The metal nanocluster precatalyst is combined with a working electrode and placed in an electrolyte containing a guiding agent, and the metal nanocluster precatalyst is subjected to electrochemical oxidation-reduction treatment by cyclic voltammetry to obtain a stable metal nanocluster catalyst, wherein the guiding agent is a target product of a reaction that can be catalyzed by the metal nanocluster catalyst; the guiding agent is O2, H2, CO, CH4, H2O2, sodium nitrite, formic acid or acetic acid.
2. The biosensor according to claim 1, characterized in that The molar ratio of the metal salt, the metal chelate, and the nitrogen source calculated as a molar amount of the metal atom is 1:(1-5):(5-30).
3. The biosensor according to claim 1 or 2, characterized in that: The metal salt is one or more of a Pt salt, an Au salt, an Ag salt, an Ir salt, a Pd salt and a Rh salt; The metal chelate is a sugar; The nitrogen source is one or more of melamine, dicyandiamide and urea; The solvent is water, or a mixture of water and alcohol; The carbon material is one or more of carbon nanoparticles, conductive carbon black, lamp black carbon, carbon fibers, single-walled carbon nanotubes, multi-walled carbon nanotubes, graphene fibers, two-dimensional graphene paper, three-dimensional carbon foam and three-dimensional graphene aerogel.
4. The biosensor according to claim 3, characterized in that The carbon material is one or more of single-walled carbon nanotubes and multi-walled carbon nanotubes.
5. The biosensor according to claim 3, characterized in that The carbon material is modified with N atoms or S atoms.
6. The biosensor according to claim 1, characterized in that The scanning speed of the electrochemical redox treatment is 10 to 200 mV / s; the scanning potential window is -5V to 5V, and the scanning times are 1 to 500 times.
7. The biosensor according to claim 1, characterized in that include: basal layer; A working electrode is arranged on the surface of the substrate layer; as well as The electrocatalytic layer is arranged on the surface of the working electrode and includes the carbon-supported metal nanocluster catalyst.
8. The biosensor according to claim 7, characterized in that Also includes: The biocatalytic layer is arranged on the surface of the electrocatalytic layer and includes a bioenzyme.
9. The biosensor according to claim 8, characterized in that The biological enzyme is glucose oxidase, galactose oxidase, cholesterol oxidase, amino acid oxidase, alcohol oxidase, lactate oxidase or uricase.
10. The biosensor according to claim 8, characterized in that Also includes: The polymer layer is arranged on the surface of the biocatalytic layer.
11. Use of the biosensor according to any one of claims 1 to 7 for detecting H2O2 concentration.
12. Use of the biosensor according to any one of claims 8 to 10 for detecting the concentration of biomolecules.
13. The use according to claim 12, characterized in that The biomolecule is blood glucose, galactose, cholesterol, amino acid, alcohol, lactic acid or uric acid.