A NdFeB permanent magnet material
By adding Se, fullerene and other elements to the NdFeB permanent magnet material and applying specific anticorrosion coatings, the problem of easy corrosion and high cost in humid environments is solved, and higher magnetic properties and corrosion resistance are achieved Performance, reduces production costs and simplifies the preparation process.
Patent Information
- Application Number
- CN202210421386.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-21
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-04-21
AI Technical Summary
The existing neodymium iron boron permanent magnet materials are prone to corrosion in humid environments, have high cost, and insufficient magnetic and corrosion resistance, which limits its further development.
A permanent magnet material body consisting of Nd, Fe, B, other rare earth elements, Se, fullerene and M, and a surface of N-(4-cyano-3-trifluoromethylphenyl is coated on it ) Anticorrosion coating composed of methacrylamide/3-(1,1-difluoroallyl)quinoxaline-2-ol/glycidyl methacrylate copolymer, the material is enhanced by formula design and preparation method Magnetic properties and corrosion resistance.
It significantly improves the comprehensive magnetic properties and corrosion resistance of neodymium iron boron permanent magnet materials, extends service life, reduces production costs, and is simple and easy to industrialize.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnetic materials, and in particular to a neodymium iron boron permanent magnet material. Background Art
[0002] NdFeB permanent magnet materials are known as the "King of Magnets" due to their extremely high magnetic energy product, coercive force and energy density. They are widely used in computer hardware drive devices, various household appliances, electroacoustic equipment, multimedia equipment, electronic instruments, meters, medical equipment, industrial motors, wind turbines, as well as automotive sensors, electric vehicles and hybrid electric vehicles drive motors, etc. Its output and usage have become one of the important indicators of a country's comprehensive national strength and national economic development level, and are closely related to people's lives.
[0003] Although NdFeB permanent magnet materials have excellent magnetic properties, traditional NdFeB permanent magnet materials have porous and multi-phase structures, and there is a large chemical potential difference between each phase. In a humid environment, corrosion cells are easily formed, resulting in intergranular corrosion. They contain a large amount of precious rare earth elements such as neodymium, which are expensive. In addition, the NdFeB permanent magnet materials on the market have more or less defects such as brittleness, low Curie temperature, poor temperature characteristics, and easy pulverization and corrosion. These defects restrict the further development of NdFeB permanent magnet materials.
[0004] In order to solve the above problems, patent CN105405555B discloses a cerium-holmium-containing sintered NdFeB permanent magnet material, which is composed of the following components: ((PrNd) 1-x-y Ce x Ho y ) a (FeCoCuAlN b ) 100-a-b B b , wherein a=30~33, b=0.95~1.05, x=0.05~0.30, y≤0.20. The preparation method of the material comprises the following steps: (1) batch smelting, (2) hydrogen crushing, (3) mixed powder making, (4) orientation molding, (5) sintering and tempering, wherein holmium is added in the form of hydrogen crushed holmium iron in the mixed powder making process. The invention solves the problem of high cost caused by the high price of praseodymium, neodymium and dysprosium by adding low-priced cerium and holmium to replace high-priced praseodymium, neodymium and dysprosium, thereby reducing the cost of sintered neodymium iron boron permanent magnet materials. However, the comprehensive magnetic properties and corrosion resistance of the material need to be further improved.
[0005] It can be seen that the field still needs a NdFeB permanent magnet material with good comprehensive magnetic properties and good corrosion resistance. Summary of the invention
[0006] The main purpose of the present invention is to solve the above technical problems and provide a NdFeB permanent magnet material with good comprehensive magnetic properties and good corrosion resistance and a preparation method thereof through formula design.
[0007] To achieve the above object, the present invention provides a NdFeB permanent magnet material, characterized in that it comprises a permanent magnet material body and an anti-corrosion coating with a thickness of 5-15 μm coated on the permanent magnet material body; the permanent magnet material body is composed of Nd, Fe, B, other rare earth elements, Se, fullerene and M; the M is a mixture of Ni, Co, Sb and Ca in a mass ratio of 1:(0.8-1.2):(0.2-0.4):(0.08-0.12); the mass ratio of Nd, Fe, B, other rare earth elements, Se, fullerene and M is (10-15):(65-7 5):(0.5-0.8):(3-6):(0.01-0.04):(0.1-0.3):(0.5-3); The anti-corrosion coating is composed of the following materials by weight: 35-55 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / methacrylate glycidyl ester copolymer, 4-6 parts of 2,4-diamino-6-phenyl-1,3,5-triazine, 1-3 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and 25-35 parts of solvent.
[0008] Preferably, the solvent is at least one of dimethyl sulfoxide, N,N-dimethylformamide and N-methylpyrrolidone.
[0009] Preferably, the preparation method of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer comprises the following steps: adding N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate, and an initiator to dimethyl sulfoxide, mixing evenly, stirring and reacting in an inert gas or nitrogen atmosphere at 50-65° C. for 3-5 hours, and then precipitating in water, washing the precipitated polymer with ethanol for 3-6 times, and then drying it in a vacuum drying oven at 85-95° C. to constant weight to obtain N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer.
[0010] Preferably, the mass ratio of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate, initiator and dimethyl sulfoxide is (3-5):(0.3-0.5):1:(0.03-0.06):(15-25).
[0011] Preferably, the initiator is azobisisobutyronitrile.
[0012] Preferably, the inert gas is any one of helium, neon and argon.
[0013] Preferably, the other rare earth elements are a mixture of Y, Ho and Dy in a mass ratio of 1:(0.8-1.2):(2-3).
[0014] Another object of the present invention is to provide a method for preparing the NdFeB permanent magnet material, characterized in that it comprises the following steps:
[0015] Step S1, after Nd, Fe, B, other rare earth elements, Se, and M are mixed according to the proportion, the mixture is placed in a quartz boat or a graphite boat, the quartz boat or the graphite boat is placed in a quartz tube, and nitrogen is introduced into the quartz tube; the quartz tube is placed in a synthesis furnace for smelting, and then the temperature is reduced, the mixture is taken out of the furnace, and a permanent magnet ingot is obtained after homogenization treatment; the obtained permanent magnet ingot is then powdered into a permanent magnet material powder with an average particle size of 3-8 μm by using a jet mill;
[0016] Step S2, uniformly dispersing fullerene in anhydrous ethanol, then adding the permanent magnetic material powder prepared in step S1 thereto, mixing evenly, vacuum drying at 85-95° C. to constant weight, and then putting into a molding press mold for orientation and shaping to form a blank;
[0017] Step S3, sintering the blanks made in step S2 in turn at high temperature, and after tempering, obtaining a permanent magnetic material body; then, stirring the components of the coating evenly, coating them on the permanent magnetic material body, and after solidification, obtaining a NdFeB permanent magnetic material.
[0018] Preferably, the temperature of the homogenization treatment in step S1 is 800-1000° C., and the treatment time is 1-3 hours.
[0019] Preferably, the orientation shaping in step S2 is specifically: orientation molding under a nitrogen protective atmosphere, in a magnetic field with a magnetic field strength of 1.5-2.5T and a pressure of 50-100MPa; and then cold isostatic pressing with an isostatic pressure of 210-310MPa for 3-6min.
[0020] Preferably, the high temperature sintering temperature in step S3 is 1050-1100° C., and the sintering time is 3-6 hours.
[0021] Preferably, the tempering treatment in step S3 includes primary tempering treatment and secondary tempering treatment, wherein the primary tempering treatment temperature is 880-920° C., and the insulation lasts for 2-3 hours, and the secondary tempering treatment temperature is 520-620° C., and the insulation lasts for 2-3 hours.
[0022] Preferably, in step S3, the curing temperature is 110-120° C., and the curing time is 2-4 hours.
[0023] Due to the application of the above technical solution, the present invention has the following beneficial effects:
[0024] (1) The NdFeB permanent magnet material disclosed in the present invention has a simple preparation method, does not require special equipment, requires little capital investment, has high preparation efficiency, and is easy to operate and industrialize.
[0025] (2) The NdFeB permanent magnet material disclosed in the present invention is composed of Nd, Fe, B, other rare earth elements, Se, fullerene and M; the M is a mixture of Ni, Co, Sb and Ca in a mass ratio of 1: (0.8-1.2): (0.2-0.4): (0.08-0.12); through the interaction of the components, the permanent magnet material has better comprehensive magnetic properties and corrosion resistance. The addition of fullerene can enhance the mechanical properties, corrosion resistance and comprehensive magnetic properties of the permanent magnet material. The addition of Se, Ni, Co, Sb and Ca can improve the grain boundary microstructure, inhibit the growth of each group of grains in the system, significantly improve the magnetic properties such as coercivity of the magnetic material, significantly increase the working temperature, and greatly improve the corrosion resistance and mechanical properties.
[0026] (3) The NdFeB permanent magnet material disclosed in the present invention, wherein the anti-corrosion coating is composed of the following materials in parts by weight: 35-55 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer, 4-6 parts of 2,4-diamino-6-phenyl-1,3,5-triazine, 1-3 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and 25-35 parts of solvent. The epoxy groups on the copolymer of N-(4-cyano-3-trifluoromethylphenyl) methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate undergo epoxy ring-opening reaction with the amino groups on 2,4-diamino-6-phenyl-1,3,5-triazine and 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and the generated hydroxyl groups can enhance the bonding performance between the anti-corrosion coating and the permanent magnetic material body; the molecular structure of the coating formed after the reaction forms an interpenetrating network structure, which effectively improves the corrosion resistance of the permanent magnetic material; 4-cyano-3-trifluoromethylphenyl, amide group, quinoxaline group, phenyl-1,3,5-triazine and fluorinated phenyl ether are simultaneously introduced into the molecular structure; under the multiple effects of electronic effect, steric effect and conjugation effect, the coating has good performance stability and good weather resistance, thereby making the permanent magnetic material have a long service life. DETAILED DESCRIPTION
[0027] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations. Example 1
[0028] A NdFeB permanent magnet material, comprising a permanent magnet material body and a 5 μm thick anti-corrosion coating coated on the permanent magnet material body; the permanent magnet material body is composed of Nd, Fe, B, other rare earth elements, Se, fullerene and M; the M is a mixture of Ni, Co, Sb and Ca in a mass ratio of 1:0.8:0.2:0.08; the mass ratio of Nd, Fe, B, other rare earth elements, Se, fullerene and M is 10:65:0.5:3:0.0 1:0.1:0.5; the anti-corrosion coating is composed of the following materials in parts by weight: 35 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer, 4 parts of 2,4-diamino-6-phenyl-1,3,5-triazine, 1 part of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and 25 parts of solvent; the solvent is dimethyl sulfoxide.
[0029] The preparation method of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer comprises the following steps: adding N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate and an initiator into dimethyl sulfoxide, mixing them evenly, stirring and reacting them at 50°C in a nitrogen atmosphere for 3 hours, and then precipitating them in water, washing the precipitated polymer with ethanol for 3 times, and then drying them in a vacuum drying oven at 85°C to constant weight to obtain the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer.
[0030] The mass ratio of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate, initiator, and dimethyl sulfoxide is 3:0.3:1:0.03:15; the initiator is azobisisobutyronitrile.
[0031] The other rare earth elements are a mixture of Y, Ho and Dy in a mass ratio of 1:0.8:2.
[0032] A method for preparing the NdFeB permanent magnet material comprises the following steps:
[0033] Step S1, after Nd, Fe, B, other rare earth elements, Se, and M are mixed according to the proportion, the mixture is placed in a quartz boat, the quartz boat is placed in a quartz tube, and nitrogen is introduced into the quartz tube; the quartz tube is placed in a synthesis furnace for smelting, and then the temperature is reduced, the mixture is taken out of the furnace, and a permanent magnet ingot is obtained after homogenization treatment; the obtained permanent magnet ingot is then powdered into a permanent magnet material powder with an average particle size of 3 μm by using a jet mill;
[0034] Step S2, uniformly dispersing fullerene in anhydrous ethanol, then adding the permanent magnetic material powder prepared in step S1 thereto, mixing evenly, vacuum drying at 85° C. to constant weight, and then placing into a molding press mold for orientation shaping to form a blank;
[0035] Step S3, sintering the blanks made in step S2 in turn at high temperature, and after tempering, obtaining a permanent magnetic material body; then, stirring the components of the coating evenly, coating them on the permanent magnetic material body, and after solidification, obtaining a NdFeB permanent magnetic material.
[0036] The temperature of the homogenization treatment in step S1 is 800° C. and the treatment time is 1 hour.
[0037] The orientation shaping in step S2 is specifically as follows: orientation shaping is performed in a nitrogen protective atmosphere in a magnetic field with a magnetic field strength of 1.5 T and a pressure of 50 MPa; and then cold isostatic pressing is performed with an isostatic pressure of 210 MPa for 3 minutes.
[0038] The high-temperature sintering temperature in step S3 is 1050°C, and the sintering time is 3 hours; the tempering treatment includes primary tempering treatment and secondary tempering treatment, wherein the primary tempering treatment temperature is 880°C, and the insulation lasts for 2 hours, and the secondary tempering treatment temperature is 520°C, and the insulation lasts for 2 hours; the curing temperature in step S3 is 110°C, and the curing time is 2 hours. Example 2
[0039] A NdFeB permanent magnet material, comprising a permanent magnet material body and a 7 μm thick anti-corrosion coating coated on the permanent magnet material body; the permanent magnet material body is composed of Nd, Fe, B, other rare earth elements, Se, fullerene and M; the M is a mixture of Ni, Co, Sb and Ca in a mass ratio of 1:0.9:0.25:0.09; the mass ratio of Nd, Fe, B, other rare earth elements, Se, fullerene and M is 11:67:0.6:4:0.02:0. 15:1; the anti-corrosion coating is composed of the following materials by weight: 40 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer, 4.5 parts of 2,4-diamino-6-phenyl-1,3,5-triazine, 1.5 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and 27 parts of solvent; the solvent is N,N-dimethylformamide.
[0040] The preparation method of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer comprises the following steps: adding N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate and an initiator into dimethyl sulfoxide, mixing them evenly, stirring and reacting them at 55°C in an inert gas atmosphere for 3.5 hours, and then precipitating them in water, washing the precipitated polymer with ethanol for 4 times, and then drying them in a vacuum drying oven at 87°C to constant weight to obtain the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer.
[0041] The mass ratio of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate, initiator, and dimethyl sulfoxide is 3.5:0.35:1:0.04:17; the initiator is azobisisobutyronitrile; and the inert gas is helium.
[0042] The other rare earth elements are a mixture of Y, Ho and Dy in a mass ratio of 1:0.9:2.2.
[0043] A method for preparing the NdFeB permanent magnet material comprises the following steps:
[0044] Step S1, after Nd, Fe, B, other rare earth elements, Se, and M are mixed according to the proportion, the mixture is placed in a graphite boat, the graphite boat is placed in a quartz tube, and nitrogen is introduced into the quartz tube; the quartz tube is placed in a synthesis furnace for smelting, and then the temperature is reduced, the mixture is taken out of the furnace, and a permanent magnet ingot is obtained after homogenization treatment; the obtained permanent magnet ingot is then powdered into a permanent magnet material powder with an average particle size of 4 μm by using a jet mill;
[0045] Step S2, dispersing fullerene uniformly in anhydrous ethanol, adding the permanent magnetic material powder prepared in step S1 thereto, mixing uniformly, vacuum drying at 87° C. to constant weight, and then placing the mixture into a molding press mold for orientation shaping to form a blank;
[0046] Step S3, sintering the blanks made in step S2 in turn at high temperature, and after tempering, obtaining a permanent magnetic material body; then, stirring the components of the coating evenly, coating them on the permanent magnetic material body, and after solidification, obtaining a NdFeB permanent magnetic material.
[0047] The temperature of the homogenization treatment in step S1 is 850° C. and the treatment time is 1.5 h.
[0048] The orientation shaping in step S2 is specifically as follows: orientation shaping is performed in a nitrogen protective atmosphere in a magnetic field with a magnetic field strength of 1.8 T and a pressure of 60 MPa; and then cold isostatic pressing is performed with an isostatic pressure of 230 MPa for 4 minutes.
[0049] The high-temperature sintering temperature in step S3 is 1060°C, and the sintering time is 4 hours; the tempering treatment in step S3 includes primary tempering treatment and secondary tempering treatment, wherein the primary tempering treatment temperature is 890°C, and the insulation duration is 2.3 hours, and the secondary tempering treatment temperature is 540°C, and the insulation duration is 2.3 hours; the curing temperature is 113°C, and the curing time is 2.5 hours. Example 3
[0050] A NdFeB permanent magnet material, comprising a permanent magnet material body and a 10 μm thick anti-corrosion coating coated on the permanent magnet material body; the permanent magnet material body is composed of Nd, Fe, B, other rare earth elements, Se, fullerene and M; the M is a mixture of Ni, Co, Sb and Ca in a mass ratio of 1:1:0.3:0.1; the mass ratio of Nd, Fe, B, other rare earth elements, Se, fullerene and M is 13:70:0.65:4.5:0.025 :0.2:1.5; the anti-corrosion coating is composed of the following materials in parts by weight: 45 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer, 5 parts of 2,4-diamino-6-phenyl-1,3,5-triazine, 2 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and 30 parts of solvent; the solvent is N-methylpyrrolidone.
[0051] The preparation method of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer comprises the following steps: adding N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate and an initiator into dimethyl sulfoxide, mixing them evenly, stirring and reacting them at 59° C. in an inert gas atmosphere for 4 hours, and then precipitating them in water, washing the precipitated polymer with ethanol for 5 times, and then drying them in a vacuum drying oven at 90° C. to constant weight to obtain the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer.
[0052] The mass ratio of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate, initiator, and dimethyl sulfoxide is 4:0.4:1:0.045:20; the initiator is azobisisobutyronitrile; and the inert gas is neon.
[0053] The other rare earth elements are a mixture of Y, Ho and Dy in a mass ratio of 1:1:2.5.
[0054] The method for preparing the NdFeB permanent magnet material comprises the following steps:
[0055] Step S1, after Nd, Fe, B, other rare earth elements, Se, and M are mixed according to the proportion, the mixture is placed in a quartz boat, the quartz boat is placed in a quartz tube, and nitrogen is introduced into the quartz tube; the quartz tube is placed in a synthesis furnace for smelting, and then the temperature is reduced, the mixture is taken out of the furnace, and a permanent magnet ingot is obtained after homogenization treatment; the obtained permanent magnet ingot is then powdered into a permanent magnet material powder with an average particle size of 6 μm by using a jet mill;
[0056] Step S2, uniformly dispersing fullerene in anhydrous ethanol, then adding the permanent magnetic material powder prepared in step S1 thereto, mixing evenly, vacuum drying at 90° C. to constant weight, and then placing into a molding press mold for orientation shaping to form a blank;
[0057] Step S3, sintering the blanks made in step S2 in turn at high temperature, and after tempering, obtaining a permanent magnetic material body; then, stirring the components of the coating evenly, coating them on the permanent magnetic material body, and after solidification, obtaining a NdFeB permanent magnetic material.
[0058] The temperature of the homogenization treatment in step S1 is 900° C. and the treatment time is 2 h.
[0059] The orientation shaping in step S2 is specifically as follows: orientation shaping is performed in a nitrogen protective atmosphere in a magnetic field with a magnetic field strength of 2T and a pressure of 75MPa; and then cold isostatic pressing is performed with an isostatic pressure of 270MPa for 4.5min.
[0060] The high temperature sintering temperature in step S3 is 1080°C, and the sintering time is 4.5 hours; the tempering treatment includes primary tempering treatment and secondary tempering treatment, wherein the primary tempering treatment temperature is 900°C, and the insulation duration is 2.5 hours, and the secondary tempering treatment temperature is 570°C, and the insulation duration is 2.5 hours.
[0061] The curing temperature in step S3 is 115° C. and the curing time is 3 hours. Example 4
[0062] A NdFeB permanent magnet material, comprising a permanent magnet material body and a 13 μm thick anti-corrosion coating coated on the permanent magnet material body; the permanent magnet material body is composed of Nd, Fe, B, other rare earth elements, Se, fullerene and M; the M is a mixture of Ni, Co, Sb and Ca in a mass ratio of 1:1.1:0.35:0.11; the mass ratio of Nd, Fe, B, other rare earth elements, Se, fullerene and M is 14:73:0.75:5.5:0.035:0.25:2.5; the anti-corrosion coating is The invention is composed of the following materials in parts by weight: 53 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer, 5.5 parts of 2,4-diamino-6-phenyl-1,3,5-triazine, 2.5 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and 33 parts of solvent; the solvent is a mixture of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone in a mass ratio of 1:2:1.
[0063] The preparation method of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer comprises the following steps: adding N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate and an initiator into dimethyl sulfoxide, mixing them evenly, stirring and reacting them at 63°C in an inert gas atmosphere for 4.5 hours, and then precipitating them in water, washing the precipitated polymer with ethanol for 6 times, and then drying them in a vacuum drying oven at 93°C to constant weight to obtain the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer.
[0064] The mass ratio of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate, initiator, and dimethyl sulfoxide is 4.5:0.45:1:0.055:23; the initiator is azobisisobutyronitrile; and the inert gas is argon.
[0065] The other rare earth elements are a mixture of Y, Ho and Dy in a mass ratio of 1:1.1:2.8.
[0066] A method for preparing the NdFeB permanent magnet material comprises the following steps:
[0067] Step S1, after Nd, Fe, B, other rare earth elements, Se, and M are mixed according to the proportion, the mixture is placed in a quartz boat or a graphite boat, the quartz boat or the graphite boat is placed in a quartz tube, and nitrogen is introduced into the quartz tube; the quartz tube is placed in a synthesis furnace for smelting, and then the temperature is reduced, the mixture is taken out of the furnace, and a permanent magnet ingot is obtained after homogenization treatment; the obtained permanent magnet ingot is then powdered into a permanent magnet material powder with an average particle size of 7 μm by using a jet mill;
[0068] Step S2, dispersing fullerene uniformly in anhydrous ethanol, adding the permanent magnetic material powder prepared in step S1 thereto, mixing uniformly, vacuum drying at 93° C. to constant weight, and then placing the mixture into a molding press mold for orientation shaping to form a blank;
[0069] Step S3, sintering the blanks made in step S2 in turn at high temperature, and after tempering, obtaining a permanent magnetic material body; then, stirring the components of the coating evenly, coating them on the permanent magnetic material body, and after solidification, obtaining a NdFeB permanent magnetic material.
[0070] The temperature of the homogenization treatment in step S1 is 950° C. and the treatment time is 2.5 h.
[0071] The orientation shaping in step S2 is specifically as follows: orientation shaping is performed in a nitrogen protective atmosphere in a magnetic field with a magnetic field strength of 2.3 T and a pressure of 90 MPa; and then cold isostatic pressing is performed with an isostatic pressure of 300 MPa for 5.5 minutes.
[0072] The high temperature sintering temperature in step S3 is 1090° C., and the sintering time is 5.5 hours.
[0073] The tempering treatment in step S3 includes primary tempering treatment and secondary tempering treatment, wherein the primary tempering treatment temperature is 910°C, and the insulation lasts for 2.8 hours, and the secondary tempering treatment temperature is 610°C, and the insulation lasts for 2.8 hours; the curing temperature is 118°C, and the curing time is 3.5 hours. Example 5
[0074] A NdFeB permanent magnet material comprises a permanent magnet material body and a 15 μm thick anti-corrosion coating coated on the permanent magnet material body; the permanent magnet material body is composed of Nd, Fe, B, other rare earth elements, Se, fullerene and M; the M is a mixture of Ni, Co, Sb and Ca in a mass ratio of 1:1.2:0.4:0.12; the mass ratio of Nd, Fe, B, other rare earth elements, Se, fullerene and M is 15:75:0.8:6:0.04: 0.3:3; the anti-corrosion coating is composed of the following materials by weight: 55 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer, 6 parts of 2,4-diamino-6-phenyl-1,3,5-triazine, 3 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and 35 parts of solvent; the solvent is N,N-dimethylformamide.
[0075] The preparation method of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer comprises the following steps: adding N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate and an initiator into dimethyl sulfoxide, mixing them evenly, stirring and reacting them at 65°C in a nitrogen atmosphere for 5 hours, and then precipitating them in water, washing the precipitated polymer with ethanol for 6 times, and then drying them in a vacuum drying oven at 95°C to constant weight to obtain the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer.
[0076] The mass ratio of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate, initiator, and dimethyl sulfoxide is 5:0.5:1:0.06:25; the initiator is azobisisobutyronitrile.
[0077] The other rare earth elements are a mixture of Y, Ho and Dy in a mass ratio of 1:1.2:3.
[0078] A method for preparing the NdFeB permanent magnet material comprises the following steps:
[0079] Step S1, after Nd, Fe, B, other rare earth elements, Se, and M are mixed according to the proportion, the mixture is placed in a quartz boat or a graphite boat, the quartz boat or the graphite boat is placed in a quartz tube, and nitrogen is introduced into the quartz tube; the quartz tube is placed in a synthesis furnace for smelting, and then the temperature is reduced, the mixture is taken out of the furnace, and a permanent magnet ingot is obtained after homogenization treatment; and the obtained permanent magnet ingot is then powdered into a permanent magnet material powder with an average particle size of 8 μm by using a jet mill;
[0080] Step S2, uniformly dispersing fullerene in anhydrous ethanol, then adding the permanent magnetic material powder prepared in step S1 thereto, mixing evenly, vacuum drying at 95° C. to constant weight, and then putting into a molding press mold for orientation and shaping to form a blank;
[0081] Step S3, sintering the blanks made in step S2 in turn at high temperature, and after tempering, obtaining a permanent magnetic material body; then, stirring the components of the coating evenly, coating them on the permanent magnetic material body, and after solidification, obtaining a NdFeB permanent magnetic material.
[0082] The temperature of the homogenization treatment in step S1 is 1000° C. and the treatment time is 3 hours.
[0083] The orientation shaping in step S2 is specifically as follows: orientation shaping is performed under a nitrogen protective atmosphere in a magnetic field with a magnetic field strength of 2.5 T and a pressure of 100 MPa; and then cold isostatic pressing is performed with an isostatic pressure of 310 MPa for 6 minutes.
[0084] The high temperature sintering temperature in step S3 is 1100°C, and the sintering time is 6 hours; the tempering treatment in step S3 includes primary tempering treatment and secondary tempering treatment, wherein the primary tempering treatment temperature is 920°C, and the insulation lasts for 3 hours, and the secondary tempering treatment temperature is 620°C, and the insulation lasts for 3 hours.
[0085] The curing temperature in step S3 is 120° C. and the curing time is 4 hours.
[0086] Comparative Example 1
[0087] The present invention provides a NdFeB permanent magnet material, the formula and preparation method of which are similar to those of Example 1, except that Se and Sb are not added.
[0088] Comparative Example 2
[0089] The present invention provides a NdFeB permanent magnet material, the formula and preparation method of which are similar to those of Example 1, except that fullerene and Y are not added.
[0090] Comparative Example 3
[0091] The present invention provides a NdFeB permanent magnet material, the formula and preparation method of which are similar to those of Example 1, except that no Ca and Co are added.
[0092] Among them, the performance test results of the NdFeB permanent magnet materials of Examples 1-5 and Comparative Examples 1-3 are shown in Table 1; Test method: Test according to GB / T3217 permanent magnet (hard magnet) material magnetic test method. The NdFeB permanent magnet material was subjected to a neutral salt spray test, using a 5wt% sodium chloride aqueous solution to spray the test material with a salt spray test at a test temperature of 30°C, and the rust condition was observed after 200h.
[0093] Table 1 NdFeB permanent magnet material performance test results
[0094]
[0095] As can be seen from Table 1, the NdFeB permanent magnet material disclosed in the embodiment of the present invention has excellent comprehensive magnetic properties and corrosion resistance, which is the result of the synergistic effect of various components.
[0096] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.
Claims
1. A neodymium iron boron permanent magnet material, characterized in that: It comprises a permanent magnetic material body and an anti-corrosion coating with a thickness of 5-15 μm coated on the permanent magnetic material body; the permanent magnetic material body is composed of Nd, Fe, B, other rare earth elements, Se, fullerene and M; the M is a mixture of Ni, Co, Sb and Ca in a mass ratio of 1:(0.8-1.2):(0.2-0.4):(0.08-0.12); the mass ratio of Nd, Fe, B, other rare earth elements, Se, fullerene and M is (10-15):(65-75):(0.5-0.8):(3-6):(0.01-0.04):(0.1-0.3):(0.5-3); the anti-corrosion coating is composed of the following materials in parts by weight: 35-55 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer, 4-6 parts of 2,4-diamino-6-phenyl-1,3,5-triazine, 1-3 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and 25-35 parts of solvent; the other rare earth elements are a mixture of Y, Ho, and Dy in a mass ratio of 1:(0.8-1.2):(2-3); The preparation method of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer comprises the following steps: adding N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate and an initiator into dimethyl sulfoxide, mixing them evenly, stirring and reacting them at 50-65° C. for 3-5 hours in an inert gas or nitrogen atmosphere, precipitating them in water, and washing the precipitated polymer with ethanol. 3-6 times, and then placed in a vacuum drying oven at 85-95° C. to dry to constant weight to obtain N-(4-cyano-3-trifluoromethylphenyl)methacrylamide / 3-(1,1-difluoroallyl)quinoxaline-2-ol / glycidyl methacrylate copolymer; the mass ratio of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 3-(1,1-difluoroallyl)quinoxaline-2-ol, glycidyl methacrylate, initiator, and dimethyl sulfoxide is (3-5):(0.3-0.5):1:(0.03-0.06):(15-25).
2. The NdFeB permanent magnet material according to claim 1, characterized in that: The solvent is at least one of dimethyl sulfoxide, N,N-dimethylformamide and N-methylpyrrolidone.
3. The NdFeB permanent magnet material according to claim 1, characterized in that: The initiator is azobisisobutyronitrile; the inert gas is any one of helium, neon and argon.
4. A method for preparing the NdFeB permanent magnet material according to any one of claims 1 to 3, characterized in that: The steps include: Step S1, after Nd, Fe, B, other rare earth elements, Se, and M are mixed according to the proportion, the mixture is placed in a quartz boat or a graphite boat, the quartz boat or the graphite boat is placed in a quartz tube, and nitrogen is introduced into the quartz tube; the quartz tube is placed in a synthesis furnace for smelting, and then the temperature is reduced, the mixture is taken out of the furnace, and a permanent magnet ingot is obtained after homogenization treatment; the obtained permanent magnet ingot is then powdered into a permanent magnet material powder with an average particle size of 3-8 μm by using a jet mill; Step S2, uniformly dispersing fullerene in anhydrous ethanol, then adding the permanent magnetic material powder prepared in step S1 thereto, mixing evenly, vacuum drying at 85-95° C. to constant weight, and then putting into a molding press mold for orientation and shaping to form a blank; Step S3, sintering the blanks made in step S2 in turn at high temperature, and after tempering, obtaining a permanent magnetic material body; then, stirring the components of the coating evenly, coating them on the permanent magnetic material body, and after solidification, obtaining a NdFeB permanent magnetic material.
5. The method for preparing the NdFeB permanent magnet material according to claim 4, characterized in that: The temperature of the homogenization treatment in step S1 is 800-1000° C., and the treatment time is 1-3 hours.
6. The method for preparing the NdFeB permanent magnet material according to claim 4, characterized in that: The orientation shaping in step S2 is specifically as follows: orientation shaping in a nitrogen protective atmosphere, in a magnetic field with a magnetic field strength of 1.5-2.5T and a pressure of 50-100MPa; and then cold isostatic pressing with an isostatic pressure of 210-310MPa for 3-6min.
7. The method for preparing the NdFeB permanent magnet material according to claim 4, characterized in that: The high temperature sintering temperature in step S3 is 1050-1100°C, and the sintering time is 3-6 hours; the tempering treatment includes primary tempering treatment and secondary tempering treatment, wherein the primary tempering treatment temperature is 880-920°C, and the insulation lasts for 2-3 hours, and the secondary tempering treatment temperature is 520-620°C, and the insulation lasts for 2-3 hours; the curing temperature is 110-120°C, and the curing time is 2-4 hours.