Lithium metal anode and preparation method thereof

By using carbon nanotube sponge structure and carbon deposit layer in lithium metal anode, the problem of uneven deposition of lithium metal anode is solved, and stable deposition of lithium and extended battery cycle life are achieved.

CN114824184BActive Publication Date: 2024-11-05TSINGHUA UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110123588.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-29
Publication Date
2024-11-05
Estimated Expiration
2041-01-29

AI Technical Summary

Technical Problem

The existing lithium metal anode is unevenly deposited during circulation, resulting in the growth and structural loss of lithium dendrites, which in turn affects battery capacity and Coulomb efficiency and increases the risk of failure.

Method used

Using a carbon nanotube sponge structure, a porous structure is formed by forming a carbon layer on the surface of the carbon nanotube and filling it with lithium metal material to form a porous structure to stabilize the deposition and peeling of lithium, reduce the current density, and inhibit the formation of lithium dendritic crystals.

Benefits of technology

The uniform distribution and stable deposition of lithium are achieved, the cycle life of lithium-ion batteries is extended, and the Coulomb efficiency and battery stability are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114824184B_ABST
    Figure CN114824184B_ABST
Patent Text Reader

Abstract

A lithium metal anode includes a carbon nanotube sponge and a lithium metal material, wherein the carbon nanotube sponge includes a plurality of carbon nanotubes with surfaces covered by a carbon deposition layer and a plurality of micropores, wherein the plurality of micropores are formed by the plurality of carbon nanotubes with surfaces covered by a carbon deposition layer, and the lithium metal material is filled in the plurality of micropores and covers the carbon nanotubes covered by the carbon deposition layer. The present invention also relates to a method for preparing a lithium metal anode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a lithium metal anode and a preparation method thereof. Background Art

[0002] Lithium-ion batteries are widely used in electric vehicles, portable electronic devices, etc. The negative electrode of conventional lithium-ion batteries is graphite, with a theoretical capacity of 372 mAh g -1 , unable to meet the growing demand for higher lithium-ion battery capacity. Lithium metal anodes are considered the "holy grail" electrode for next-generation rechargeable batteries due to their high theoretical capacity of 3860 mAh g-1 and low redox potential of -3.04 V.

[0003] However, existing lithium metal anodes have some problems that hinder their practical application. The deposition of lithium in the cycle is uneven, and the uneven deposition will lead to the growth of lithium dendrites. The chemical reaction between lithium and liquid electrolyte forms a solid electrolyte interface (SEI) on the surface of lithium metal. Lithium dendrites penetrate SEI, and the fresh lithium under SEI reacts with the liquid electrolyte, resulting in electrolyte consumption and side reactions. When the dendrites are too long, the lithium dendrites will break and lose contact with the lithium metal anode, which will lead to "lithium depletion" and the structure of the lithium metal anode will disappear. And these problems ultimately lead to capacity loss, low coulombic efficiency and high risk of battery failure. Therefore, solving the lithium dendrite problem, improving the coulombic efficiency of the lithium anode and the volume effect problem are the only way to promote the industrialization of lithium anodes or lithium metal batteries. Summary of the invention

[0004] In view of this, it is indeed necessary to provide a lithium metal anode that can overcome the above shortcomings.

[0005] A lithium metal anode includes a carbon nanotube sponge and a lithium metal material. The carbon nanotube sponge includes a plurality of carbon nanotubes whose surfaces are covered with a carbon deposition layer and a plurality of micropores. The plurality of micropores are formed by the plurality of carbon nanotubes whose surfaces are covered with a carbon deposition layer. The lithium metal material is filled in the plurality of micropores and covers the carbon nanotubes covered with the carbon deposition layer.

[0006] A lithium metal anode includes a metal lithium block and a plurality of carbon nanotube wires, wherein the metal lithium block includes a plurality of gaps, each of the gaps is filled with at least one carbon nanotube wire, and the carbon nanotube wire includes a carbon nanotube and a carbon deposition layer, wherein the carbon deposition layer is wrapped around the surface of the carbon nanotube.

[0007] A method for preparing a lithium metal anode comprises:

[0008] Prepare a carbon nanotube raw material, wherein the carbon nanotube raw material is directly scraped from a carbon nanotube array;

[0009] The carbon nanotube raw material is added into an organic solvent and subjected to ultrasonic vibration to form a flocculent structure;

[0010] washing the flocculent structure with water;

[0011] The washed flocculent structure is freeze-dried under a vacuum environment to obtain a carbon nanotube sponge preform;

[0012] Performing carbon deposition on the carbon nanotube sponge preform to form a carbon deposition layer to obtain the carbon nanotube sponge;

[0013] The molten lithium is placed in contact with the carbon nanotube sponge in an oxygen-free atmosphere, and the molten lithium is hot-injected into the carbon nanotube sponge and cooled to form a lithium metal anode.

[0014] The lithium metal anode provided by the present invention has the following beneficial effects: amorphous carbon covers the surface of carbon nanotubes and improves the mechanical strength of carbon nanotubes, and separates carbon nanotubes to prevent carbon nanotubes from agglomerating; the structure of carbon nanotube sponge is stable and porous, with strong mechanical strength, which is conducive to the recombination of lithium. The amorphous carbon layer has good lithium affinity, so that the lithium in the lithium metal anode is evenly distributed and filled in the micropores of the carbon nanotube sponge. At the same time, the porous carbon nanotube sponge acts as a stable skeleton of lithium, provides a strong skeleton and sufficient space for lithium deposition / stripping, and reduces the current density along the surface of the lithium metal anode, inhibits the formation of lithium dendrites, and makes SEI complete and stable, which is conducive to improving the cycle life of the lithium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 A flow chart of a method for preparing a lithium metal anode provided in an embodiment of the present invention.

[0016] Figure 2 This is a scanning electron microscope (SEM) image of a lithium metal anode provided in an embodiment of the present invention.

[0017] Figure 3 Schematic diagram and cross-sectional diagram of the structure of the lithium metal anode provided in an embodiment of the present invention.

[0018] Figure 4 This is a schematic diagram of an enlarged local structure of a carbon nanotube sponge provided in an embodiment of the present invention.

[0019] Figure 5 This is a schematic diagram of the structure of a lithium-ion battery provided by an embodiment of the present invention.

[0020] Figure 6Transmission electron microscope (TEM) images of the carbon nanotube sponge preform and the carbon nanotube sponge of Example 1 of the present invention.

[0021] Figure 7 1 is a SEM image of the carbon nanotube sponge preform and the carbon nanotube sponge of Example 1 of the present invention.

[0022] Figure 8 This is a Raman spectrum diagram of the carbon nanotube sponge preform and the carbon nanotube sponge of Example 1 of the present invention.

[0023] Fig. 9 This is a BET side view of the carbon nanotube sponge preform and the carbon nanotube sponge of Example 1 of the present invention.

[0024] Fig.10 This is a pore size distribution diagram of the carbon nanotube sponge preform and the carbon nanotube sponge of Example 1 of the present invention.

[0025] Fig.11 This is a diagram of the pressure test process of the carbon nanotube sponge preform and the carbon nanotube sponge of Example 1 of the present invention.

[0026] Fig.12 These are structural comparison diagrams before and after adding electrolyte to the carbon nanotube sponge preform and the carbon nanotube sponge in Example 1 of the present invention.

[0027] Fig.13 This is a process diagram of hot-injection of molten lithium into carbon nanotube sponge according to Example 1 of the present invention.

[0028] Fig.14 This is a comparison chart of lithium affinity tests of the carbon nanotube sponge, the carbon nanotube sponge preform, the amorphous carbon coated stainless steel and the original stainless steel according to Example 1 of the present invention.

[0029] Fig.15 This is the XPS spectrum of the lithium metal anode of Example 1 of the present invention.

[0030] Fig.16 This is a voltage-time curve of a symmetrical battery using a pure lithium metal electrode according to Example 2 of the present invention.

[0031] Fig.17 This is a voltage-time curve of a symmetrical battery using a lithium metal anode according to Example 2 of the present invention.

[0032] Fig.18 The voltage-time curve of the symmetrical battery of the pure lithium metal electrode and the lithium metal anode in Example 2 of the present invention at a cycle time of 78-80h.

[0033] Fig.19 This is a voltage-time curve of a symmetrical battery using a pure lithium metal electrode according to Example 2 of the present invention.

[0034] Fig. 20 This is a voltage-time curve of a symmetrical battery using a lithium metal anode according to Example 2 of the present invention.

[0035] Fig.21 Nyquist diagrams of a symmetric battery using a pure lithium metal electrode and a symmetric battery using a lithium metal anode before cycling according to Example 2 of the present invention.

[0036] Fig. 22 The Nyquist diagram of a symmetric battery using a pure lithium metal electrode and a symmetric battery using a lithium metal anode after cycling for 20 hours according to Example 2 of the present invention.

[0037] Fig.23 This is a surface SEM image of a pure lithium metal electrode after the symmetric battery using the pure lithium metal electrode of Example 2 of the present invention was cycled for 100 hours.

[0038] Fig.24 This is a surface SEM image of the lithium metal anode of the symmetric battery using the lithium metal anode of Example 2 of the present invention after cycling for 100 hours.

[0039] Fig.25 This is a cross-sectional SEM image of a pure lithium metal electrode after the symmetric battery using the pure lithium metal electrode was cycled for 100 hours in Example 2 of the present invention.

[0040] Fig.26 This is a cross-sectional SEM image of the lithium metal anode of the symmetrical battery using the lithium metal anode according to Example 2 of the present invention after cycling for 100 hours.

[0041] Fig. 27 Graph showing the cycle performance of a half-cell containing a pure lithium anode and a half-cell containing a lithium metal anode according to Example 3 of the present invention.

[0042] Fig.28 Graph showing the rate performance of a half-cell containing a pure lithium anode and a half-cell containing a lithium metal anode according to Example 3 of the present invention.

[0043] Main component symbols

[0044] Lithium metal anode 10

[0045] Carbon nanotube sponge 12

[0046] Carbon Nanotubes 122

[0047] Carbon deposit layer 124

[0048] Micropore 126

[0049] Lithium metal materials14

[0050] Lithium-ion battery 100

[0051] Housing 20

[0052] Cathode 30

[0053] Electrolyte 40

[0054] Diaphragm 50

[0055] The following specific implementation manner will further illustrate the present invention in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION

[0056] Please refer to Figure 1 The present invention provides a method for preparing a lithium metal anode, comprising:

[0057] Step 1, preparing a carbon nanotube raw material, wherein the carbon nanotube raw material is directly scraped from a carbon nanotube array;

[0058] Step 2, adding the carbon nanotube raw material into an organic solvent and ultrasonically vibrating the organic solvent to form a flocculent structure;

[0059] Step 3, washing the flocculent structure with water;

[0060] Step 4: freeze-drying the washed flocculent structure under vacuum to obtain a carbon nanotube sponge preform;

[0061] Step 5, performing carbon deposition on the carbon nanotube sponge preform to form a carbon deposition layer to obtain the carbon nanotube sponge;

[0062] Step six, placing molten lithium in contact with the carbon nanotube sponge in an oxygen-free atmosphere, hot-injecting the molten lithium into the carbon nanotube sponge and cooling the carbon nanotube sponge to form a lithium metal anode.

[0063] In step 1, the carbon nanotube raw material is composed of a plurality of carbon nanotubes. The carbon nanotubes include single-walled carbon nanotubes, double-walled carbon nanotubes or multi-walled carbon nanotubes. The diameter of the carbon nanotubes is 10 nanometers to 30 nanometers. The length of the carbon nanotubes is greater than 100 micrometers, preferably, the length of the carbon nanotubes is greater than 300 micrometers. In this embodiment, the diameter of the carbon nanotubes is 10 nanometers to 20 nanometers, and the length of the carbon nanotubes is 300 micrometers. The carbon nanotubes are preferably carbon nanotubes with a pure surface free of impurities and without any chemical modification. It can be understood that impurities or chemical modification will destroy the interaction between carbon nanotubes. The preparation method of the carbon nanotube raw material is: prepare a carbon nanotube array on a substrate; use a blade or other tool to scrape the carbon nanotube array from the substrate to obtain the carbon nanotube raw material. Since the carbon nanotube raw material is directly obtained from the carbon nanotube array, the carbon nanotube sponge prepared using the carbon nanotube raw material has better strength. Preferably, the carbon nanotube array is a super-ordered carbon nanotube array. The so-called super-ordered carbon nanotube array means that the carbon nanotubes in the carbon nanotube array are relatively long, generally greater than or equal to 300 microns, the surface of the carbon nanotubes is pure, and basically does not contain impurities such as amorphous carbon or residual catalyst metal particles, and the arrangement direction of the carbon nanotubes is basically consistent.

[0064] In step 2, the carbon nanotube raw material is added into an organic solvent and ultrasonically vibrated for a period of time to form a flocculent structure.

[0065] The organic solvent is preferably an organic solvent having good wettability with carbon nanotubes, such as ethanol, methanol, acetone, isopropanol, dichloroethane or chloroform, etc. The ratio of the carbon nanotube raw material to the organic solvent can be selected according to actual needs.

[0066] The power of the ultrasonic oscillation is 300 watts to 1500 watts, preferably 500 watts to 1200 watts. The time of ultrasonic oscillation is 10 minutes to 60 minutes. After the ultrasonic oscillation, the carbon nanotubes in the carbon nanotube raw material will be evenly distributed in the organic solvent to form a flocculent structure. Since the carbon nanotube raw material is directly scraped from a super-aligned carbon nanotube array, even through the above-mentioned ultrasonic oscillation process, the carbon nanotubes in the carbon nanotube raw material will not separate from each other, but will maintain a flocculent structure that is mutually entangled, attracted, and entangled. The flocculent structure has a plurality of pores. Since the organic solvent has good wetting properties for carbon nanotubes, the carbon nanotube raw material can be evenly distributed in the organic solvent. In the present embodiment, the carbon nanotube raw material is added to ethanol and ultrasonically oscillated for 30 minutes.

[0067] Step three, washing the flocculent structure with water.

[0068] Since the freezing point of the organic solvent is generally lower than -100°C, it is not conducive to subsequent freeze drying. Therefore, by washing the flocculent structure with water, the pores in the flocculent structure can be filled with water, which is conducive to subsequent freeze drying. In this embodiment, the flocculent structure is washed with deionized water to remove ethanol, so that the pores in the flocculent structure are filled with water.

[0069] Step 4: freeze-dry the washed flocculent structure under a vacuum environment to obtain a carbon nanotube sponge preform.

[0070] The step of freeze-drying the flocculent structure includes: placing the flocculent structure in a freeze dryer and rapidly cooling it to below -40°C; and evacuating the flocculent structure and gradually raising the temperature to room temperature in stages, and drying it for 1-10 hours when the temperature of each stage is reached. It can be understood that vacuum freeze drying can prevent the collapse of the carbon nanotube sponge preform, which is conducive to the subsequent formation of a fluffy carbon nanotube sponge. The density of the carbon nanotube sponge preform is 0.5 mg / cm 3 To 100mg / cm 3 In this embodiment, the carbon nanotube sponge preform is cut into a cylinder with a diameter of 16 mm and a density of 10 mg / cm 3 .

[0071] In step five, the method of carbon deposition on the carbon nanotube sponge preform is not limited, and may be chemical vapor deposition or electrochemical deposition. The chemical vapor deposition method is to introduce a carbon source gas such as methane or acetylene, and under the condition of a protective gas such as argon, heat it to 700°C-1200°C to decompose the carbon source gas, thereby forming a carbon deposition layer. The carbon deposition layer uniformly covers the surface of each carbon nanotube, and the carbon deposition layer is connected into one piece at the connection between the carbon nanotubes and forms a plurality of micropores. The time for carbon deposition on the carbon nanotube sponge preform may be 1 minute to 240 minutes. It is understood that the longer the carbon deposition time is, the thicker the carbon deposition layer can be formed on the surface of each carbon nanotube. It may be crystalline carbon, amorphous carbon or a mixture thereof. The thickness of the carbon deposition layer is 2 nanometers to 100 nanometers. In this embodiment, the carbon nanotube sponge preform is heated at 800° C. for 10 minutes in a mixed atmosphere of nitrogen and acetylene to form an amorphous carbon layer to obtain the carbon nanotube sponge. The thickness of the amorphous carbon layer is 4 nanometers.

[0072] Step six, placing molten lithium in contact with carbon nanotube sponge in an oxygen-free atmosphere, hot-injecting the molten lithium into the carbon nanotube sponge and cooling the carbon nanotube sponge to form a lithium metal anode.

[0073] A lithium sheet is heated to 200°C to 300°C to obtain molten lithium, and the molten lithium is placed on one surface of the carbon nanotube sponge in an oxygen-free atmosphere, so that the molten lithium slowly penetrates into the micropores of the carbon nanotube sponge and fills the micropores and cools. In this embodiment, a pure lithium sheet is heated to 300°C to obtain molten lithium, and argon is filled in a glove box to place the molten lithium on the surface of the carbon nanotube sponge, so that the molten lithium slowly penetrates into the micropores of the carbon nanotube sponge and cools at room temperature to form a lithium metal anode. The amount of molten lithium can be selected according to actual needs, specifically, it can be selected according to the size of the lithium metal anode to be formed. Preferably, the amount of molten lithium can cover the entire carbon nanotube sponge. The internal space of the carbon nanotube sponge with the same density or the same mass is basically the same, so the amount of injected molten lithium is also basically the same. In this embodiment, the mass of the amount of injected molten lithium is about 170mg-180mg.

[0074] Furthermore, a step of cutting the lithium metal anode may be included. The lithium metal anode may be cut into a desired size according to actual needs. Further, a rolling step may be included to press the lithium metal anode to a desired thickness. In this embodiment, the lithium metal anode is pressed to a thickness of 600 μm by a rolling mill.

[0075] The method for preparing a lithium metal anode provided by the present invention has the following beneficial effects: an amorphous carbon layer is deposited on the surface of the carbon nanotube sponge preform, molten lithium is placed in contact with the carbon nanotube sponge, and a lithium metal anode with the carbon nanotube sponge is manufactured by simple hot injection, and the preparation process is simple and easy to operate. At the same time, the carbon nanotube sponge coated with amorphous carbon shows a stable structure, and the amorphous carbon has good lithium affinity and can interact with lithium, thereby achieving direct diffusion of molten lithium into the micropores of the carbon nanotube sponge to form a lithium metal anode.

[0076] Please refer to Figure 2-4 The present invention provides a lithium metal anode 10 prepared by the above method. The lithium metal anode 10 includes a carbon nanotube sponge 12 and a lithium metal material 14. The carbon nanotube sponge 12 includes a plurality of carbon nanotubes 122 whose surfaces are covered by a carbon deposition layer 124 and a plurality of micropores 126. The plurality of micropores 126 are formed by the plurality of carbon nanotubes 122 whose surfaces are covered by a carbon deposition layer 124, and the lithium metal material 14 is filled in the plurality of micropores 126.

[0077] The carbon nanotube sponge 12 includes a plurality of carbon nanotubes 122, which are intertwined to form a carbon nanotube network structure, and a plurality of pores are formed between the plurality of intertwined carbon nanotubes 122. The carbon deposition layer 124 uniformly covers the surface of each of the carbon nanotubes 122, and the carbon deposition layer 124 is connected to form a plurality of micropores 126 at the connection between the carbon nanotubes. The lithium metal material 14 is attached to the surface of the carbon deposition layer 124 and filled in the micropores 126. Preferably, the lithium metal anode 10 is composed of the carbon nanotube sponge 12 and the lithium metal material 14. The carbon nanotube sponge 12 is composed of the plurality of carbon nanotubes 122 and the carbon deposition layer 124. The plurality of carbon nanotubes 122 are intertwined to form a carbon nanotube network structure, and a plurality of pores are formed between the plurality of intertwined carbon nanotubes 122. The carbon deposition layer 124 uniformly covers the surface of each carbon nanotube 122, and the carbon deposition layer 124 is connected to form a piece at the connection between the carbon nanotubes and forms a plurality of micropores 126. The intersection of two adjacent carbon nanotubes 122 forms at least one contact portion, and the contact portion is entirely covered by the carbon deposition layer 124, and the carbon deposition layer 124 does not prevent the carbon nanotubes 122 from directly contacting each other at the contact portion. The lithium metal material 14 covers the surface of the carbon deposition layer 124 and fills the micropores 126. The lithium metal material 14 is a pure lithium material.

[0078] The carbon nanotubes include single-walled carbon nanotubes, double-walled carbon nanotubes or multi-walled carbon nanotubes. The diameter of the carbon nanotubes is 10 nanometers to 30 nanometers. The length of the carbon nanotubes is greater than 100 micrometers, and preferably, the length of the carbon nanotubes is greater than 300 micrometers. In this embodiment, the diameter of the carbon nanotubes is 10 nanometers to 20 nanometers, and the length of the carbon nanotubes is 300 micrometers. The carbon nanotubes are pure carbon nanotubes. The carbon nanotubes are pure and free of impurities on the surface and have not undergone any chemical modification. That is, the surface of the carbon nanotubes does not contain impurities such as amorphous carbon; the carbon nanotubes are also not modified with functional groups, such as hydroxyl groups, carboxyl groups, etc.

[0079] The carbon deposit layer 124 may be crystalline carbon, amorphous carbon or a mixture thereof. The thickness of the carbon deposit layer is 2 nanometers to 100 nanometers. In the present embodiment, the carbon deposit layer 124 is an amorphous carbon layer, and the thickness of the amorphous carbon layer is 4 nanometers. In the lithium metal anode 10, the mass percentage of carbon nanotubes is 6% to 10%, the mass percentage of the carbon deposit layer is 0.5% to 1%, and the mass percentage of metallic lithium is 85% to 95%. In the present embodiment, in the lithium metal anode 10, the mass percentage of carbon nanotubes is 7.8%, the mass percentage of the carbon deposit layer is 0.77%, and the mass percentage of metallic lithium is 91.43%.

[0080] The carbon nanotubes 122 coated with the carbon deposition layer 124 on the outside can also be called carbon nanotube wires. That is, the lithium metal anode 10 includes a metal lithium block and a plurality of carbon nanotube wires. The plurality of carbon nanotube wires are in contact with each other to form a carbon nanotube wire network structure. The metal lithium block includes a plurality of gaps, each of which is filled with at least one carbon nanotube wire. Specifically, at a location where two carbon nanowires intersect with each other, the intersection of two adjacent carbon nanotubes 122 forms at least one contact portion, and the contact portion is entirely coated with the carbon deposition layer 124, and the carbon deposition layer 124 does not prevent the carbon nanotubes 122 from directly contacting each other at the contact portion.

[0081] Preferably, the carbon nanotube wire fills up the plurality of gaps in the metal lithium block. The at least one carbon nanotube wire is composed of a pure carbon nanotube and the carbon deposition layer.

[0082] The lithium metal anode provided by the present invention has the following beneficial effects: amorphous carbon covers the surface of carbon nanotubes and improves the mechanical strength of carbon nanotubes, separates carbon nanotubes to prevent carbon nanotubes from agglomerating, and the structure of carbon nanotube sponge is stable and porous, has strong mechanical strength, and is conducive to the recombination of lithium. The amorphous carbon layer has good lithium affinity, so that the lithium in the lithium metal anode is evenly distributed and filled in the micropores of the carbon nanotube sponge. At the same time, the porous carbon nanotube sponge acts as a stable skeleton of lithium, provides a strong skeleton and sufficient space for lithium deposition / stripping, and reduces the current density along the surface of the lithium metal anode, inhibits the formation of lithium dendrites, and makes SEI complete and stable, which is conducive to improving the cycle life of the lithium ion battery.

[0083] Please refer to Figure 5 The present invention further provides a lithium ion battery 100 using the above-mentioned lithium metal anode, which includes: a shell 20 and a lithium metal anode 10, a cathode 30, an electrolyte 40 and a separator 50 placed in the shell 20. In the lithium ion battery 100, the electrolyte 40 is placed in the shell 20, the lithium metal anode 10, the cathode 30 and the separator 50 are placed in the electrolyte 40, and the separator 50 is placed between the lithium metal anode 10 and the cathode 30, dividing the internal space of the shell 20 into two parts, and the lithium metal anode 10 and the separator 50 and the cathode 30 and the separator 50 are kept spaced apart.

[0084] The lithium metal anode 10 is the lithium metal anode including the carbon nanotube sponge 12 and the lithium metal material, which will not be described again.

[0085] The lithium-ion battery cathode 30 includes a cathode active material layer and a current collector. The cathode material layer includes a uniformly mixed cathode active material, a conductive agent and a binder. The cathode active material can be lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide or lithium iron phosphate. The current collector can be a metal sheet, such as a platinum sheet.

[0086] The separator 50 may be a polypropylene microporous membrane, the electrolyte salt in the electrolyte may be lithium hexafluorophosphate, lithium tetrafluoroborate or lithium bis(oxalato)borate, etc., and the organic solvent in the electrolyte may be ethylene carbonate, diethyl carbonate or dimethyl carbonate, etc. It is understood that the separator 50 and the electrolyte may also be made of other commonly used materials.

[0087] Example 1

[0088] A super ordered carbon nanotube array is provided, wherein the diameter of the carbon nanotubes in the carbon nanotube array is 20 nanometers and the length is 300 micrometers; 100 milligrams of the carbon nanotube array is scraped, added to a mixture of 100 milliliters of ethanol and 100 milliliters of deionized water, and ultrasonically stirred for 30 minutes with an ultrasonic wave of 400 watts to form a flocculent structure; the flocculent structure is washed with water; the washed flocculent structure is placed in a freeze dryer, and rapidly cooled to -30°C and frozen for 12 hours; then the temperature is raised to -10°C, vacuumed to 10Pa, and dried for 12 hours, then the vacuum system is closed, the air inlet valve of the freeze dryer is opened, the sample is taken out, and the carbon nanotube sponge preform is obtained; the carbon nanotube sponge preform is transferred to a reactor, acetylene (flow rate is 10 sccm) and argon are introduced, and the mixture is heated to 800°C to decompose the acetylene, and carbon is deposited in the carbon nanotube sponge preform for 10 minutes. The mass percentage of amorphous carbon in the carbon nanotube sponge is about 9%, and the thickness of the amorphous carbon layer is 4 nanometers. The pure lithium sheet is heated to 300° C. to obtain liquid lithium, and argon gas is filled in a glove box to place the molten lithium on the surface of the carbon nanotube sponge to form a lithium metal anode.

[0089] Comparative Example 1

[0090] The sample of Comparative Example 1 is the carbon nanotube sponge preform in Example 1.

[0091] The properties of the carbon nanotube sponge in Example 1 and the carbon nanotube sponge preform in Comparative Example 1 are compared below.

[0092] The morphology of the carbon nanotube sponge preform and carbon nanotube sponge was examined by transmission electron microscopy (TEM) and scanning electron microscopy (SEM). Figure 6 (a) TEM image of carbon nanotube sponge preform; Figure 6 (b) is a TEM image of a carbon nanotube sponge. The thickness of the carbon nanotube wall in the carbon nanotube sponge is 8.5 nm, and the thickness of the carbon nanotube wall in the carbon nanotube sponge preform is 4.5 nm. The thicker carbon nanotube wall in the carbon nanotube sponge is due to the amorphous carbon layer coating the surface of the carbon nanotube wall. Figure 7 (a) is the SEM image of the carbon nanotube sponge preform; Figure 7(b) SEM image of carbon nanotube sponge preform and carbon nanotube sponge. Figure 7 (a) and 7(b) show that the carbon nanotube sponge preform and the carbon nanotube sponge have a 3D porous structure. It can be seen that amorphous carbon does not affect the porous structure of the carbon nanotube sponge.

[0093] The amorphous carbon on the carbon nanotube sponge was further detected by Raman test. The Raman spectrum contains two characteristic bands, D band (1374cm -1 ) and G belt (1580cm -1 ). The intensity ratio of the D band and the G band (Id / Ig) indicates the concentration of defects and amorphous carbon in the carbon nanotubes. Figure 8 The Id / Ig ratio of the carbon nanotube sponge preform was shown to be 0.853. In the carbon nanotube sponge, the intensity of the D band increased and the Id / Ig ratio increased to 1.061. Raman spectroscopy showed that amorphous carbon was introduced into the carbon nanotube sponge.

[0094] The specific surface areas of the carbon nanotube sponge preform and the carbon nanotube sponge were detected by BET test. Fig. 9 BET side view of carbon nanotube sponge preform and carbon nanotube sponge. Fig. 9 The specific surface area of ​​carbon nanotube sponge is 60.12 m 2 g -1 The specific surface area of ​​the carbon nanotube sponge preform is 86.82m 2 g -1 . Fig.10 Figure 2 is the pore size distribution diagram of carbon nanotube sponge preform and carbon nanotube sponge. Fig.10 As shown, mesopores and micropores were observed in both the carbon nanotube sponge preform and the carbon nanotube sponge, and macropores were dominant, indicating that both the carbon nanotube sponge preform and the carbon nanotube sponge had porous structures. Although the specific surface area and the number of mesopores and micropores of the carbon nanotube sponge decreased after the introduction of amorphous carbon into the carbon nanotube sponge, the carbon nanotube sponge still showed a relatively large surface area and provided sufficient space for lithium.

[0095] In addition to sufficient space, a stable structure is also important for the lithium metal anode. Therefore, experimental tests were conducted to verify the stable structure of the carbon nanotube sponge. Fig.11 The figure shows the pressure test process of carbon nanotube sponge preform and carbon nanotube sponge. Fig.11 As shown in (a) and 11(b), pressure is applied to the carbon nanotube sponge preform and the carbon nanotube sponge, and the carbon nanotube sponge preform and the carbon nanotube sponge are pressed into a thin film, and the pressure is removed after a few seconds. The carbon nanotube sponge preform cannot recover and remains in a thin film state after pressing, while the carbon nanotube sponge can return to the previous state. Fig.12The following are structural comparison diagrams before and after adding electrolyte to the carbon nanotube sponge preform and carbon nanotube sponge. Fig.12 As shown in (a) and 12(b), after 200 μl of electrolyte was dropped onto the carbon nanotube sponge preform and the carbon nanotube sponge respectively, the carbon nanotube sponge remained fluffy, while the carbon nanotube sponge preform collapsed after adding the electrolyte. The above tests confirmed that the carbon nanotube sponge preform became more stable after being coated with amorphous carbon, which covered the surface of the carbon nanotubes and improved the mechanical strength of the carbon nanotubes, and separated the carbon nanotubes to prevent the carbon nanotubes from agglomerating. Therefore, the carbon nanotube sponge has a stable structure, strong mechanical strength, and is conducive to the recombination of lithium.

[0096] Lithium Affinity Test of Lithium Metal Anode

[0097] Fig.13 A diagram of the process of hot-pouring carbon nanotube sponge with molten lithium. The carbon nanotube sponge is placed on top of the molten lithium, and the molten lithium starts to enter the carbon nanotube sponge from the bottom after 20 minutes. It takes about another 20 minutes for the molten lithium to finally fill the entire carbon nanotube sponge.

[0098] Fig.14 Comparison chart of lithium affinity tests of carbon nanotube sponge, carbon nanotube sponge preform, amorphous carbon coated stainless steel and original stainless steel. Fig.14 (a) is the lithium affinity test diagram of carbon nanotube sponge. Fig.14 (b) is the lithium affinity test diagram of the carbon nanotube sponge preform. Fig.14 (c) is the lithium affinity test diagram of amorphous carbon coated stainless steel. Fig.14 (d) is the lithium affinity test diagram of the original stainless steel. Fig.13 As shown, molten lithium was placed on the surfaces of carbon nanotube sponge, carbon nanotube sponge preform, amorphous carbon-coated stainless steel and original stainless steel, respectively. After 40 minutes, the molten lithium was injected into the carbon nanotube sponge; while the molten lithium could not be injected into the carbon nanotube sponge preform and remained in the state of spherical lithium beads with a contact angle of 113°, indicating that the carbon nanotube sponge preform had poor lithium affinity. The molten lithium on the stainless steel was also spherical lithium beads, and the contact angle of the molten lithium on the original stainless steel was 149°. After the original stainless steel was modified with amorphous carbon, the contact angle between the molten lithium and the stainless steel with amorphous carbon coating was 57°, indicating that amorphous carbon can improve the lithium affinity of lithium. In order to further understand the connection between lithium and amorphous carbon, the lithium metal anode was tested by XPS. Fig.14 This is the XPS spectrum of the lithium metal anode. Fig.15As shown in the figure, there is a Li-C peak at 55.45 eV, indicating that lithium and amorphous carbon react chemically at high temperature. During the preparation of lithium metal anode, molten lithium first reacts with amorphous carbon on the surface, and its reaction product has lithium affinity. Therefore, molten lithium is slowly injected into the carbon nanotube sponge and reacts with the internal amorphous carbon, and finally the molten lithium diffuses into the entire carbon nanotube sponge.

[0099] Example 2

[0100] The symmetric cell was assembled in a glove box (M. Braun Inert Gas Systems GmbH, Germany) under argon atmosphere. The working and counter electrodes of the symmetric cell were lithium metal anodes. 1M LiPF6 with 2 wt% VC in EC:DMC:DEC (volume ratio of 1:1:1:1) was used as the electrolyte.

[0101] Comparative Example 2

[0102] The symmetrical battery structure of Comparative Example 2 is substantially the same as that of Example 2, except that the working electrode and the counter electrode of the symmetrical battery are bare pure lithium metal sheets, hereinafter referred to as pure lithium metal electrodes.

[0103] Galvanostatic cycling measurements were performed in symmetric cells to evaluate the electrochemical performance of pure Li metal electrodes and Li metal anodes. Fig.16 The voltage-time curve of a symmetric battery using pure lithium metal electrodes. Fig.17 The voltage-time curve of a symmetric battery using a lithium metal anode. Fig.16 and Fig.17 In 1mAcm -2 A fixed current density of 1 mA cm -2 The cycling performance of a symmetric battery using a pure lithium metal electrode and a symmetric battery using a lithium metal anode were tested under deposition / stripping capacity conditions. Fig.18 The voltage-time curve of a symmetrical battery with a pure lithium metal electrode and a lithium metal anode at a cycle time of 78-80h. Figure 16-18 As shown in the figure, the voltage hysteresis of the symmetric cell using lithium metal anode is less than 0.2V and remains unchanged throughout the 500h cycle. The voltage hysteresis of the symmetric cell using pure lithium metal electrode gradually increases with the increase of cycle time, and the voltage hysteresis fluctuates irregularly after a cycle time of 90h, and a sudden voltage drop occurs at a cycle time of 250h. The voltage fluctuations in the symmetric cell using pure lithium metal electrode can be explained by the uneven deposition of lithium and unstable SEI, while the sudden drop can be attributed to the internal short circuit caused by Li dendrite penetration. From the above comparison, it can be seen that the lithium metal anode effectively reduces the voltage hysteresis of the symmetric cell and stabilizes the cycle performance of the symmetric cell. Fig.19The voltage-time curve of a symmetric battery using pure lithium metal electrodes. Fig. 20 The voltage-time curve of a symmetric battery using a lithium metal anode. Fig.18 and Fig. 20 In 2mAcm -2 A fixed current density of 1 mA cm -2 The cycling performance of a symmetric battery using a pure lithium metal electrode and a symmetric battery using a lithium metal anode were tested under the conditions of deposition / stripping capacity. Fig.18 and Fig.19 As shown, when the current density increases to 2 mA cm -2 When the lithium metal anode is used, it still effectively reduces the voltage hysteresis, stabilizes the cycle performance, and prolongs the battery life.

[0104] Fig.21 Nyquist plots of a symmetric battery using pure lithium metal electrode and a symmetric battery using lithium metal anode before cycling. Fig. 22 Nyquist plots of a symmetric battery using a pure lithium metal electrode and a symmetric battery using a lithium metal anode after cycling for 20 h. Fig.21 and Fig. 22 The deposition / stripping capacities are 1 mAh cm -2 Under the conditions of , electrochemical impedance spectroscopy (EIS) was performed on symmetric cells using pure lithium metal electrodes and symmetric cells using lithium metal anodes to analyze the difference in cycling performance. For symmetric cells, the semicircle in the high-frequency range is an indicator of the interfacial resistance at the SEI and the charge transfer resistance at the lithium surface. Before cycling, the symmetric cell using pure lithium metal electrodes and the symmetric cell using lithium metal anodes showed similar interfacial resistances, indicating that the interfaces were similar. After 10 cycles, the impedance of the symmetric cell using lithium metal anodes was smaller than that of the symmetric cell using pure lithium metal electrodes. The smaller impedance indicates that the lithium metal anode has better electrode stability and lithium deposition / stripping kinetics, which is consistent with the stable voltage-time curve in the symmetric cell with lithium metal anode.

[0105] Fig.23 This is the surface SEM image of a pure lithium metal electrode after a symmetric battery using a pure lithium metal electrode was cycled for 100 h. Fig.24 This is the surface SEM image of the lithium metal anode after the symmetric battery using the lithium metal anode was cycled for 100 h. Fig.25 This is a cross-sectional SEM image of the bare lithium metal electrode after a symmetric battery using a pure lithium metal electrode was cycled for 100 h. Fig.26 This is a cross-sectional SEM image of the lithium metal anode after a symmetric battery using a lithium metal anode was cycled for 100 h. Figure 23 to Figure 26 The deposition / stripping capacities are 1 mAh cm -2Under the conditions of , a symmetrical battery using pure lithium metal electrodes and a symmetrical battery using lithium metal anodes were cycled. Fig.24 As shown in Figure 2, the surface of pure lithium metal electrode is rough with random cracks and uneven lithium islands. Fig.24 As shown in Figure 1, the surface of the lithium metal anode is relatively flat with a few small pores. Fig.25 As shown in Figure 2, the volume change of the pure lithium metal electrode is large, and a 275 μm thick “bare lithium” layer is observed on top of the bare lithium metal electrode. Fig.26 As shown in the figure, the volume change of the lithium metal anode is small, and the "dead lithium" layer is thinner (118μm) and dense. The loose and unstable structure of the pure lithium metal electrode is attributed to the unstable SEI and lithium dendrites. The uneven lithium deposition / stripping of the pure lithium metal electrode will lead to lithium dendrites, which will penetrate into the unstable SEI, resulting in random cracks and surface unevenness. The electrolyte passes through the SEI from the cracks and reacts with fresh lithium to form a new SEI. However, the new SEI is also unstable, the electrolyte is consumed, the SEI is repeatedly formed and broken, and the long lithium dendrites fall off the pure lithium metal electrode, resulting in a thick layer of "failed lithium", loose structure and battery failure. The carbon nanotube sponge in the lithium metal anode acts as a matrix of the lithium metal anode, acting as a stable skeleton for the deposition / stripping of lithium, reducing the local current density along the surface of the lithium metal anode. Therefore, lithium can be deposited uniformly, the formation of lithium dendrites is suppressed, and the SEI is intact and stable.

[0106] Example 3

[0107] The lithium cobalt oxide electrode slurry was prepared by mixing lithium cobalt oxide, super-P acetylene black and poly(vinylidene fluoride) in a weight ratio of 8:1:1 in N-methylpyrrolidone (NMP), and then the uniform lithium cobalt oxide electrode slurry was pasted on an aluminum sheet to form a lithium cobalt oxide electrode. The lithium cobalt oxide electrode was used as the cathode, the lithium metal anode was used as the anode, and 1M LiPF6 with 2wt% VC in EC:DMC:DEC (volume ratio of 1:1:1:1) was used as the electrolyte to form a half-cell. In this embodiment, after the lithium cobalt oxide electrode was dried at 120°C for 24h, the lithium cobalt oxide electrode was cut into a circle with a diameter of 10mm and an area density of 10mg cm -2 The size of the lithium metal anode corresponds to the size of the lithium cobalt oxide electrode.

[0108] Comparative Example 3

[0109] The half-cell structure of Comparative Example 3 is substantially the same as that of Example 3, except that the anode of the half-cell is a bare pure lithium metal sheet, hereinafter referred to as a pure lithium anode.

[0110] The half-cells of Example 3 and Comparative Example 3 were respectively subjected to half-cell constant current cycle measurement by Land Battery System (Wuhan Electronics Co., Ltd., Wuhan, China), and the cut-off voltage was 3-4.3V. Fig. 27 Figure 2 is a graph showing the cycling performance of a half-cell containing a pure lithium anode and a half-cell containing a lithium metal anode. Fig.28 As shown, the half-cell containing pure lithium anode and the half-cell containing lithium metal anode were first cycled 3 times at 0.1C and then continued to cycle at 1C. When cycled 3 times at 0.1C, the specific capacity of the half-cell containing lithium metal anode was 152 mAh g -1 The specific capacity of the half-cell containing pure lithium anode is 145.1 mAh g -1 The half-cell with a lithium metal anode has a specific capacity of 71 mAh g after 200 cycles at 1C. -1 , with a Coulombic efficiency of 99.3%; the half-cell containing a pure lithium anode failed after 182 cycles. After the half-cell containing a pure lithium anode failed, the battery was disassembled, and the pure lithium anode was replaced with a new pure lithium anode, and a new half-cell was reassembled.

[0111] Fig.28 Figure 2 is a rate performance diagram of a half-cell containing a pure lithium anode and a half-cell containing a lithium metal anode. Fig.28 As shown, the specific capacities of the half-cell containing lithium metal anode at 0.1C, 0.2C, 0.5C, 1C, 2C and 5C are 165.4 mAh g -1 、152.1mAh g -1 , 144.3mAh g -1 , 137mAh g -1 , 126.9mAh g -1 and 108mAh g -1 In contrast, the half-cell with pure lithium anode has lower capacity values ​​at 0.1-5C. When the cycling rate drops again to 0.1C, the capacity of the half-cell with pure lithium anode is 152 mAh g -1 , while the capacity of the half-cell containing a lithium metal anode is 164 mAh g -1 It can be seen that the half-cell containing lithium metal anode has better half-cell constant current performance, demonstrating its potential in practical lithium metal batteries.

[0112] In addition, those skilled in the art may also make other changes within the spirit of the present invention. Of course, these changes made according to the spirit of the present invention should be included in the scope of protection required by the present invention.

Claims

1. A lithium metal anode, composed of a carbon nanotube sponge and a lithium metal material, wherein the carbon nanotube sponge is composed of a plurality of carbon nanotubes whose surfaces are covered with a carbon deposition layer and includes a plurality of micropores, wherein the plurality of micropores are formed by the plurality of carbon nanotubes whose surfaces are covered with a carbon deposition layer, the carbon nanotubes are pure carbon nanotubes, and the lithium metal material is filled in the plurality of micropores and covers the carbon nanotubes covered with the carbon deposition layer.

2. The lithium metal anode according to claim 1, characterized in that The lithium metal material covers the surface of the carbon deposition layer and fills the plurality of micropores.

3. The lithium metal anode according to claim 1, characterized in that The thickness of the carbon deposition layer is 2 nanometers to 100 nanometers.

4. The lithium metal anode according to claim 1, characterized in that In the lithium metal anode, the mass percentage of the carbon nanotubes is 6% to 10%, the mass percentage of the carbon deposition layer is 0.5% to 1%, and the mass percentage of the lithium metal material is 85% to 95%.

5. A method for preparing a lithium metal anode, comprising: preparing a carbon nanotube raw material, wherein the carbon nanotube raw material is directly scraped from a carbon nanotube array; The carbon nanotube raw material is added into an organic solvent and subjected to ultrasonic vibration to form a flocculent structure; washing the flocculent structure with water; The washed flocculent structure is freeze-dried under a vacuum environment to obtain a carbon nanotube sponge preform; Carrying out carbon deposition on the carbon nanotube sponge preform to form a carbon deposition layer, thereby obtaining the carbon nanotube sponge, wherein the carbon nanotube sponge is composed of a plurality of carbon nanotubes whose surfaces are covered by the carbon deposition layer, and the carbon nanotubes are pure carbon nanotubes; The molten lithium is placed in contact with the carbon nanotube sponge in an oxygen-free atmosphere, and the molten lithium is hot-injected into the carbon nanotube sponge and cooled to form a lithium metal anode.

6. The method for preparing a lithium metal anode according to claim 5, characterized in that: Lithium is heated to 200° C. to 300° C. to obtain liquid lithium, and argon gas is filled into a glove box to place the liquid lithium on the surface of the carbon nanotube sponge.

7. A lithium ion battery comprising: A shell and a lithium metal anode, a cathode, an electrolyte and a diaphragm placed in the shell, the electrolyte is placed in the shell, the lithium metal anode, the cathode and the diaphragm are placed in the electrolyte, the diaphragm is placed between the lithium metal anode and the cathode, and the internal space of the shell is divided into two parts. The lithium metal anode and the diaphragm, and the cathode and the diaphragm are kept apart, and the lithium metal anode adopts any one of the lithium metal anodes in claims 1-4.