Electromagnetic shielding film
Patent Information
- Application Number
- CN202210185841.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-06-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2039-06-28
AI Technical Summary
目前这类膜不具有防指纹性能,在多次使用后残留的指纹痕迹不但影响外观,同样会对膜材的性能产生一定的影响
[0011]本发明电磁屏蔽膜,其通过在水性聚氨酯、炭黑和1,1’,1"-次甲基三(4-异氰酸)苯中添加聚乙烯亚胺、十八烷基二甲基苄基氯化铵,使本发明的防指纹胶带具有防指纹性能,在各种环境下多次使用不会残留指纹痕迹,可以避免指纹汗液污渍对该胶带造成的腐蚀;同时,增强了本发明防指纹胶带的耐脏污性能,即胶带上的脏污在高温高湿环境下残留一段时间仍可以轻松擦去且不残留,既减少了污渍的附着,也大大降低了清洁难度。
Smart Images

Figure CN114828603B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adhesive tapes, and in particular relates to an electromagnetic shielding film. Background Art
[0002] Electromagnetic shielding film is a light-transmitting shielding material that can block electromagnetic wave penetration, prevent electromagnetic radiation, protect electronic components, and resist electromagnetic interference. In recent years, with the continuous development of electronic products, the requirements for electromagnetic shielding film have also been continuously improved. Wireless charging technology is mainly divided into three categories: magnetic induction wireless charging, magnetic resonance wireless charging, and wireless charging with radio frequency technology. With the popularization of wireless charging technology, many products using magnetic induction wireless charging technology have emerged on the market. In order to obtain higher charging efficiency and reduce or eliminate the impact of electromagnetic fields on mobile phones during charging, electromagnetic shielding film is needed for shielding. The function of electromagnetic shielding film is to isolate the impact of electromagnetic fields on mobile phones and prevent metals and other materials from absorbing electromagnetic waves emitted by the transmitting device and generating magnetic fields in the opposite direction. In the wireless charging receiving end of the mobile phone, if there is no electromagnetic shielding film, the wireless charging device cannot complete the close-range charging work. The electromagnetic shielding film needs to be fixed to the interference source with tape. At present, this type of film does not have anti-fingerprint performance. The fingerprint traces left after repeated use not only affect the appearance, but also have a certain impact on the performance of the film material. Summary of the invention
[0003] The present invention aims to provide an electromagnetic shielding film, which has anti-fingerprint performance and will not leave any fingerprint traces after repeated use in various environments, thereby preventing corrosion of the tape caused by fingerprint sweat stains.
[0004] To achieve the above object, the technical solution adopted by the present invention is: an electromagnetic shielding film, comprising a black ink layer, a substrate layer and an adhesive layer, wherein the black ink layer and the adhesive layer are respectively located on the upper surface and the lower surface of the substrate layer, and a release layer is provided on the side of the adhesive layer opposite to the substrate layer;
[0005] The black ink layer is obtained by drying the black ink, and the black ink consists of the following components in parts by weight: 60 parts of waterborne polyurethane, 1 part of carbon black, 1.5 parts of 1,1',1"-methylenetri(4-isocyanate)benzene, 1.5 parts of sodium silicate, 1.2 parts of carboxymethyl cellulose, 0.1 parts of sodium tripolyphosphate, 1 part of polyethyleneimine, 2 parts of octadecyldimethylbenzyl ammonium chloride, 2 parts of light absorber, 1 part of coupling agent, 0.8 parts of chitosan, and 18 parts of deionized water.
[0006] The technical solution further improved in the above technical solution is as follows:
[0007] 1. In the above scheme, the light absorber is selected from nano Al / Al2O3 core-shell materials.
[0008] 2. In the above scheme, the coupling agent is selected from coupling agent KH-580.
[0009] 3. In the above solution, the substrate layer is a PET polyester film with a thickness of 2~4μm.
[0010] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0011] The electromagnetic shielding film of the present invention is prepared by adding polyethyleneimine and octadecyldimethylbenzyl ammonium chloride to waterborne polyurethane, carbon black and 1,1',1"-methylenetri(4-isocyanate)benzene, so that the anti-fingerprint adhesive tape of the present invention has anti-fingerprint performance, and will not leave fingerprint traces after repeated use in various environments, thereby avoiding corrosion of the adhesive tape caused by fingerprint sweat stains; at the same time, the anti-fouling performance of the anti-fingerprint adhesive tape of the present invention is enhanced, that is, the dirt on the adhesive tape can be easily wiped off without residue even if it remains for a period of time in a high temperature and high humidity environment, thereby reducing the adhesion of stains and greatly reducing the difficulty of cleaning. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Attached Figure 1 It is a schematic diagram of the structure of the electromagnetic shielding film of the present invention.
[0013] In the above figures: 1, black ink layer; 2, substrate layer; 3, adhesive layer; 4, release layer. DETAILED DESCRIPTION
[0014] In the description of this patent, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention; the terms "first", "second", and "third" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance; in addition, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be a connection between the two elements. For those of ordinary skill in the art, the specific meanings of the above terms in this patent can be understood according to specific circumstances.
[0015] The present invention will be further described below in conjunction with embodiments:
[0016] Embodiment: An electromagnetic shielding film comprises a black ink layer 1, a substrate layer 2 and an adhesive layer 3, wherein the black ink layer 1 and the adhesive layer 3 are respectively located on the upper surface and the lower surface of the substrate layer 2, and a release layer 4 is provided on the side of the adhesive layer 3 opposite to the substrate layer 2;
[0017] The black ink layer 1 is obtained by drying the black ink, and the black ink is composed of the following components by weight: 60 parts of water-based polyurethane, 1 part of carbon black, 1.5 parts of 1,1',1"-methylenetri(4-isocyanate)benzene, 1.5 parts of sodium silicate, 1.2 parts of carboxymethyl cellulose, 0.1 parts of sodium tripolyphosphate, 1 part of polyethyleneimine, 2 parts of octadecyldimethylbenzyl ammonium chloride, 2 parts of light absorber, 1 part of coupling agent, 0.8 parts of chitosan, and 18 parts of deionized water.
[0018] The light absorber is selected from nano Al / Al2O3 core-shell material, and the coupling agent is selected from coupling agent KH-580.
[0019] The preparation method of the electromagnetic shielding film is as follows: 60-80 parts of waterborne polyurethane, 15-25 parts of deionized water, 1-5 parts of 1,1',1"-methylene tris(4-isocyanato)benzene, 0.01-0.03 parts of sodium tripolyphosphate, 1-5 parts of carbon black, 1-1.5 parts of sodium silicate, 1-5 parts of polyethyleneimine, 0.5-2 parts of octadecyl dimethyl benzyl ammonium chloride, 0.5-1.5 parts of coupling agent, 1-1.5 parts of carboxymethyl cellulose, 2-4 parts of light absorber, and 0.5-1 part of chitosan are added into a high-speed stirring dispersant, stirred, and mixed evenly to obtain a black ink;
[0020] The black ink is coated on the substrate layer 2 and dried to obtain an electromagnetic shielding film.
[0021] Comparative Examples 1-2: An electromagnetic shielding film, comprising a black ink layer 1, a substrate layer 2 and an adhesive layer 3, wherein the black ink layer 1 and the adhesive layer 3 are respectively located on the upper surface and the lower surface of the substrate layer 2, and a release layer 4 is provided on the side of the adhesive layer 3 opposite to the substrate layer 2;
[0022] The black ink layer 1 is obtained by drying black ink, and the black ink is composed of the following components in parts by weight, as shown in Table 2:
[0023] Components Comparative Example 1 Comparative Example 2 Waterborne polyurethane 60 servings 80 servings Carbon Black 1 serving 5 servings 1,1',1"-Methylenetri(4-isocyanato)benzene 1.8 servings 2 servings Sodium silicate 1.5 servings 1.2 servings Carboxymethyl cellulose 1.2 servings 1.5 servings Sodium tripolyphosphate 0.1 part 0.2 parts Polyethyleneimine - 5 servings Octadecyl dimethyl benzyl ammonium chloride 2 servings - Light absorber 2.5 servings 3 servings Coupling agent 0.8 parts 0.5 serving Chitosan 0.8 parts 0.6 parts Deionized water 18 servings 20 servings
[0024] The preparation method of the comparative example is the same as that of the embodiment.
[0025] In Comparative Example 1, the light absorber is selected from nano Al / Al2O3 core-shell material, the coupling agent is selected from coupling agent KH-580, the substrate layer 2 is a 2 μm thick PET layer, and the thickness of the black ink layer 1 is 1 μm.
[0026] In Comparative Example 2, the light absorber is selected from nano nickel powder, the coupling agent is selected from coupling agent KBM403, the substrate layer 2 is a 2.5 μm thick PET layer, and the thickness of the black ink layer 1 is 1.3 μm.
[0027] The properties of the electromagnetic shielding films obtained in the above examples and comparative examples 1-2 are shown in Table 2:
[0028] Table 2
[0029]
[0030] The test method is as follows:
[0031] Anti-fingerprint test: Press the black ink layer with your finger 10 times and observe the appearance of the black ink layer. The meanings of the relevant symbols in Table 2 are as follows:
[0032] ○: No fingerprints
[0033] ×: fingerprints are present;
[0034] Dirt resistance test: Use a ZEBRA oil pen at an angle of about 90° to the film surface, apply a force of about 1N to uniformly draw 5 10mm marks on the film surface, then place the sample in an environment with a temperature of 60℃ and a humidity of 95% for 2 hours. After taking it out, wipe the surface with alcohol. The sample is qualified if there is no trace left on the surface.
[0035] As shown in the evaluation results of Table 2, the electromagnetic shielding film of the embodiment has excellent anti-fingerprint performance, and no traces will be left even after multiple finger presses. The dirt on the tape can be easily wiped off without residue even after remaining for a period of time in a high temperature and high humidity environment, while the anti-fingerprint performance of comparative example 1 is relatively poor, and the dirt resistance of comparative example 2 is even worse. It can be seen that the present invention not only improves the anti-fingerprint performance, but also enhances the dirt resistance of the electromagnetic shielding film, that is, the dirt on the tape can be easily wiped off without residue even after remaining for a period of time in a high temperature and high humidity environment, which not only reduces the adhesion of stains, but also greatly reduces the difficulty of cleaning.
[0036] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. An electromagnetic shielding film, characterized in that: The invention comprises a black ink layer (1), a substrate layer (2) and an adhesive layer (3), wherein the black ink layer (1) and the adhesive layer (3) are respectively located on the upper surface and the lower surface of the substrate layer (2), and a release layer (4) is provided on the side of the adhesive layer (3) opposite to the substrate layer (2); The black ink layer (1) is obtained by drying black ink, wherein the black ink comprises the following components in parts by weight: 60 parts of waterborne polyurethane, 1 part of carbon black, 1.5 parts of 1,1',1"-methylenetri(4-isocyanato)benzene, 1.5 parts of sodium silicate, 1.2 parts of carboxymethyl cellulose, 0.1 parts of sodium tripolyphosphate, 1 part of polyethyleneimine, 2 parts of octadecyldimethylbenzyl ammonium chloride, 2 parts of light absorber, 1 part of coupling agent, 0.8 parts of chitosan, and 18 parts of deionized water.
2. The electromagnetic shielding film according to claim 1, characterized in that: The light absorber is selected from nano Al / Al2O3 core-shell materials.
3. The electromagnetic shielding film according to claim 1, characterized in that: The coupling agent is selected from coupling agent KH-580.
4. The electromagnetic shielding film according to any one of claims 1 to 3, characterized in that: The substrate layer (2) is a PET polyester film with a thickness of 2 to 4 μm.