A method for preparing homoepitaxial gallium oxide thin film on an unintentionally doped substrate and a molecular beam epitaxy device
By using a laser to evenly heat the stainless steel tray in the molecular beam epitaxy equipment, the problem of uneven heating of the gallium oxide substrate is solved, the quality and thickness uniformity of the gallium oxide film are improved, and it is suitable for the preparation of high-sensitivity sun-blind UV detectors.
Patent Information
- Application Number
- CN202210466536.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-04-29
AI Technical Summary
In the prior art, when molecular beam epitaxy equipment is used to prepare gallium oxide homoepitaxial films, the gallium oxide substrate is heated unevenly, which affects the quality and thickness uniformity of the film, and even causes the epitaxial layer to crack.
In the molecular beam epitaxy equipment, the laser is used to uniformly heat the stainless steel tray, and the laser spot covers the top of the tray to achieve uniform heating of the gallium oxide substrate. The laser output power and the beam intensity and oxygen flow rate of the Ga metal evaporation source are adjusted to control film growth. temperature and speed.
The high quality and thickness uniformity of the gallium oxide film are achieved, which is suitable for preparing high-sensitivity sun-blind ultraviolet detectors.
Smart Images

Figure CN114823287B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of gallium oxide film preparation, and in particular to a method for preparing a homoepitaxial gallium oxide film on an unintentionally doped substrate and a molecular beam epitaxy device. Background Art
[0002] Gallium oxide (Ga2O3) is an emerging third-generation wide bandgap semiconductor with the advantages of ultra-wide bandgap and high breakdown field strength. It is a transparent oxide semiconductor material. Due to its excellent physical and chemical properties, good conductivity and luminescence performance, it has broad application prospects in the fields of power semiconductor devices, ultraviolet detectors, gas sensors and optoelectronic devices. Gallium oxide has five crystal structures, namely rhombohedral (α), monoclinic (β), defective spinel (γ), cubic (δ) and orthorhombic (ε). β-Ga2O3 has gradually become a research hotspot at home and abroad in recent years due to its stability at high temperatures. Unless otherwise specified, the gallium oxide mentioned below refers to β-Ga2O3.
[0003] Among the epitaxy methods of gallium oxide, molecular beam epitaxy (MBE) is one of the main means to grow high-purity, high-quality gallium oxide epitaxial films. The use of ultra-high vacuum and high-purity source materials can effectively reduce the concentration of unintentionally doped impurities and achieve precise control of growth at the atomic scale. Gallium oxide films epitaxially grown by MBE have the advantages of good crystal quality, flat surface, and controllable electron concentration, which are necessary conditions for obtaining high-performance gallium oxide-based power electronic devices and photoelectric conversion devices. Therefore, MBE equipment can be used to prepare high-quality gallium oxide unintentionally doped homoepitaxial wafers on unintentionally doped substrates; differential finger electrodes (MSM) are arranged on gallium oxide unintentionally doped homoepitaxial wafers, which can be used to prepare high-performance solar-blind ultraviolet detectors to meet the urgent needs for high-sensitivity solar-blind ultraviolet detectors in extreme occasions.
[0004] In view of the characteristics of existing MBE technology, in the process of using MBE equipment to prepare homoepitaxial gallium oxide thin films, it is necessary to maintain the gallium oxide substrate at a high temperature suitable for the growth of gallium oxide thin films. In the prior art, the gallium oxide substrate is heated by heating wires arranged behind the substrate to heat the gallium oxide substrate by thermal radiation. Since the arrangement of the heating wires always has a certain spatial distribution, the heating of the substrate is uneven, which seriously affects the quality and thickness uniformity of the prepared epitaxial wafer, and even causes cracking of the epitaxial layer.
[0005] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0006] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a method for preparing a homoepitaxial gallium oxide thin film on an unintentionally doped substrate and a molecular beam epitaxy device, aiming to solve the problem of poor quality and thickness uniformity of gallium oxide epitaxial wafers prepared by the prior art.
[0007] The technical solution of the present invention is as follows:
[0008] A molecular beam epitaxy device for preparing a homoepitaxial gallium oxide film on an unintentionally doped substrate comprises an MBE growth chamber, a stainless steel tray arranged in the MBE growth chamber, and an unintentionally doped gallium oxide substrate fixedly arranged at the bottom of the stainless steel tray, wherein a laser is arranged above the stainless steel tray, and a laser spot emitted by the laser covers the entire top of the stainless steel tray.
[0009] The molecular beam epitaxy equipment, wherein a beam expander is provided on the laser.
[0010] The molecular beam epitaxy equipment, wherein the laser wavelength emitted by the laser is 500-1500nm.
[0011] A method for preparing a homoepitaxial gallium oxide thin film on an unintentionally doped substrate based on a molecular beam epitaxy device, comprising the steps of:
[0012] Start the molecular pump in advance to evacuate the MBE growth chamber;
[0013] Fixing the unintentionally doped gallium oxide substrate on the bottom end of the stainless steel tray, with the growth surface of the unintentionally doped gallium oxide substrate facing downward;
[0014] Stop the molecular pump, fill the rapid injection chamber with nitrogen to break the vacuum, and then place the stainless steel tray fixed with the unintentionally doped gallium oxide substrate into the rapid injection chamber;
[0015] Setting the evaporation temperature of the Ga metal evaporation source, and when the Ga metal evaporation source reaches the preset evaporation temperature, controlling the velocity flow intensity of the Ga metal evaporation source;
[0016] Start the molecular pump to evacuate the fast injection chamber. When the vacuum degree of the fast injection chamber is lower than 10 - 8 mbar, introducing the stainless steel tray with the non-intentionally doped gallium oxide substrate fixed thereon into the MBE growth chamber, and turning on the laser to heat the stainless steel tray;
[0017] Slowly open the angle valve of the oxygen plasma source pipeline and set the oxygen flow rate to 0.1-0.5sccm on the digital flow meter;
[0018] After the laser heats the stainless steel tray to a preset film growth temperature, the oxygen source is turned on to ignite the oxygen plasma, and the oxygen pressure is waited to be stable, and the baffle control of the Ga metal evaporation source is set to an automatic mode to perform homoepitaxial gallium oxide film growth;
[0019] When the growth thickness of the homoepitaxial gallium oxide film reaches 50-500 nanometers, the growth is completed, and the baffle of the Ga metal evaporation source is automatically closed to maintain the oxygen source supply; when the temperature of the stainless steel tray is lower than 200°C, the oxygen source is cut off, the laser is turned off, and the preparation of the homoepitaxial gallium oxide film is completed.
[0020] The method for preparing a homoepitaxial gallium oxide film on an unintentionally doped substrate comprises the following steps: in the step of starting a molecular pump in advance to evacuate an MBE growth chamber, the MBE growth chamber is evacuated to a vacuum level of less than 2×10 -9 mbar.
[0021] The method for preparing a homoepitaxial gallium oxide film on an unintentionally doped substrate comprises the following steps: the Ga metal evaporation source has a pre-set evaporation temperature of 1000-1200° C. and a heating rate of 2-10° C. / min.
[0022] The method for preparing a homoepitaxial gallium oxide film on an unintentionally doped substrate, wherein the velocity flux intensity of the Ga metal evaporation source is 1×10 -8 -9×10 -7 mbar.
[0023] The method for preparing a homoepitaxial gallium oxide film on an unintentionally doped substrate comprises the following steps: the laser heats the stainless steel tray to a preset film growth temperature, the preset film growth temperature is 600-1000° C., and the heating rate is 5-15° C. / min.
[0024] The method for preparing a homoepitaxial gallium oxide film on an unintentionally doped substrate, wherein the growth rate of the homoepitaxial gallium oxide film is 10-100 nanometers / hour.
[0025] The method for preparing a homoepitaxial gallium oxide film on an unintentionally doped substrate comprises the following steps: after the homoepitaxial gallium oxide film is prepared, the prepared homoepitaxial gallium oxide film is transferred from an MBE growth chamber to a fast sampling chamber, and atmospheric pressure sampling is performed after breaking the vacuum.
[0026] Beneficial effects: The present invention provides a method for preparing a homoepitaxial gallium oxide thin film on an unintentionally doped substrate and a molecular beam epitaxy device, wherein a laser is arranged above the stainless steel tray, and the laser spot emitted by the laser covers the entire top of the stainless steel tray. The present invention uses the laser to uniformly heat the stainless steel tray in the MBE growth chamber by laser heating, thereby achieving uniform heating of the unintentionally doped gallium oxide substrate, and preparing high-quality, uniformly thick unintentionally doped gallium oxide homoepitaxial wafers. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The present invention is a schematic structural diagram of a molecular beam epitaxy device for preparing a homoepitaxial gallium oxide film on an unintentionally doped substrate.
[0028] Figure 2 Figure 2 is a graph showing the transmittance of unintentionally doped and Ta-doped gallium oxide substrates.
[0029] Figure 3 The transmittance curves of unintentionally doped and Fe-doped gallium oxide substrates.
[0030] Figure 4 The present invention is a flow chart of a method for preparing a homoepitaxial gallium oxide thin film on an unintentionally doped substrate. DETAILED DESCRIPTION
[0031] The present invention provides a method for preparing a homoepitaxial gallium oxide thin film on an unintentionally doped substrate and a molecular beam epitaxy device. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0032] In the process of preparing gallium oxide homoepitaxial thin films using molecular beam epitaxy equipment, the gallium oxide substrate needs to be maintained at a high temperature suitable for the growth of gallium oxide thin films. However, the heating methods of gallium oxide substrates in existing molecular beam epitaxy equipment will cause uneven heating of the substrate, which will seriously affect the quality and thickness uniformity of the epitaxial wafer, and even cause the epitaxial wafer to crack.
[0033] Based on this, the present invention provides a molecular beam epitaxy device for preparing homoepitaxial gallium oxide thin films on unintentionally doped substrates, such as Figure 1 As shown, it includes an MBE growth chamber 10, a stainless steel tray 20 arranged in the MBE growth chamber 10, and an unintentionally doped gallium oxide substrate 30 fixedly arranged at the bottom of the stainless steel tray 20, wherein a laser 40 is arranged above the stainless steel tray 20, and the laser spot emitted by the laser 40 covers the entire top of the stainless steel tray 20.
[0034] Specifically, according to literature reports, since unintentionally doped gallium oxide substrates are very susceptible to contamination by n-type impurity ions during the single crystal growth process, their transmittance in the infrared band has two situations: (1) If the n-type impurity ion contamination in the growth environment is low, the substrate transmittance in the infrared band is very high, see Figure 2 (Data from SCI paper: Tuning Electrical Conductivity of β-Ga2O3 Single Crystals by Ta Doping); (2) If the growth environment is heavily contaminated by n-type impurity ions, the substrate's transmittance in the infrared band will drop rapidly. Figure 3 (Data from SCI paper: Growth and physical characterization of high resistivity Fe:β-Ga2O3 crystals). In other words, since the absorption of infrared laser by unintentionally doped gallium oxide substrate is uncontrollable, when using common infrared laser to heat the unintentionally doped gallium oxide substrate, the laser cannot be directly irradiated on the unintentionally doped gallium oxide substrate, but must be irradiated evenly on the stainless steel tray. The stainless steel tray evenly heated by the laser then transfers the heat to the unintentionally doped gallium oxide substrate, thus achieving uniform heating of the unintentionally doped gallium oxide substrate in the MBE growth chamber.
[0035] The molecular beam epitaxy equipment for preparing homoepitaxial gallium oxide thin films on unintentionally doped substrates provided in this embodiment, since the laser spot emitted by the laser 40 covers the entire top of the stainless steel tray 20, the stainless steel tray in the MBE growth chamber can be uniformly heated by laser heating, thereby achieving uniform heating of the unintentionally doped gallium oxide substrate, and preparing high-quality, uniformly thick gallium oxide unintentionally doped gallium oxide homoepitaxial wafers for preparing high-sensitivity solar-blind ultraviolet detectors.
[0036] In some embodiments, two or more lasers may be disposed above the stainless steel tray. Figure 1 As shown, two lasers can be arranged below the stainless steel tray, or three, four, five, six, etc. lasers can be arranged; it is necessary to ensure that the multiple lasers can evenly cover the top of the stainless steel tray so that the stainless steel tray is evenly heated.
[0037] In some embodiments, a beam expander is provided on the laser. In this embodiment, by providing a beam expander on the laser, the laser spot size of the laser can be adjusted so that the laser spot of the laser can cover the entire top of the stainless steel tray.
[0038] In some embodiments, the laser emits a laser with a wavelength of 500-1500 nm. Preferably, the laser emits a laser with a wavelength of 800-1200 nm. For example, the laser emits a laser with a wavelength of 800 nm, 900 nm, 1000 nm, 1000 nm, 1200 nm, etc.
[0039] The molecular beam epitaxy equipment, wherein a beam expander is provided on the laser.
[0040] The molecular beam epitaxy equipment, wherein the laser wavelength emitted by the laser is 500-1500nm.
[0041] In some embodiments, a method for preparing a homoepitaxial gallium oxide thin film on an unintentionally doped substrate based on a molecular beam epitaxy device is also provided. Figure 4 As shown, it includes the steps of:
[0042] S10, starting the molecular pump in advance to evacuate the MBE growth chamber;
[0043] S20, fixing the unintentionally doped gallium oxide substrate on the bottom end of the stainless steel tray, with the growth surface of the unintentionally doped gallium oxide substrate facing downward;
[0044] S30, stopping the molecular pump, filling the rapid injection chamber with nitrogen to break the vacuum, and placing the stainless steel tray fixed with the unintentionally doped gallium oxide substrate into the rapid injection chamber;
[0045] S40, setting the evaporation temperature of the Ga metal evaporation source, and when the Ga metal evaporation source reaches the preset evaporation temperature, controlling the velocity flow intensity of the Ga metal evaporation source;
[0046] S50, start the molecular pump to evacuate the fast injection chamber. When the vacuum degree of the fast injection chamber is lower than 10 -8 mbar, introducing the stainless steel tray with the unintentionally doped gallium oxide substrate fixed thereon into the MBE growth chamber, and turning on the laser to heat the stainless steel tray;
[0047] S60, slowly open the angle valve of the oxygen plasma source pipeline, and set the oxygen flow rate to 0.1-0.5 sccm on the digital flow meter;
[0048] S70, when the laser heats the stainless steel tray to a preset film growth temperature, the oxygen source is turned on to ignite the oxygen plasma, the oxygen pressure is waited to be stable, the baffle control of the Ga metal evaporation source is set to an automatic mode, and homoepitaxial gallium oxide film growth is performed;
[0049] S80. When the growth thickness of the homoepitaxial gallium oxide film reaches 50-500 nanometers, the growth is completed, and the baffle of the Ga metal evaporation source is automatically closed to maintain the oxygen source supply; when the temperature of the stainless steel tray is lower than 200°C, the oxygen source is cut off, the laser is turned off, and the preparation of the homoepitaxial gallium oxide film is completed.
[0050] In this embodiment, the heating temperature of the stainless steel tray can be adjusted by controlling the power of the laser, thereby adjusting the heating temperature of the unintentionally doped gallium oxide substrate; the growth rate of the homoepitaxial gallium oxide film can be controlled by adjusting the beam intensity of the Ga metal evaporation source and the flow rate of oxygen. In the process of preparing the homoepitaxial gallium oxide film on the unintentionally doped substrate, the stainless steel tray is uniformly heated under the irradiation of the laser, thereby achieving uniform heating of the unintentionally doped gallium oxide substrate. At the same time, the temperature of the unintentionally doped gallium oxide substrate is measured in real time by a temperature sensor and fed back to the laser, thereby adjusting the laser output power so that the temperature of the unintentionally doped gallium oxide substrate is maintained in a temperature range suitable for the epitaxial growth of gallium oxide.
[0051] In some embodiments, in the step of pre-starting the molecular pump to evacuate the MBE growth chamber, the MBE growth chamber is evacuated to a vacuum level of less than 2×10 -9 mbar.
[0052] In some embodiments, the Ga metal evaporation source has a pre-set evaporation temperature of 1000-1200° C. and a heating rate of 2-10° C. / min.
[0053] In some embodiments, the Ga metal evaporation source has a flow rate of 1×10 -8 -9×10 -7 mbar, but not limited thereto.
[0054] In some embodiments, in the step where the laser heats the stainless steel tray to a preset film growth temperature, the preset film growth temperature is 600-1000° C., and the heating rate is 5-15° C. / min.
[0055] In some embodiments, the growth rate of the homoepitaxial gallium oxide thin film is 10-100 nm / hour.
[0056] In some embodiments, after the homoepitaxial gallium oxide film is prepared, the prepared homoepitaxial gallium oxide film is transferred from the MBE growth chamber to the fast sampling chamber, and the vacuum is broken and then the atmospheric pressure sampling is performed.
[0057] The present invention is further explained below by specific embodiments:
[0058] Example 1
[0059] A method for preparing a homoepitaxial gallium oxide film on an unintentionally doped substrate based on a molecular beam epitaxy device, the molecular beam epitaxy device comprising an MBE growth chamber, a stainless steel tray arranged in the MBE growth chamber, and an unintentionally doped gallium oxide substrate arranged on the stainless steel tray, wherein the growth surface of the unintentionally doped gallium oxide substrate faces downward, and a laser is arranged below the stainless steel tray, and the laser spot emitted by the laser covers the entire top of the stainless steel tray; the method comprises the steps of:
[0060] Confirm that the water, electricity and gas supply of the MBE equipment is normal, and start the molecular pump to evacuate the MBE growth chamber until the vacuum degree is less than 2×10 -9 mbar;
[0061] Fixing a cleaned 2-inch unintentionally doped gallium oxide substrate on the bottom of a stainless steel tray, with the growth surface of the unintentionally doped gallium oxide substrate facing downward;
[0062] Stop the molecular pump, fill the rapid injection chamber with nitrogen to break the vacuum, and then place the stainless steel tray fixed with the unintentionally doped gallium oxide substrate into the rapid injection chamber;
[0063] The evaporation temperature of the Ga metal evaporation source was set to 1100°C, and the heating and cooling rates were 6°C / min. When the Ga metal evaporation source reached the preset evaporation temperature of 1100°C, the beam current intensity was measured using a beam current gauge. The temperature of the evaporation source was adjusted according to the stabilized beam current gauge reading to maintain the beam current intensity at 5×10 -7 mbar, until the most suitable evaporation temperature is found;
[0064] Start the molecular pump to evacuate the fast injection chamber. When the vacuum degree of the fast injection chamber is lower than 10 - 8 mbar, the stainless steel tray with the non-intentionally doped gallium oxide substrate fixed thereon is introduced into the MBE growth chamber, the laser is turned on to heat the stainless steel tray to 800°C, the heating rate is set to 10°C / min, and at the same time, the substrate temperature is measured in real time by a temperature sensor and fed back to the laser, and then the laser output power is adjusted to maintain the substrate temperature in a temperature range suitable for epitaxial growth;
[0065] Slowly open the angle valve of the oxygen plasma source pipeline and set the oxygen flow rate to 0.3 sccm on the digital flow meter;
[0066] After the laser heats the stainless steel tray to a preset film growth temperature of 800° C., the oxygen source is turned on to ignite the oxygen plasma, and the oxygen pressure is waited to be stable. The baffle control of the Ga metal evaporation source is set to an automatic mode, and the growth rate is set to 50 nanometers / hour to perform homoepitaxial gallium oxide film growth;
[0067] When the thickness of the homoepitaxial gallium oxide film reaches 200 nanometers, the growth is completed, and the baffle of the Ga metal evaporation source is automatically closed to maintain the oxygen source supply; when the temperature of the stainless steel tray is lower than 200°C, the oxygen source is cut off and the laser is turned off;
[0068] The prepared sample is transferred to the fast sampling chamber, and sampling is performed at normal pressure after breaking the vacuum, thereby completing the preparation of homoepitaxial high-quality unintentionally doped gallium oxide film on the unintentionally doped gallium oxide substrate.
[0069] Example 2
[0070] A method for preparing a homoepitaxial gallium oxide film on an unintentionally doped substrate based on a molecular beam epitaxy device, the molecular beam epitaxy device comprising an MBE growth chamber, a stainless steel tray arranged in the MBE growth chamber, and an unintentionally doped gallium oxide substrate arranged on the stainless steel tray, wherein the growth surface of the unintentionally doped gallium oxide substrate faces downward, and a laser is arranged below the stainless steel tray, and the laser spot emitted by the laser covers the entire top of the stainless steel tray; the method comprises the steps of:
[0071] Confirm that the water, electricity and gas supply of the MBE equipment is normal, and start the molecular pump to evacuate the MBE growth chamber until the vacuum degree is less than 2×10 -9 mbar;
[0072] Fixing a cleaned 2-inch unintentionally doped gallium oxide substrate on the bottom of a stainless steel tray, with the growth surface of the unintentionally doped gallium oxide substrate facing downward;
[0073] Stop the molecular pump, fill the rapid injection chamber with nitrogen to break the vacuum, and then place the stainless steel tray fixed with the unintentionally doped gallium oxide substrate into the rapid injection chamber;
[0074] The evaporation temperature of the Ga metal evaporation source was set to 1000°C, and the heating and cooling rates were 2°C / min. When the Ga metal evaporation source reached the preset evaporation temperature of 1000°C, the beam current intensity was measured using a beam current gauge. The temperature of the evaporation source was adjusted according to the stabilized beam current gauge reading to maintain the beam current intensity at 1×10 -8 mbar, until the most suitable evaporation temperature is found;
[0075] Start the molecular pump to evacuate the fast injection chamber. When the vacuum degree of the fast injection chamber is lower than 10 - 8mbar, the stainless steel tray with the non-intentionally doped gallium oxide substrate fixed thereon is introduced into the MBE growth chamber, the laser is turned on to heat the stainless steel tray to 600°C, the heating rate is set to 5°C / min, and at the same time, the substrate temperature is measured in real time by a temperature sensor and fed back to the laser, and then the laser output power is adjusted to maintain the substrate temperature in a temperature range suitable for epitaxial growth;
[0076] Slowly open the angle valve of the oxygen plasma source pipeline and set the oxygen flow rate to 0.1-0.5sccm on the digital flow meter;
[0077] After the laser heats the stainless steel tray to a preset film growth temperature of 600° C., the oxygen source is turned on to ignite the oxygen plasma, and the oxygen pressure is waited to be stable. The baffle control of the Ga metal evaporation source is set to an automatic mode, and the growth rate is set to be controlled at 10 nanometers / hour to perform homoepitaxial gallium oxide film growth;
[0078] When the thickness of the homoepitaxial gallium oxide film reaches 200 nanometers, the growth is completed, and the baffle of the Ga metal evaporation source is automatically closed to maintain the oxygen source supply; when the temperature of the stainless steel tray is lower than 200°C, the oxygen source is cut off and the laser is turned off;
[0079] The prepared sample is transferred to the fast sampling chamber, and sampling is performed at normal pressure after breaking the vacuum, thereby completing the preparation of homoepitaxial high-quality unintentionally doped gallium oxide thin film on the unintentionally doped gallium oxide substrate.
[0080] Example 3
[0081] A method for preparing a homoepitaxial gallium oxide film on an unintentionally doped substrate based on a molecular beam epitaxy device, the molecular beam epitaxy device comprising an MBE growth chamber, a stainless steel tray arranged in the MBE growth chamber, and an unintentionally doped gallium oxide substrate arranged on the stainless steel tray, wherein the growth surface of the unintentionally doped gallium oxide substrate faces downward, and a laser is arranged below the stainless steel tray, and the laser spot emitted by the laser covers the entire top of the stainless steel tray; the method comprises the steps of:
[0082] Confirm that the water, electricity and gas supply of the MBE equipment is normal, and start the molecular pump to evacuate the MBE growth chamber until the vacuum degree is less than 2×10 -9 mbar;
[0083] Fixing a cleaned 2-inch unintentionally doped gallium oxide substrate on the bottom of a stainless steel tray, with the growth surface of the unintentionally doped gallium oxide substrate facing downward;
[0084] Stop the molecular pump, fill the rapid injection chamber with nitrogen to break the vacuum, and then place the stainless steel tray fixed with the unintentionally doped gallium oxide substrate into the rapid injection chamber;
[0085] The evaporation temperature of the Ga metal evaporation source was set to 1200°C, and the heating and cooling rates were 10°C / min. When the Ga metal evaporation source reached the preset evaporation temperature of 1200°C, the beam intensity was measured using a beam gauge. The temperature of the evaporation source was adjusted according to the stabilized beam gauge reading to maintain the beam intensity at 9×10 -7 mbar, until the most suitable evaporation temperature is found;
[0086] Start the molecular pump to evacuate the fast injection chamber. When the vacuum degree of the fast injection chamber is lower than 10 - 8 mbar, the stainless steel tray with the non-intentionally doped gallium oxide substrate fixed thereon is introduced into the MBE growth chamber, the laser is turned on to heat the stainless steel tray to 1000°C, and the heating rate is set to 15°C / min. At the same time, the substrate temperature is measured in real time by a temperature sensor and fed back to the laser, and the laser output power is then adjusted to maintain the substrate temperature within a temperature range suitable for epitaxial growth;
[0087] Slowly open the angle valve of the oxygen plasma source pipeline and set the oxygen flow rate to 0.5 sccm on the digital flow meter;
[0088] After the laser heats the stainless steel tray to a preset film growth temperature of 1000° C., the oxygen source is turned on to ignite the oxygen plasma, and the oxygen pressure is waited to be stable. The baffle control of the Ga metal evaporation source is set to an automatic mode, and the growth rate is set to be controlled at 100 nanometers / hour to perform homoepitaxial gallium oxide film growth;
[0089] When the thickness of the homoepitaxial gallium oxide film reaches 200 nanometers, the growth is completed, and the baffle of the Ga metal evaporation source is automatically closed to maintain the oxygen source supply; when the temperature of the stainless steel tray is lower than 200°C, the oxygen source is cut off and the laser is turned off;
[0090] The prepared sample is transferred to the fast sampling chamber, and sampling is performed at normal pressure after breaking the vacuum, thereby completing the preparation of homoepitaxial high-quality unintentionally doped gallium oxide thin film on the unintentionally doped gallium oxide substrate.
[0091] Comparative Example 1
[0092] A method for preparing a homoepitaxial gallium oxide thin film on an unintentionally doped substrate based on a molecular beam epitaxy device, the molecular beam epitaxy device comprising an MBE growth chamber, a stainless steel tray arranged in the MBE growth chamber, and an unintentionally doped gallium oxide substrate arranged on the stainless steel tray, wherein a heating wire is arranged above the stainless steel tray; the method comprises the steps of:
[0093] Confirm that the water, electricity and gas supply of the MBE equipment is normal, and start the molecular pump to evacuate the MBE growth chamber until the vacuum degree is less than 2×10 -9 mbar;
[0094] Fixing a cleaned 2-inch unintentionally doped gallium oxide substrate on the bottom of a stainless steel tray, with the growth surface of the unintentionally doped gallium oxide substrate facing downward;
[0095] Stop the molecular pump, fill the rapid injection chamber with nitrogen to break the vacuum, and then place the stainless steel tray fixed with the unintentionally doped gallium oxide substrate into the rapid injection chamber;
[0096] The evaporation temperature of the Ga metal evaporation source was set to 1100°C, and the heating and cooling rates were 6°C / min. When the Ga metal evaporation source reached the preset evaporation temperature of 1100°C, the beam current intensity was measured using a beam current gauge. The temperature of the evaporation source was adjusted according to the stabilized beam current gauge reading to maintain the beam current intensity at 5×10 -7 mbar, until the most suitable evaporation temperature is found;
[0097] Start the molecular pump to evacuate the fast injection chamber. When the vacuum degree of the fast injection chamber is lower than 10 - 8 mbar, the stainless steel tray fixed with the non-intentionally doped gallium oxide substrate is introduced into the MBE growth chamber, the stainless steel tray is heated to 800°C by a heating wire, and the heating rate is set to 10°C / min. At the same time, the substrate temperature is measured in real time by a temperature sensor and fed back to the laser, and then the laser output power is adjusted to maintain the substrate temperature in a temperature range suitable for epitaxial growth;
[0098] Slowly open the angle valve of the oxygen plasma source pipeline and set the oxygen flow rate to 0.3 sccm on the digital flow meter;
[0099] After the laser heats the stainless steel tray to a preset film growth temperature of 800° C., the oxygen source is turned on to ignite the oxygen plasma, and the oxygen pressure is waited to be stable. The baffle control of the Ga metal evaporation source is set to an automatic mode, and the growth rate is set to 50 nanometers / hour to perform homoepitaxial gallium oxide film growth;
[0100] When the thickness of the homoepitaxial gallium oxide film reaches 200 nanometers, the growth is completed, and the baffle of the Ga metal evaporation source is automatically closed to maintain the oxygen source supply; when the temperature of the stainless steel tray is lower than 200°C, the oxygen source is cut off and the power supply of the heating wire is turned off;
[0101] The prepared sample is transferred to the fast sampling chamber, and sampling is performed at normal pressure after breaking the vacuum, thereby completing the preparation of homoepitaxial high-quality unintentionally doped gallium oxide thin film on the unintentionally doped gallium oxide substrate.
[0102] Example 4
[0103] The thickness and thickness standard deviation of the homoepitaxial gallium oxide films prepared in Examples 1-3 and Comparative Example 1 were measured.
[0104] After the homoepitaxial gallium oxide film on the wafer is prepared, 32 points are selected in a cross-shaped pattern on the wafer (8 points are distributed at equal intervals in four diameter directions, and the four directions are equally spaced at an angle of 45 degrees, excluding the center of the circle) for film thickness measurement: a cross-sectional fault is made at the test point position on the surface of the epitaxial wafer using a focused ion beam (FIB). The interface between the epitaxial layer and the substrate can be clearly seen using a SEM, and the thickness of the homoepitaxial gallium oxide film can be accurately measured. The results are shown in Table 1:
[0105] Table 1 Homoepitaxial gallium oxide film thickness measurement results
[0106]
[0107] It can be seen from the results in Table 1 that, compared with the comparative example, the thickness of the homoepitaxial gallium oxide film prepared by the method of the present invention is closer to the target thickness, and the standard deviation of the thickness of the homoepitaxial gallium oxide film prepared by the method of the present invention is smaller, indicating that the homoepitaxial gallium oxide film prepared by the present invention has higher thickness uniformity and better quality.
[0108] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing a homoepitaxial gallium oxide thin film on an unintentionally doped substrate based on a molecular beam epitaxy device, characterized in that: The molecular beam epitaxy equipment comprises an MBE growth chamber, a stainless steel tray arranged in the MBE growth chamber, and an unintentionally doped gallium oxide substrate fixedly arranged at the bottom of the stainless steel tray, a laser is arranged above the stainless steel tray, the laser wavelength emitted by the laser is 500-1500nm, and the laser spot emitted by the laser covers the entire top of the stainless steel tray; The method comprises the steps of: Start the molecular pump in advance to evacuate the MBE growth chamber; Fixing the unintentionally doped gallium oxide substrate on the bottom end of the stainless steel tray, with the growth surface of the unintentionally doped gallium oxide substrate facing downward; Stop the molecular pump, fill the rapid injection chamber with nitrogen to break the vacuum, and then place the stainless steel tray fixed with the unintentionally doped gallium oxide substrate into the rapid injection chamber; Setting the evaporation temperature of the Ga metal evaporation source, and when the Ga metal evaporation source reaches the preset evaporation temperature, controlling the velocity flow intensity of the Ga metal evaporation source; Start the molecular pump to evacuate the fast injection chamber. When the vacuum degree of the fast injection chamber is lower than 10 -8 mbar, introducing the stainless steel tray with the non-intentionally doped gallium oxide substrate fixed thereon into the MBE growth chamber, and turning on the laser to heat the stainless steel tray; Slowly open the angle valve of the oxygen plasma source pipeline and set the oxygen flow rate to 0.1-0.5sccm on the digital flow meter; After the laser heats the stainless steel tray to a preset film growth temperature, the oxygen source is turned on to ignite the oxygen plasma, and the oxygen pressure is waited to be stable, and the baffle control of the Ga metal evaporation source is set to an automatic mode to perform homoepitaxial gallium oxide film growth; When the thickness of the homoepitaxial gallium oxide film reaches 50-500 nanometers, the growth is completed, and the baffle of the Ga metal evaporation source is automatically closed to maintain the oxygen source supply; when the temperature of the stainless steel tray is lower than 200°C, the oxygen source is cut off, the laser is turned off, and the preparation of the homoepitaxial gallium oxide film is completed; In the step of starting the molecular pump to evacuate the MBE growth chamber in advance, the MBE growth chamber is evacuated to a vacuum level lower than 2×10 -9 mbar; The Ga metal evaporation source has a preset evaporation temperature of 1000-1200°C and a heating rate of 2-10°C / min. The Ga metal evaporation source has a flow rate of 1×10 -8 -9×10 -7 mbar; The laser heats the stainless steel tray to a preset film growth temperature step, the preset film growth temperature is 600-1000° C., and the heating rate is 5-15° C. / min; The growth rate of homoepitaxial gallium oxide films is 10-100 nm / hour.
2. The method for preparing a homoepitaxial gallium oxide thin film on an unintentionally doped substrate according to claim 1, characterized in that: After the homoepitaxial gallium oxide film is prepared, the prepared homoepitaxial gallium oxide film is transferred from the MBE growth chamber to the fast sampling chamber, and sampling is performed at normal pressure after breaking the vacuum.
3. The method for preparing a homoepitaxial gallium oxide thin film on an unintentionally doped substrate according to claim 1, characterized in that: The laser is provided with a beam expander.
Citation Information
Patent Citations
Crystal laminate structure and method for producing same
CN103781948A
ZnO-BASED p-TYPE SEMICONDUCTOR CRYSTAL, SEMICONDUCTOR COMPOSITE BODY OBTAINED BY USING THE SAME, LIGHT EMITTING ELEMENT OBTAINED BY USING THE SAME AND ITS MANUFACTURING METHOD