Semi-hot-melt flange and manufacturing method thereof
By adding support blocks to the semi-hot-melt flange and using HDPE/LLDPE hybrid materials and fillers such as quartz fiber and talc powder, the mechanical and corrosion-resistant problems of the hot-melt flange on the polyethylene storage tank are solved and the sealing performance is improved. and service life.
Patent Information
- Application Number
- CN202110714364.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-06-26
AI Technical Summary
Existing hot-melt flanges made of polymer materials have poor mechanical strength and insufficient acid and alkali corrosion resistance during use. They are prone to corrosion on polyethylene high-strength storage tanks, causing leakage and damage. They are also prone to cracking under external stress, affecting sealing. Effect.
Using a semi-hot melt flange design, the pressure-bearing strength is increased by setting up support blocks in the support part, and combined with a mixed material of HDPE and LLDPE, adding reinforcing fillers such as quartz fiber and talc powder, adjusting the melt index and filler ratio, and improving environmental stress resistance and bonding properties.
The mechanical strength, acid and alkali corrosion resistance and sealing effect of the semi-hot melt flange are significantly improved, the service life is extended, the stability to external stress is enhanced, and the risk of leakage is reduced.
Smart Images

Figure CN114811222B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field classified as B65D90 / 00, and specifically relates to a semi-hot-melt flange and a manufacturing method thereof. Background Art
[0002] Flange, also known as flange flange or flange. Flanges can be used at the inlet and outlet ends of storage tanks, and can also be used to connect pipe ends, and have good sealing and connection functions. Most existing flanges are made of metal materials, such as carbon steel, chrome steel, and stainless steel flanges. When used, metal flanges need to be welded to the inlet and outlet ends of the equipment or one end of the pipeline. However, for composite material storage tanks, because the composite material contains polymer materials, which are incompatible with metals, metal flanges cannot be welded to the storage tank. Therefore, hot-melt flanges made of polymer materials came into being. The hot-melt flanges are bonded to the composite material storage tank body by hot melting, thereby achieving a sealed connection.
[0003] Polyethylene high-strength storage tanks for acidic or alkaline liquids are generally connected and sealed with hot-melt flanges. However, the existing hot-melt flanges made of polymer materials have poor mechanical strength and poor acid and alkali corrosion resistance. In particular, the hot-melt flanges used on the upper part of polyethylene high-strength storage tanks will be corroded during long-term use, resulting in leakage and damage, causing great economic losses and even causing certain harm to the operator's body. Therefore, a hot-melt flange with high mechanical strength and good acid and alkali corrosion resistance is urgently needed. Summary of the invention
[0004] For purposes of the following detailed description, it is to be understood that the invention may assume various alternative variations and step sequences, except where expressly specified to the contrary.
[0005] The melt index in the present invention refers to the melt index obtained by ASTM D-1238 test method at 190° C. and 2.16 kg.
[0006] A semi-hot-melt flange comprises an annular flange with a center hole, N connecting holes are formed on the annular flange, X sealing gasket grooves are formed on the outer side of the center hole of the annular flange, an annular protrusion is formed on the outer side of the sealing gasket groove, wherein N≥2, X≥1; a supporting portion, the supporting portion extends to one side from the circumference of the center hole of the annular flange, M supporting blocks are formed on the upper half of the supporting portion, one end of the supporting block is in contact with the annular flange, wherein M≥1.
[0007] The inventors provide a support block on the circumference of the support portion, one end of which is connected to the annular flange. By providing the support block, the pressure bearing strength of the semi-melt flange is increased, and the service life of the semi-melt flange is increased. When the semi-melt flange is in use, the lower half of the support portion is heated and bonded to the storage tank to be packaged, which plays a role in further sealing and guiding.
[0008] As a preferred technical solution, 4, 5, 6, 7, 8, 9 or 10 support blocks may be provided on the circumference of the support portion.
[0009] As a preferred technical solution, the cross-section of the support block is a Y-gon, where Y≥3.
[0010] As a preferred technical solution, the cross-section of the support block can be a triangle, a quadrilateral, a pentagon, a hexagon, a heptagon, an octagon, a nonagon, or a decagon, and the quadrilateral can be a square, a rectangle, a parallelogram, or a trapezoid.
[0011] As a preferred technical solution, the raw materials for preparing the semi-hot-melt flange include, by weight, at least 15-40 parts of HDPE, 15-30 parts of LLDPE, 1-6 parts of reinforcing filler, 0.5-1.5 parts of silane coupling agent, 0.5-1 parts of lubricant and 1-2 parts of light stabilizer.
[0012] As a preferred technical solution, the melt index of the HDPE is 7-8 g / 10 min, and the melt index of the LLDPE is 1.5-2.5 g / 10 min.
[0013] The existing plastic storage tanks are basically made of polyethylene. In order to improve the compatibility of the semi-hot-melt flange with the storage tank base during hot-melting, the inventors selected polyethylene as the main material of the semi-hot-melt flange. HDPE has good acid resistance, alkali resistance and corrosion resistance to various salts, and HDPE has good chemical stability. However, the inventors found that the semi-hot-melt flange made of HDPE will be subjected to certain external stresses during the actual use process as the storage tank body is transported. The semi-hot-melt flange made of HDPE has poor environmental stress cracking resistance. Flange cracks will appear in the case of long-term use, causing the stored liquid to leak from the gap. The inventors unexpectedly found that by adding a certain amount of LLDPE, the environmental stress cracking resistance of the semi-hot-melt flange can be improved, the impact strength and tear resistance of the hot-melt flange can be improved, and the sealing effect of the semi-hot-melt flange can be improved. However, since the hot-melt temperature of LLDPE is lower than the hot-melt point of HDPE, the semi-hot-melt flange cannot be uniformly hot-melted with the storage tank body during hot-melt bonding, which reduces the bonding performance between the semi-hot-melt flange and the storage tank body. The inventor unexpectedly discovered that when using HDPE with a melt index of 7-8g / 10min and LLDPE with a melt index of 1.5-2.5g / 10min, the uniformity and bonding performance of the semi-hot-melt flange during hot-melt bonding can be improved by adjusting the melt fluidity. However, the full hot-melt flange formed by mixed injection molding of HDPE and LLDPE has poor deformation resistance when subjected to external pressure.
[0014] As a preferred technical solution, the reinforcing filler is selected from at least one of calcium carbonate, mica powder, quartz fiber, wollastonite, talc, kaolin, asbestos, calcium sulfate, barium sulfate, alumina, silicon dioxide, zirconium oxide, magnesium oxide and sodium silicate.
[0015] As a preferred technical solution, the reinforcing filler is a mixture of talcum powder and quartz fiber, and the weight ratio of the mica powder, talcum powder and quartz fiber is 1:(3-5).
[0016] As a preferred technical solution, the mesh size of the talcum powder is 1000-1500 meshes.
[0017] As a preferred technical solution, the mesh size of the talcum powder is 1250 meshes.
[0018] As a preferred technical solution, the diameter of the quartz fiber is 5-10 um, and the length of the quartz fiber is 20-350 um.
[0019] In order to improve the dimensional stability of the semi-hot-melt flange under external force conditions, the inventor added a certain amount of quartz fiber. The inventor found that quartz fiber can significantly improve the dimensional stability and mechanical strength of the semi-hot-melt flange, but the mechanical strength of the semi-hot-melt flange is unevenly improved. The inventor believes that the possible reason is that the fibers in the quartz fiber are three-dimensional structures, and there will be gaps and steric hindrances between each other, which leads to uneven improvement of the mechanical properties of the semi-hot-melt flange. The inventor unexpectedly found that when a certain amount of talcum powder is added, especially when 1250 mesh talcum powder is added, the mechanical properties of the semi-hot-melt flange will be uniformly improved, and the smoothness of the semi-hot-melt flange can be further improved, thereby improving the sealing of the semi-hot-melt flange during bonding. The inventor believes that the possible reason is that talcum powder can be interspersed in the gaps of quartz fiber, making up for the gaps between quartz fibers, thereby improving the mechanical uniformity of the semi-hot-melt flange, reducing the roughness of the semi-hot-melt flange, and improving the smoothness of the semi-hot-melt flange. However, if the mesh number of talcum powder is too small, it cannot improve the mechanical properties of the semi-hot-melt flange. If the mesh number of talcum powder is too large, it will increase the roughness of the semi-hot-melt flange, resulting in an uneven sealing connection surface of the semi-hot-melt flange, and even cause leakage of the hot-melt flange. If the amount of quartz fiber added is too much, it will also reduce the toughness and weather resistance of the semi-hot-melt flange.
[0020] As a preferred technical solution, the lubricant is selected from at least one of calcium stearate, magnesium stearate, zinc stearate, butyl stearate, oleamide and ethylene bisstearamide.
[0021] As a preferred technical solution, the lubricant is ethylene bisstearamide.
[0022] The inventors improved the processability and smoothness of the semi-hot-melt flange by adding a certain amount of ethylene bisstearamide.
[0023] A second aspect of the present invention provides a method for preparing the semi-hot-melt flange, wherein the semi-hot-melt flange is produced by injection molding.
[0024] Beneficial effects:
[0025] (1) The inventor provides a support block on the circumference of the support portion, one end of which is connected to the annular flange. By providing the support block, the pressure bearing strength of the full hot-melt flange is improved, and the service life of the full hot-melt flange is increased.
[0026] (2) The inventors have made the hot-melt flange have better acid resistance, alkali resistance and corrosion resistance to various salts by mixing HDPE and LLDPE with a certain melt index, improved the environmental stress cracking resistance of the semi-hot-melt flange, and made the semi-hot-melt flange have uniform hot melt properties.
[0027] (3) The inventors have enhanced the addition of fillers to make the full hot-melt flange have better mechanical strength, wear resistance, weather resistance, dimensional stability and smoothness, thereby improving the use effect and sealing effect of the semi-hot-melt flange. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a front view structural schematic diagram of the semi-hot-melt flange in Example 1.
[0029] Figure 2 It is a schematic diagram of the top view of the semi-hot-melt flange in Example 1.
[0030] Figure 3 It is a schematic diagram of the overall structure of the semi-hot-melt flange in Example 1.
[0031] 1- annular flange, 2- supporting block, 3- supporting portion, 4- annular protrusion, 5- connecting hole, 6- sealing gasket groove, 7- center hole. DETAILED DESCRIPTION
[0032] Example 1
[0033] like Figure 1-Figure 3 As shown, a semi-hot-melt flange comprises an annular flange 1 with a center hole 7, and the annular flange 1 is provided with 8 connecting holes 5, through which the semi-hot-melt flange is connected to other parts, and three sealing gasket grooves 6 are provided on the outer side of the center hole 7 of the annular flange 1, and a sealing gasket is placed in the sealing gasket groove 6 to improve the sealing performance of the hot-melt flange, and an annular protrusion 4 is provided on the circumference of the sealing gasket groove 6 to further improve the convenience of use and sealing performance of the hot-melt flange; a support portion 3, the support portion 3 extends from the circumference of the center hole 7 of the annular flange 1 to one side, and the support portion 3 gradually decreases in diameter from one side of the annular flange 1 to the outside, and is in a truncated cone shape. Four support blocks 2 are provided on the circumference of the support portion 3, and one end of the support block 2 abuts against the annular flange 1. By setting the support block 2, the support capacity and service life of the semi-hot-melt flange are improved. The cross section of the support block 2 in the technical solution is a quadrilateral, and the quadrilateral is a trapezoid. When the semi-hot-melt flange is in use, the lower part of the support portion 3 on which the support block 2 is mounted is heated to become partially molten and bonded to the storage tank to be packaged, thereby achieving sealing of the storage tank through the semi-molten flange.
[0034] Example 2
[0035] The structure of the semi-hot-melt flange in this embodiment is the same as that of the semi-hot-melt flange in Example 1, except that the raw materials for preparing the semi-hot-melt flange in this embodiment include, by weight, 15 parts of HDPE, 15 parts of LLDPE, 1 part of reinforcing filler, 0.5 parts of silane coupling agent, 0.5 parts of lubricant and 1 part of light stabilizer, the HDPE having a melt index of 7-8 g / 10 min, purchased from Shanghai Hongwei Plastics Co., Ltd., with the item number: FHC7260, and the LLDPE having a melt index of 1.5-2.5 g / 10 min, purchased from Suzhou Yunmao New Materials Co., Ltd., with the item number: 1. The reinforcing filler is a mixture of talcum powder and quartz fiber, the weight ratio between the talcum powder and the quartz fiber is 1:3, the mesh number of the talcum powder is 1250 mesh, and the talcum powder is purchased from Changxing Longfeng Powder Material Co., Ltd., with the item number being 1250 mesh. The diameter of the quartz fiber is 5-10um, the length of the quartz fiber is 20-350um, and it is purchased from Lianyungang Rui Innovation Material Technology Co., Ltd. The silane coupling agent is KH-560, the lubricant is ethylene bis stearamide, and the CAS number of the ethylene bis stearamide is 110-30-5. The light stabilizer is UV770, the brand is: BASF Tinuvin770.
[0036] The second aspect of this embodiment provides a method for preparing the semi-hot-melt flange, which comprises mixing HDPE, LLDPE, reinforcing filler, silane coupling agent, lubricant and light stabilizer, and performing injection molding.
[0037] Example 3
[0038] The structure of the semi-hot-melt flange in this embodiment is the same as that of the semi-hot-melt flange in Example 1, except that the raw materials for preparing the semi-hot-melt flange in this embodiment include, by weight, 28 parts of HDPE, 22 parts of LLDPE, 4 parts of reinforcing fillers, 1 part of silane coupling agent, 0.75 parts of lubricant and 1 part of light stabilizer, the HDPE having a melt index of 7-8 g / 10 min, purchased from Shanghai Hongwei Plastics Co., Ltd., with the item number: FHC7260, and the LLDPE having a melt index of 1.5-2.5 g / 10 min, purchased from Suzhou Yunmao New Materials Co., Ltd., with the item number: 1. The reinforcing filler is a mixture of talcum powder and quartz fiber, the weight ratio between the talcum powder and the quartz fiber is 1:3, the mesh number of the talcum powder is 1250 mesh, and the talcum powder is purchased from Changxing Longfeng Powder Material Co., Ltd., with the item number being 1250 mesh. The diameter of the quartz fiber is 5-10um, the length of the quartz fiber is 20-350um, and it is purchased from Lianyungang Rui Innovation Material Technology Co., Ltd. The silane coupling agent is KH-560, the lubricant is ethylene bis stearamide, and the CAS number of the ethylene bis stearamide is 110-30-5. The light stabilizer is UV770, the brand is: BASF Tinuvin770.
[0039] The second aspect of this embodiment provides a method for preparing the semi-hot-melt flange, which comprises mixing HDPE, LLDPE, reinforcing filler, silane coupling agent, lubricant and light stabilizer, and performing injection molding.
[0040] Example 4
[0041] The structure of the semi-hot-melt flange in this embodiment is the same as that of the semi-hot-melt flange in Example 1, except that the raw materials for preparing the semi-hot-melt flange in this embodiment include, by weight, 40 parts of HDPE, 30 parts of LLDPE, 6 parts of reinforcing fillers, 1.5 parts of silane coupling agents, 1 part of lubricants and 2 parts of light stabilizers, the HDPE having a melt index of 7-8 g / 10 min, purchased from Shanghai Hongwei Plastics Co., Ltd., with the item number: FHC7260, and the LLDPE having a melt index of 1.5-2.5 g / 10 min, purchased from Suzhou Yunmao New Materials Co., Ltd., with the item number: 1. The reinforcing filler is a mixture of talcum powder and quartz fiber, the weight ratio between the talcum powder and the quartz fiber is 1:3, the mesh number of the talcum powder is 1250 mesh, and the talcum powder is purchased from Changxing Longfeng Powder Material Co., Ltd., with the item number being 1250 mesh. The diameter of the quartz fiber is 5-10um, the length of the quartz fiber is 20-350um, and it is purchased from Lianyungang Rui Innovation Material Technology Co., Ltd. The silane coupling agent is KH-560, the lubricant is ethylene bis stearamide, and the CAS number of the ethylene bis stearamide is 110-30-5. The light stabilizer is UV770, the brand is: BASF Tinuvin770.
[0042] The second aspect of this embodiment provides a method for preparing the semi-hot-melt flange, which comprises mixing HDPE, LLDPE, reinforcing filler, silane coupling agent, lubricant and light stabilizer, and performing injection molding.
[0043] Example 5
[0044] The structure of the semi-hot-melt flange in this embodiment is the same as that of the semi-hot-melt flange in Example 1, except that the raw materials for preparing the semi-hot-melt flange in this embodiment include 50 parts of LLDPE, 4 parts of reinforcing fillers, 1 part of silane coupling agent, 0.75 parts of lubricant and 1 part of light stabilizer by weight, and the LLDPE has a melt index of 1.5-2.5g / 10min and is purchased from Suzhou Yunmao New Materials Co., Ltd. with the item number: 1. The reinforcing filler is a mixture of talcum powder and quartz fiber, and the weight ratio between the talcum powder and the quartz fiber is 1:3. The mesh number of the talcum powder is 1250 mesh, and the talcum powder is purchased from Changxing Longfeng Powder Material Co., Ltd. with the item number 1250 mesh. The diameter of the quartz fiber is 5-10um, and the length of the quartz fiber is 20-350um, which is purchased from Lianyungang Rui Innovation Materials Technology Co., Ltd. The silane coupling agent is KH-560, the lubricant is ethylene bis stearamide, and the CAS number of the ethylene bis stearamide is 110-30-5. The light stabilizer is UV770, and the brand is BASF Tinuvin770.
[0045] The second aspect of this embodiment provides a method for preparing the semi-hot-melt flange, wherein the method for preparing the semi-hot-melt flange comprises mixing LLDPE, reinforcing filler, silane coupling agent, lubricant and light stabilizer, and performing injection molding.
[0046] Example 6
[0047] The structure of the semi-hot-melt flange in this embodiment is the same as that of the semi-hot-melt flange in Example 1, except that the raw materials for preparing the semi-hot-melt flange in this embodiment include 28 parts of HDPE, 22 parts of LLDPE, 4 parts of reinforcing fillers, 1 part of silane coupling agent, 0.75 parts of lubricant and 1 part of light stabilizer by weight, the HDPE having a melt index of 7-8 g / 10 min, purchased from Shanghai Hongwei Plastics Co., Ltd., with the item number: FHC7260, and the LLDPE having a melt index of 1.5-2.5 g / 10 min, purchased from Suzhou Yunmao New Materials Co., Ltd., with the item number: 1. The reinforcing filler is talcum powder, the mesh number of the talcum powder is 1250 mesh, and the talcum powder is purchased from Changxing Longfeng Powder Material Co., Ltd., with the item number being 1250 mesh. The silane coupling agent is KH-560, and the lubricant is ethylene bis stearamide, and the CAS number of the ethylene bis stearamide is 110-30-5. The light stabilizer is UV770, brand: BASF Tinuvin770.
[0048] The second aspect of this embodiment provides a method for preparing the semi-hot-melt flange, which comprises mixing HDPE, LLDPE, reinforcing filler, silane coupling agent, lubricant and light stabilizer, and performing injection molding.
[0049] Example 7
[0050] The structure of the semi-hot-melt flange in this embodiment is the same as that of the semi-hot-melt flange in Example 1, except that the raw materials for preparing the semi-hot-melt flange in this embodiment include, by weight, 28 parts of HDPE, 22 parts of LLDPE, 4 parts of reinforcing fillers, 1 part of silane coupling agent, 0.75 parts of lubricant and 1 part of light stabilizer, the HDPE having a melt index of 7-8 g / 10 min, purchased from Shanghai Hongwei Plastics Co., Ltd., with the item number: FHC7260, and the LLDPE having a melt index of 1.5-2.5 g / 10 min, purchased from Suzhou Yunmao New Materials Co., Ltd., with the item number: 1. The reinforcing filler is quartz fiber, the diameter of the quartz fiber is 5-10 um, the length of the quartz fiber is 20-350 um, purchased from Lianyungang Rui Innovation Materials Technology Co., Ltd. The silane coupling agent is KH-560, the lubricant is ethylene bis stearamide, and the CAS number of the ethylene bis stearamide is 110-30-5. The light stabilizer is UV770, brand: BASF Tinuvin770.
[0051] The second aspect of this embodiment provides a method for preparing the semi-hot-melt flange, which comprises mixing HDPE, LLDPE, reinforcing filler, silane coupling agent, lubricant and light stabilizer, and performing injection molding.
[0052] Performance Testing
[0053] Performance Test 1
[0054] With reference to the test method of GB / T 9341-2008, the samples to be tested were injection molded according to the raw material ratios in Example 3, Example 5-Example 7, and the flexural modulus of the samples was tested according to the test method of GB / T 9341-2008. The test results are shown in Table 1.
[0055] Performance Test 2
[0056] With reference to the test method of GB / T1040.3-2006, the samples to be tested were injection molded according to the raw material ratios in Example 3, Example 5-Example 7, and the tensile strength of the samples was tested according to the test method of GB / T1040.3-2006. The test results are shown in Table 1.
[0057] Table 1
[0058] Flexural modulus (MPa) Tensile strength(MPa) Example 3 811 26.4 Example 5 743 20.1 Example 6 754 21.5 Example 7 762 22.8
[0059] The above is only a preferred embodiment of the present invention and is not intended to limit the invention in other forms. Any technician familiar with the profession may use the technical content disclosed above to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A semi-hot-melt flange, characterized in that: It comprises an annular flange with a center hole, the annular flange is provided with N connecting holes, the outer side of the center hole of the annular flange is provided with X sealing gasket grooves, the outer side of the sealing gasket groove is provided with an annular protrusion, wherein N≥2, X≥1; a support portion, the support portion is extended to one side from the circumference of the center hole of the annular flange, the upper half of the support portion is provided with M support blocks, one end of the support block is in contact with the annular flange, wherein M≥1; The raw materials for preparing the semi-hot-melt flange include, by weight, at least 15-40 parts of HDPE, 15-30 parts of LLDPE, 1-6 parts of reinforcing filler, 0.5-1.5 parts of silane coupling agent, 0.5-1 parts of lubricant and 1-2 parts of light stabilizer; The melt index of the HDPE is 7-8 g / 10 min, and the melt index of the LLDPE is 1.5-2.5 g / 10 min; The reinforcing filler is a mixture of talcum powder and quartz fiber, the weight ratio of the talcum powder to the quartz fiber is 1:(3-5); the mesh size of the talcum powder is 1000-1500 mesh; the diameter of the quartz fiber is 5-10um, and the length of the quartz fiber is 20-350um; The lubricant is selected from at least one of calcium stearate, magnesium stearate, zinc stearate, butyl stearate, oleamide and ethylene bis stearamide.
2. The semi-hot-melt flange according to claim 1, characterized in that: The support portion may be provided with 4, 5, 6, 7, 8, 9 or 10 support blocks in the circumferential direction.
3. The semi-thermal fusion flange according to claim 1, characterized in that: The cross section of the support block is a Y-gon, where Y≥3.
4. The semi-hot-melt flange according to claim 3, characterized in that: The cross section of the support block may be a triangle, a quadrilateral, a pentagon, a hexagon, a heptagon, an octagon, a nonagon, or a decagon, and the quadrilateral may be a square, a rectangle, a parallelogram, or a trapezoid.
5. A method for preparing a semi-hot-melt flange according to any one of claims 1 to 4, characterized in that: The semi-hot-melt flange is formed by injection molding.
Citation Information
Patent Citations
Metal plastic composite tube with thermoplastic tube end contact flange
CN101514771A
Halogen-free flame retardant thermoplastic compositions
CN101945937A
PC-ASA alloy material with excellent low-temperature toughness and preparation method thereof
CN105153671A
HDPE flame-retardant communication sub-pipe
CN109687363A
Polyethylene composite material for injection molding and preparation method thereof
CN112759809A