Nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst and its preparation method and application
By forming a nickel-modified carbonized wood/sulfide heterojunction structure on carbonized wood, the problem of insufficient activity of carbonized wood-based electrocatalysts is solved, and the application of efficient urea oxidation current density and low-cost electrocatalysts is achieved.
Patent Information
- Application Number
- CN202210379690.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-12
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-04-12
AI Technical Summary
Existing carbonized wood-based electrocatalysts have problems such as low electrochemical active area, poor mass and electricity transfer capabilities, and low UOR catalytic activity in urea-assisted electrolysis of water for hydrogen production, which limits their application in low-cost, high-performance electrocatalysts.
Using a nickel-modified carbonized wood/sulfide heterojunction composite electrocatalyst, the NiS/Ni3S4 heterojunction is grown on the cell wall of the nickel-modified carbonized wood. The nickel-modified carbonized wood includes the cell wall of the carbonized wood inlaid with nickel metal. particles to improve conductivity and catalytic activity.
It achieves the effects of high electrochemical active area, good mass and electricity transfer capabilities, and excellent UOR catalytic activity. It can obtain higher urea oxidation current density at a lower potential, and is suitable for urea-assisted electrolysis of water for hydrogen production.
Smart Images

Figure CN114836784B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalyst preparation, and relates to a nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst, a preparation method and application thereof, and specifically relates to a metal nickel-modified carbonized wood-loaded sulfide heterojunction composite electrocatalyst, a preparation method thereof and application thereof in urea-assisted electrolysis for hydrogen production. Background Art
[0002] Hydrogen energy is regarded as the clean energy with the greatest development potential in the 21st century and is one of the main ways to achieve the goals of "carbon peak" and "carbon neutrality". Hydrogen production by water electrolysis includes hydrogen evolution reaction at the cathode and oxygen evolution reaction at the anode. The oxygen evolution reaction at the anode has seriously restricted the promotion and application of water electrolysis hydrogen production technology due to its high theoretical potential (1.23V vs. RHE). Using small molecules with low theoretical reaction potential to assist water electrolysis to produce hydrogen and reduce the energy consumption required for water electrolysis to produce hydrogen is one of the main directions of current research and development of water electrolysis hydrogen production technology. For example, urea-assisted water electrolysis to produce hydrogen has a low theoretical potential (0.67V vs. RHE) and can also achieve efficient degradation of urea-containing wastewater, making it more concerned among various small molecule-assisted electrolysis hydrogen production technologies. However, because there is multi-electron transfer in the urea oxidation reaction process and the reaction kinetics are slow, a suitable catalyst is needed to reduce the reaction energy barrier to avoid excessive energy consumption. Currently, catalysts based on precious metals such as Pt, Ru, and Ir are considered to be the most efficient urea oxidation catalysts, but their scarcity and high price on Earth hinder their large-scale commercial application. Therefore, the development of low-cost, high-performance electrocatalysts has gradually become a current research hotspot.
[0003] As an abundant renewable resource on earth, wood is widely used in traditional fields such as construction, furniture, and railways. However, the use of wood still has problems such as single product function and low added value. It is urgent to explore the use of wood in new functional materials and other fields with high added value. Wood has its unique cell wall structure and rich active groups such as hydroxyl groups, which can provide reaction sites for wood to anchor active components. At the same time, wood has an anisotropic multi-porous structure, which can provide a large specific surface area, making it have the potential to prepare low-cost, high-performance electrocatalysts. At present, some researchers have actively explored the application of wood in the field of electrocatalysts. However, most of the work is to directly carbonize wood and then load the corresponding active components. The carbonized wood-based electrocatalyst loaded with active components after direct carbonization still has poor conductivity due to the low carbonization temperature (most of which is below 1000℃), which needs to be further improved. Therefore, it is impossible to give full play to its structural advantages, which seriously limits the application and promotion of wood in the preparation of low-cost and high-performance electrocatalysts. In addition, the existing carbonized wood-based electrocatalysts obtained by directly loading active components on carbonized wood still have the defect of poor catalytic activity. For example, when nickel sulfide is directly loaded on carbonized wood by a solvothermal method, the obtained carbonized wood-based electrocatalyst still requires a higher potential to obtain a higher urea oxidation current density, which is not conducive to its wide application in the field of urea-assisted water electrolysis for hydrogen production. Therefore, obtaining a carbonized wood-based electrocatalyst with a high electrochemical active area, good mass and electricity transfer capabilities, and excellent UOR catalytic activity is of great significance for improving the performance of urea-assisted hydrogen production. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst with high electrochemical active area, good mass transfer and power transfer capacity, and excellent UOR catalytic activity, as well as a preparation method and application thereof.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions.
[0006] A nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst, the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst comprising nickel-modified carbonized wood, a sulfide heterojunction growing on the cell wall of the nickel-modified carbonized wood; the sulfide heterojunction is a NiS / Ni3S4 heterojunction; the nickel-modified carbonized wood comprises carbonized wood, a cell wall of the carbonized wood is inlaid with nickel metal particles.
[0007] The above-mentioned nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst is further improved, wherein the mass percentage of sulfide heterojunction in the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst is 57% to 67%; the mass percentage of nickel metal particles in the nickel-modified carbonized wood is 38% to 48%.
[0008] The above-mentioned nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst is further improved, wherein the NiS / Ni3S4 heterojunction is a nanorod with an average diameter of 50nm to 100nm and an average length of 1μm to 2μm; and the nickel metal particles are nanoparticles with an average diameter of 20nm to 100nm.
[0009] As a general technical concept, the present invention also provides a method for preparing a nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst, comprising the following steps:
[0010] S1, immersing wood chips into a nickel ion solution to obtain wood chips adsorbed with nickel ions;
[0011] S2, calcining the wood chips adsorbed with nickel ions obtained in step S1 to obtain nickel-modified carbonized wood;
[0012] S3, mixing the nickel-modified carbonized wood obtained in step S2 and the mixed solution of nickel nitrate / organic sulfur source to perform a hydrothermal reaction to obtain a nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst.
[0013] The above preparation method is further improved, in step S1, the mass volume ratio of the wood chip to the nickel ion solution is 0.002g~0.04g:1mL; the wood chip is obtained by cutting the wood along the horizontal growth direction; the thickness of the wood chip is 2mm~5mm; the wood chip is rectangular, square, triangle, parallelogram, trapezoid, ellipse or circular, and the length and width of the square are 1.5cm~2.5cm×0.7cm~1cm; the wood is one of poplar, masson pine, fir or a composite thereof The method comprises the following steps: the concentration of the nickel ion solution is 0.15 mol / L to 0.25 mol / L; the nickel ion solution is prepared by dissolving a nickel salt in water; the nickel salt is at least one of nickel nitrate, nickel acetate and nickel chloride; the impregnation is carried out under vacuum conditions; the impregnation is carried out at a temperature of 60°C to 80°C; the impregnation time is 8h to 10h; and after the impregnation is completed, the method further comprises: drying the impregnated wood under vacuum conditions, the drying temperature is 60°C to 80°C, and the drying time is 8h to 12h.
[0014] The above preparation method is further improved, in step S2, the calcination is carried out under a protective gas atmosphere; the protective gas is nitrogen or argon; the calcination is first heated to 500°C for 1h to 2h, and then heated to 700°C to 900°C for 1h to 2h; the heating rate during the calcination process is 2°C / min to 5°C / min.
[0015] The above preparation method is further improved, in step S3, after the calcination is completed, the following treatment is also included: using 1500-2000 mesh sandpaper to grind the calcined product, using deionized water to wash the grinded calcined product, placing the washed calcined product in ethanol for ultrasonic treatment, and drying the calcined product after ultrasonic treatment under vacuum conditions; the number of grinding times is 5 to 8 times; the number of washing times is 2 to 3 times; the time of ultrasonic treatment is 3 min to 5 min; the drying temperature is 60° C. to 80° C., and the drying time is 8 h to 12 h.
[0016] The above preparation method is further improved, in step S3, the mass volume ratio of the nickel-modified carbonized wood to the mixed solution of nickel nitrate / organic sulfur source is 0.0004g~0.013g:1mL; in the mixed solution of nickel nitrate / organic sulfur source, the concentration of nickel nitrate is 0.17mol / L~0.37mol / L, and the concentration of the organic sulfur source is 0.77mol / L~0.97mol / L; the mixed solution of nickel nitrate / organic sulfur source is prepared by dissolving nickel nitrate and an organic sulfur source in water; the organic sulfur source is at least one of thiourea, thioacetamide, and ethanol sulfur; the hydrothermal reaction is carried out at a temperature of 120°C~180°C; and the hydrothermal reaction time is 12h~24h.
[0017] The above-mentioned preparation method is further improved, in step S3, the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst includes nickel-modified carbonized wood, and a sulfide heterojunction grows on the cell wall of the nickel-modified carbonized wood; the sulfide heterojunction is a NiS / Ni3S4 heterojunction; the nickel-modified carbonized wood includes carbonized wood, and the cell wall of the carbonized wood is inlaid with nickel metal particles; the mass percentage of the sulfide heterojunction in the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst is 57% to 67%; the mass percentage of the nickel metal particles in the nickel-modified carbonized wood is 38% to 48%; the NiS / Ni3S4 heterojunction is a nanorod with an average diameter of 50nm to 100nm and an average length of 1μm to 2μm; the nickel metal particles are nanoparticles with an average diameter of 20nm to 100nm.
[0018] As a general technical concept, the present invention also provides an application of the above-mentioned nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst or the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst prepared by the above-mentioned preparation method in hydrogen production by water electrolysis.
[0019] Compared with the prior art, the advantages of the present invention are:
[0020] (1) In view of the shortcomings of existing carbonized wood-based electrocatalysts loaded with nickel sulfide, such as low electrochemical active area, poor mass and electricity transfer capacity, and low UOR catalytic activity, the present invention creatively proposes a nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst, including nickel-modified carbonized wood, a sulfide heterojunction grown on the cell wall of the nickel-modified carbonized wood, and the sulfide heterojunction is a NiS / Ni3S4 heterojunction, wherein the nickel-modified carbonized wood includes carbonized wood, and the cell wall of the carbonized wood is inlaid with nickel metal particles. In the present invention, nickel-modified carbonized wood is used as a matrix, and the carbonized wood is modified by metal nickel so that the modified carbonized wood has a higher degree of graphitization. At the same time, the metal nickel is evenly embedded in the carbonized wood skeleton, which can give the carbonized wood better conductivity. The invention is a novel electrocatalyst carrier with excellent performance. On this basis, by growing the NiS / Ni3S4 heterojunction on the cell wall of the nickel-modified carbonized wood, the nickel-modified carbonized wood can effectively anchor the sulfide heterojunction on the cell wall of the pore, which can improve the conductivity of the composite electrocatalyst and promote the rapid transfer of charges. At the same time, the NiS / Ni3S4 heterojunction structure can effectively regulate the surface electronic structure of the sulfide, so that the intermediate species of the surface urea oxidation reaction have suitable adsorption and desorption energy on its surface, thereby facilitating the improvement of the catalytic activity of the composite electrocatalyst. The nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst of the present invention has the advantages of high electrochemical active area, good mass and electricity transfer capacity, excellent UOR catalytic activity, etc. It is a new type of electrocatalyst with excellent performance and can be widely used in water electrolysis to produce hydrogen. In particular, when used for urea-assisted water electrolysis to produce hydrogen, it can obtain a higher urea oxidation current density at a lower potential, which is conducive to its wide application in the field of urea-assisted water electrolysis to produce hydrogen, has high use value, and has good application prospects.
[0021] (2) In the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst of the present invention, the mass percentage of the sulfide heterojunction is 57% to 67%. Within this range, the sulfide heterojunction will be evenly and firmly embedded in the nickel-modified carbonized wood skeleton, thereby being able to obtain a more stable and better catalytic activity. This is because the nickel-modified carbonized wood has an anisotropic multi-porous structure. Due to the limitations of the wood pores and pore structure, when excessive sulfide heterojunctions are produced, they will be disorderly accumulated on the surface and inside of the carbonized wood, and a small amount of sulfide heterojunctions will be scattered and sparsely distributed on the carbonized wood skeleton, resulting in uneven distribution. Both will reduce the exposed active sites of the composite electrocatalyst, which is not conducive to the expression of the activity of the composite electrocatalyst. In the present invention, the mass percentage of nickel metal particles in the nickel-modified carbonized wood is 38% to 48%. Within this range, nickel metal particles with smaller particle sizes can be more evenly and firmly loaded on the carbonized wood skeleton, which is not only more conducive to the formation of sulfide heterojunctions, but also more conducive to the sulfide heterojunctions being evenly and firmly embedded in the nickel-modified carbonized wood skeleton. This is because when the mass ratio of nickel metal particles is too high, agglomeration will occur on the surface and inside of the wood, resulting in uneven distribution of nickel metal particles and larger particle sizes of generated particles, while when the mass ratio is too low, it is not conducive to the formation of sulfide heterojunctions.
[0022] (3) The present invention also provides a method for preparing a nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst, which introduces a heterojunction structure into carbonized wood for the first time. Specifically, the wood chips are first immersed in a nickel ion solution so that the nickel ions are adsorbed into the skeleton material of the wood chips, and then the wood chips adsorbed with nickel ions are calcined. During the calcination process, the wood chips are converted into carbonized wood and the nickel ions are reduced to nickel metal particles and embedded in the cell walls of the carbonized wood. In addition, due to the presence of metallic nickel during the calcination process, the catalytic effect thereof is enhanced. , which can further improve the graphitization degree of carbonized wood. Finally, the nickel-modified carbonized wood obtained after calcination is used as a carrier to grow sulfide through a hydrothermal reaction, and a nickel-based sulfide heterojunction (NiS / Ni3S4 heterojunction) composed of high-valent nickel is obtained. At the same time, the NiS / Ni3S4 heterojunction grows in situ on the cell wall of the nickel-modified carbonized wood, thereby preparing a nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst with high electrochemical active area, good mass and power transfer capabilities, and excellent UOR catalytic activity.
[0023] (4) In the preparation method of the present invention, by optimizing the mass volume ratio of the mixed solution of nickel-modified carbonized wood and nickel nitrate / organic sulfur source to 0.0004g-0.013g:1mL, the content of sulfide heterojunction can be regulated, and the sulfide heterojunction can be uniformly and orderly loaded on the nickel-modified carbonized wood skeleton. In the present invention, the mixed solution of nickel nitrate / organic sulfur source used is prepared by dissolving nickel nitrate and organic sulfur source in water. If other nickel salts are used, the electrocatalyst of the present invention cannot be prepared; in the present invention, by optimizing the mass volume ratio of wood chips and nickel ion solution to 0.002g-0.04g:1mL, the content and particle size of nickel metal particles in nickel-modified carbonized wood can be regulated, and the nickel metal particles with smaller particles can be promoted to be uniformly loaded on the carbonized wood skeleton, so that the graphitization degree and conductivity of nickel-modified carbonized wood can be regulated.
[0024] (5) In the preparation method of the present invention, wood is used as raw material, which has the advantages of being renewable, cheap and easily available, and environmentally friendly, and is therefore beneficial for reducing the preparation cost of the electrocatalyst while expanding the high value-added utilization of wood. At the same time, wood also has the advantages of high mechanical strength and a three-dimensional porous structure, and thus the electrocatalyst prepared thereby has a three-dimensional porous structure and excellent electrical conductivity, which can give the electrocatalyst a higher electrochemical active area and better mass and electricity transfer capabilities, reflecting excellent urea-assisted hydrogen performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0026] Figure 1 This is a SEM image of the nickel-modified carbonized wood prepared in Example 1 of the present invention.
[0027] Figure 2 This is a SEM image of the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst prepared in Example 1 of the present invention.
[0028] Figure 3 This is the SEM image of the carbonized wood-based composite electrocatalyst loaded with nickel sulfide prepared in Comparative Example 1.
[0029] Figure 4 XRD patterns of the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst (NiS / Ni3S4 / CW) and nickel-modified carbonized wood (Ni / CW) prepared in Example 1 of the present invention, the nickel sulfide-loaded carbonized wood-based composite electrocatalyst (NiS2 / Ni3S4 / CW) and unmodified carbonized wood (CW) prepared in Comparative Example 1.
[0030] Figure 5The linear sweep voltammograms corresponding to the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst (NiS / Ni3S4 / CW) prepared in Example 1 of the present invention, the nickel-modified carbonized wood (Ni / CW), the nickel sulfide-loaded carbonized wood-based composite electrocatalyst (NiS2 / Ni3S4 / CW) prepared in Comparative Example 1, and the unmodified carbonized wood (CW) in urea-loaded water electrolysis to produce hydrogen. DETAILED DESCRIPTION
[0031] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby. The materials and instruments used in the following embodiments are all commercially available.
[0032] Example 1
[0033] A nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst comprises nickel-modified carbonized wood, on the cell wall of which a sulfide heterojunction grows, the sulfide heterojunction is a NiS / Ni3S4 heterojunction, wherein the nickel-modified carbonized wood comprises carbonized wood, on the cell wall of which nickel metal particles are inlaid.
[0034] In this embodiment, the mass percentage of the sulfide heterojunction in the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst is 62.5%, and the mass percentage of the nickel metal particles in the nickel-modified carbonized wood is 40%.
[0035] In this embodiment, the NiS / Ni3S4 heterojunction is a nanorod with an average diameter of 80 nm and an average length of 1.7 μm; the nickel metal particles are nanoparticles with an average diameter of 46 nm.
[0036] The method for preparing the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst of the embodiment of the present invention comprises the following steps:
[0037] (1) Select poplar wood with a natural porous structure, cut large pieces of poplar wood along the horizontal growth direction to make the size (square) of 2.5 cm × 1 cm × 3 mm (length × width × height), and immerse the obtained wood chips in a 0.2 mol / L nickel nitrate aqueous solution (including 2 wood chips, the masses of which are 0.1486 g and 0.1511 g, respectively, and the amount of nickel nitrate aqueous solution is 15 mL), and place them in a vacuum drying oven for immersion at a temperature of 80°C for 8 h. After completion, take them out for cleaning, and then place them in a 60°C vacuum drying oven for drying for 12 h to obtain wood chips adsorbed with nickel ions.
[0038] (2) The wood chips adsorbed with nickel ions obtained in step (1) are placed in a tubular furnace, and under the protection of a nitrogen atmosphere, the temperature is increased from room temperature to 500°C at a heating rate of 2°C / min, and the temperature is kept for 1 hour, and then the temperature is increased to 800°C at a heating rate of 2°C / min, and the temperature is kept for 2 hours, and the wood chips are naturally cooled to room temperature to obtain carbonized wood chips. The carbonized wood chips are polished with 2000 mesh silicon carbide sandpaper, and the front and back sides are evenly polished 5 times, washed with deionized water 3 times and ultrasonically cleaned in ethanol for 3 minutes, and then taken out and placed in a 60°C vacuum drying oven for 12 hours to obtain nickel-modified carbonized wood, which is recorded as Ni / CW.
[0039] (3) The nickel-modified carbonized wood obtained in step (2) is added to a mixed aqueous solution of nickel nitrate and thiourea (the concentration of nickel nitrate in the solution is 0.27 mol / L, the concentration of thiourea is 0.87 mol / L, wherein there are two pieces of nickel-modified carbonized wood, the masses of which are 0.0241 g and 0.0253 g, respectively, and the amount of the mixed aqueous solution of nickel nitrate and thiourea is 15 mL), mixed evenly, and then transferred into a reactor for hydrothermal reaction at a hydrothermal temperature of 120° C. for 12 h. After completion, the reaction mixture is taken out and ultrasonically cleaned in deionized water for 2 min, and then dried in a vacuum drying oven at 60° C. for 12 h to obtain a nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst, denoted as NiS / Ni3S4 / CW.
[0040] An application of the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst prepared in the above-mentioned embodiment in hydrogen production by water electrolysis, specifically in urea-assisted water electrolysis to produce hydrogen, comprising the following steps: directly using the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst as a working electrode, placing it in a 1.0 mol / L KOH+0.5 mol / L CO(NH2)2 electrolyte for electrolysis reaction to obtain hydrogen.
[0041] Comparative Example 1
[0042] A method for preparing a carbonized wood-based composite electrocatalyst loaded with nickel sulfide comprises the following steps:
[0043] (1) Select poplar wood with natural porous structure, cut large pieces of poplar wood along the horizontal growth direction to make the size of 2.5cm×1cm×3mm (length×width×height), place the obtained wood chips (2 pieces, with masses of 0.1523g and 0.1564g respectively) in a tube furnace, and under the protection of nitrogen atmosphere, heat from room temperature to 500℃ at a heating rate of 2℃ / min, keep warm for 1h, then heat to 800℃ at a heating rate of 2℃ / min, keep warm for 2h, and naturally cool to room temperature to obtain carbonized wood chips. The carbonized wood chips were polished with 2000 mesh silicon carbide sandpaper, and the front and back sides were evenly polished 5 times, washed with deionized water 3 times and ultrasonically cleaned in ethanol for 3min, taken out and dried in a 60℃ vacuum drying oven for 12h to obtain unmodified carbonized wood, recorded as CW.
[0044] (2) The unmodified carbonized wood obtained in step (1) is added to a mixed aqueous solution of nickel nitrate and thiourea (the concentration of nickel nitrate in the solution is 0.27 mol / L, the concentration of thiourea is 0.87 mol / L, wherein there are two pieces of unmodified carbonized wood, the masses of which are 0.0252 g and 0.0271 g, respectively, and the amount of the mixed aqueous solution of nickel nitrate and thiourea is 15 mL), mixed evenly, and then transferred into a reactor for hydrothermal reaction at a hydrothermal temperature of 120° C. for 12 h. After completion, the carbonized wood is taken out and ultrasonically cleaned in deionized water for 2 min, and then dried in a vacuum drying oven at 60° C. for 12 h to obtain a carbonized wood-based composite electrocatalyst loaded with nickel sulfide, which is recorded as NiS2 / Ni3S4 / CW.
[0045] Comparative Example 2
[0046] A method for preparing a cobalt-modified carbonized wood / sulfide composite electrocatalyst comprises the following steps:
[0047] (1) Select poplar wood with a natural porous structure, cut large pieces of poplar wood along the horizontal growth direction to make the size (square) of 2.5 cm × 1 cm × 3 mm (length × width × height), and immerse the obtained wood chips in a 0.2 mol / L cobalt nitrate aqueous solution (including 2 wood chips, the masses of which are 0.1556 g and 0.1575 g, respectively, and the amount of cobalt nitrate aqueous solution is 15 mL), and place them in a vacuum drying oven for immersion at a temperature of 80°C for 8 h. After completion, take them out for cleaning, and then place them in a vacuum drying oven at 60°C for drying for 12 h to obtain wood chips adsorbed with cobalt ions.
[0048] (2) The wood chips adsorbed with cobalt ions obtained in step (1) are placed in a tubular furnace, and under the protection of a nitrogen atmosphere, the temperature is increased from room temperature to 500°C at a heating rate of 2°C / min, and the temperature is kept for 1 hour, and then the temperature is increased to 800°C at a heating rate of 2°C / min, and the temperature is kept for 2 hours, and the wood chips are naturally cooled to room temperature to obtain carbonized wood chips. The carbonized wood chips are polished with 2000 mesh silicon carbide sandpaper, and the front and back sides are evenly polished 5 times, washed with deionized water 3 times and ultrasonically cleaned in ethanol for 3 minutes, and then taken out and placed in a 60°C vacuum drying oven for 12 hours to obtain cobalt-modified carbonized wood.
[0049] (3) The cobalt-modified carbonized wood obtained in step (2) is added to a mixed aqueous solution of cobalt nitrate and thiourea (the concentration of cobalt nitrate in the solution is 0.27 mol / L, the concentration of thiourea is 0.87 mol / L, wherein there are two pieces of cobalt-modified carbonized wood, the masses of which are 0.0264 g and 0.0283 g, respectively, and the amount of the mixed aqueous solution of cobalt nitrate and thiourea is 15 mL), mixed evenly, and then transferred into a reactor for hydrothermal reaction at a hydrothermal temperature of 120° C. for 12 h. After completion, the mixture is taken out and ultrasonically cleaned in deionized water for 2 min, and then dried in a vacuum drying oven at 60° C. for 12 h to obtain a cobalt-modified carbonized wood / sulfide composite electrocatalyst, denoted as CoS2 / CW.
[0050] The test results show that the composite electrocatalyst prepared in Comparative Example 2 is composed of a single composite of cobalt disulfide and carbonized wood, and cannot form a heterojunction composite electrocatalyst as in Example 1.
[0051] Figure 1 : is a SEM image of the nickel-modified carbonized wood prepared in Example 1 of the present invention. Figure 1 It can be seen that after the natural wood chips adsorbed with nickel ions are subjected to high-temperature carbonization treatment, nickel metal particles are evenly embedded in the cell walls of carbonized poplar wood to form metal nickel-modified carbonized wood.
[0052] Figure 2 : is a SEM image of the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst prepared in Example 1 of the present invention. Figure 2 It can be seen that in the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst (NiS / Ni3S4 / CW), nickel-based sulfide heterojunction nanorods grow uniformly on the nickel-modified carbonized wood cell wall, where the average diameter of the nanorods is 80 nm and the average length is 1.70 μm.
[0053] Figure 3 : is a SEM image of the carbonized wood-based composite electrocatalyst loaded with nickel sulfide prepared in Comparative Example 1. Figure 3It can be seen that in the carbonized wood-based composite electrocatalyst (NiS2 / Ni3S4 / CW) loaded with nickel sulfide, sulfide is grown on the unmodified carbonized wood by the solvothermal method. The generated sulfide is mainly cubic in structure and unevenly distributed, which reduces the number of active sites exposed on the surface of the composite catalyst.
[0054] Figure 4 The XRD patterns of the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst (NiS / Ni3S4 / CW) and the nickel-modified carbonized wood (Ni / CW) prepared in Example 1 of the present invention, and the carbonized wood-based composite electrocatalyst loaded with nickel sulfide (NiS2 / Ni3S4 / CW) and the unmodified carbonized wood (CW) prepared in Comparative Example 1. Figure 4 From the XRD spectrum, it can be seen that the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst (NiS / Ni3S4 / CW) prepared by the present invention has an obvious sulfide diffraction peak, and the nickel-modified carbonized wood has a sharper carbon diffraction peak than the unmodified carbonized wood, indicating that the modified carbonized wood has a higher degree of graphitization and can give the carbonized wood better conductivity. In addition, according to Figure 4 It can be seen that NiS2 / Ni3S4 / CW, because its carbonized wood has not been modified, causes its carbonized wood carrier to be amorphous (which can be proved by its XRD spectrum, which shows a broad diffraction peak at about 22°, indicating that the carbonized wood is mainly amorphous), which is not conducive to improving the conductive performance, making its conductive performance general, and is not conducive to the expression of the catalytic performance of the composite electrocatalyst.
[0055] The nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst (NiS / Ni3S4 / CW) prepared in Example 1 of the present invention, the nickel-modified carbonized wood (Ni / CW) and the nickel-sulfide-loaded carbonized wood-based composite electrocatalyst (NiS2 / Ni3S4 / CW) prepared in Comparative Example 1, and the unmodified carbonized wood (CW) were subjected to linear sweep voltammetry tests in 1.0 mol / L KOH+0.5 mol / L CO(NH2)2 electrolyte. The results are as follows: Figure 5 shown.
[0056] Figure 5 The linear sweep voltammograms of the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst (NiS / Ni3S4 / CW) prepared in Example 1 of the present invention, the nickel-modified carbonized wood (Ni / CW), the nickel-sulfide-loaded carbonized wood-based composite electrocatalyst (NiS2 / Ni3S4 / CW) prepared in Comparative Example 1, and the unmodified carbonized wood (CW) in urea-assisted water electrolysis for hydrogen production are shown in FIG. Figure 5It can be seen that compared with the carbonized wood-based composite electrocatalyst loaded with nickel sulfide (NiS2 / Ni3S4 / CW), the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst (NiS / Ni3S4 / CW) prepared in the present invention exhibits better UOR catalytic activity, requiring only 1.36 V (vs. RHE) to obtain 50 mA / cm 2 The urea oxidation current density is significantly lower than that of the carbonized wood-based composite electrocatalyst (NiS2 / Ni3S4 / CW) loaded with nickel sulfide (1.43 V).
[0057] Example 2
[0058] A nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst comprises nickel-modified carbonized wood, on the cell wall of which a sulfide heterojunction grows, the sulfide heterojunction is a NiS / Ni3S4 heterojunction, wherein the nickel-modified carbonized wood comprises carbonized wood, on the cell wall of which nickel metal particles are inlaid.
[0059] In this embodiment, the mass percentage of the sulfide heterojunction in the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst is 65%, and the mass percentage of the nickel metal particles in the nickel-modified carbonized wood is 44%.
[0060] In this embodiment, the NiS / Ni3S4 heterojunction is a nanorod with an average diameter of 70 nm and an average length of 1.6 μm; the nickel metal particles are nanoparticles with an average diameter of 54 nm.
[0061] The method for preparing the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst of the embodiment of the present invention comprises the following steps:
[0062] (1) Select poplar wood with a natural porous structure, cut large pieces of poplar wood along the horizontal growth direction to a size of 2.5 cm × 1 cm × 5 mm (length × width × height), and immerse the obtained wood chips in a 0.25 mol / L nickel nitrate aqueous solution (including 2 wood chips, the masses of which are 0.2477 g and 0.2518 g, respectively, and the amount of nickel nitrate aqueous solution is 15 mL), and place them in a vacuum drying oven for immersion at a temperature of 80°C for 10 h. After completion, take them out for cleaning, and then place them in a 60°C vacuum drying oven for drying for 12 h to obtain wood chips adsorbed with nickel ions.
[0063] (2) The wood chips adsorbed with nickel ions obtained in step (1) are placed in a tubular furnace, and under the protection of a nitrogen atmosphere, the temperature is increased from room temperature to 500°C at a heating rate of 2°C / min, and the temperature is kept for 1 hour, and then the temperature is increased to 900°C at a heating rate of 2°C / min, and the temperature is kept for 2 hours, and the wood chips are naturally cooled to room temperature to obtain carbonized wood chips. The carbonized wood chips are polished with 1500 mesh silicon carbide sandpaper, and the front and back sides are evenly polished 5 times, washed with deionized water 3 times and ultrasonically cleaned in ethanol for 3 minutes, and then taken out and placed in a 60°C vacuum drying oven for 12 hours to obtain nickel-modified carbonized wood.
[0064] (3) adding the nickel-modified carbonized wood obtained in step (2) to a mixed aqueous solution of nickel nitrate and thiourea (the concentration of nickel nitrate in the solution is 0.17 mol / L, the concentration of thiourea is 0.77 mol / L, wherein there are two pieces of nickel-modified carbonized wood, the masses of which are 0.0401 g and 0.0421 g, respectively, and the amount of the mixed aqueous solution of nickel nitrate and thiourea is 15 mL), mixing them evenly, and then transferring them into a reactor for hydrothermal reaction at a hydrothermal temperature of 180° C. for 24 h. After completion, taking them out and placing them in deionized water for ultrasonic cleaning for 2 min, placing them in a vacuum drying oven at 60° C. for 12 h, and obtaining a nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst.
[0065] An application of the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst prepared in the above-mentioned embodiment in hydrogen production by water electrolysis, specifically in urea-assisted water electrolysis to produce hydrogen, comprising the following steps: directly using the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst as a working electrode, placing it in a 1.0 mol / L KOH+0.5 mol / L CO(NH2)2 electrolyte for electrolysis reaction to obtain hydrogen.
[0066] The linear sweep voltammetry test results show that the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst prepared in Example 2 of the present invention has a conductivity of 50 mA / cm 2 The potential at 1.37 V (vs. RHE) shows excellent UOR catalytic activity.
[0067] Example 3
[0068] A nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst comprises nickel-modified carbonized wood, on the cell wall of which a sulfide heterojunction grows, the sulfide heterojunction is a NiS / Ni3S4 heterojunction, wherein the nickel-modified carbonized wood comprises carbonized wood, on the cell wall of which nickel metal particles are inlaid.
[0069] In this embodiment, the mass percentage of the sulfide heterojunction in the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst is 58%, and the mass percentage of the nickel metal particles in the nickel-modified carbonized wood is 38%.
[0070] In this embodiment, the NiS / Ni3S4 heterojunction is a nanorod with an average diameter of 80 nm and an average length of 1.8 μm; the nickel metal particles are nanoparticles with an average diameter of 41 nm.
[0071] The method for preparing the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst of the embodiment of the present invention comprises the following steps:
[0072] (1) Select poplar wood with a natural porous structure, cut large pieces of poplar wood along the horizontal growth direction to a size of 1.5 cm × 0.7 cm × 2 mm (length × width × height), and immerse the obtained wood chips in a 0.15 mol / L nickel nitrate aqueous solution (including 2 wood chips, the masses of which were 0.0416 g and 0.0422 g, respectively, and the amount of nickel nitrate aqueous solution was 15 mL), and place them in a vacuum drying oven for immersion at a temperature of 80°C for 8 h. After completion, take them out for cleaning, and then place them in a 60°C vacuum drying oven for drying for 12 h to obtain wood chips adsorbed with nickel ions.
[0073] (2) The wood chips adsorbed with nickel ions obtained in step (1) are placed in a tubular furnace, and under the protection of a nitrogen atmosphere, the temperature is increased from room temperature to 500°C at a heating rate of 5°C / min, and the temperature is kept for 1 hour, and then the temperature is increased to 700°C at a heating rate of 5°C / min, and the temperature is kept for 2 hours, and the wood chips are naturally cooled to room temperature to obtain carbonized wood chips. The carbonized wood chips are polished with 2000 mesh silicon carbide sandpaper, and the front and back sides are evenly polished 5 times, washed with deionized water 3 times and ultrasonically cleaned in ethanol for 3 minutes, and then taken out and placed in a 60°C vacuum drying oven for 12 hours to obtain nickel-modified carbonized wood.
[0074] (3) The nickel-modified carbonized wood obtained in step (2) is added to a mixed aqueous solution of nickel nitrate and thiourea (the concentration of nickel nitrate in the solution is 0.37 mol / L, the concentration of thiourea is 0.97 mol / L, wherein there are two pieces of nickel-modified carbonized wood, the masses of which are 0.0068 g and 0.0072 g, respectively, and the amount of the mixed aqueous solution of nickel nitrate and thiourea is 15 mL), mixed evenly, and then transferred into a reactor for hydrothermal reaction at a hydrothermal temperature of 160° C. for 12 h. After completion, the reaction mixture is taken out and ultrasonically cleaned in deionized water for 2 min, and then dried in a vacuum drying oven at 60° C. for 12 h to obtain a nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst.
[0075] An application of the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst prepared in the above-mentioned embodiment in hydrogen production by water electrolysis, specifically in urea-assisted water electrolysis to produce hydrogen, comprising the following steps: directly using the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst as a working electrode, placing it in a 1.0 mol / L KOH+0.5 mol / L CO(NH2)2 electrolyte for electrolysis reaction to obtain hydrogen.
[0076] The linear sweep voltammetry test results show that the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst prepared in Example 3 of the present invention has a conductivity of 50 mA / cm 2 The potential at 1.40 V (vs. RHE) shows excellent UOR catalytic activity.
[0077] Based on the above results, it can be seen that in the present invention, nickel-modified carbonized wood is used as a matrix, and the carbonized wood is modified by metal nickel, so that the modified carbonized wood has a higher degree of graphitization, and the metal nickel is evenly embedded in the carbonized wood skeleton, which can give the carbonized wood better conductivity. It is a new type of electrocatalyst carrier with excellent performance. On this basis, by growing the NiS / Ni3S4 heterojunction on the cell wall of nickel-modified carbonized wood, the nickel-modified carbonized wood can effectively anchor the sulfide heterojunction on the cell wall of the pore, which can improve the conductivity of the composite electrocatalyst and promote the rapid transfer of charge. At the same time, the NiS / Ni3S4 heterojunction structure can effectively regulate the surface electronic structure of the sulfide, so that the intermediate species of the surface urea oxidation reaction have suitable adsorption and desorption energy on its surface, which is beneficial to improve the catalytic activity of the composite electrocatalyst. The nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst of the present invention has the advantages of high electrochemical active area, good mass and electricity transfer capacity, excellent UOR catalytic activity, etc. It is a new type of electrocatalyst with excellent performance and can be widely used in water electrolysis to produce hydrogen. In particular, when used for urea-assisted water electrolysis to produce hydrogen, it can obtain a higher urea oxidation current density at a lower potential, which is conducive to its wide application in the field of urea-assisted water electrolysis to produce hydrogen, has high use value, and has good application prospects.
[0078] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as above in the preferred embodiment, it is not used to limit the present invention. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent replacement, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention, still fall within the scope of protection of the technical solution of the present invention.
Claims
1. A nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst, characterized in that: The nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst includes nickel-modified carbonized wood, on the cell wall of which a sulfide heterojunction grows; the sulfide heterojunction is a NiS / Ni3S4 heterojunction; the nickel-modified carbonized wood includes carbonized wood, on the cell wall of which nickel metal particles are embedded; the mass percentage of the sulfide heterojunction in the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst is 57% to 67%; the mass percentage of the nickel metal particles in the nickel-modified carbonized wood is 38% to 48%.
2. The nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst according to claim 1, characterized in that: The NiS / Ni3S4 heterojunction is a nanorod with an average diameter of 50nm-100nm and an average length of 1μm-2μm; the nickel metal particles are nanoparticles with an average diameter of 20nm-100nm.
3. A method for preparing a nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst, characterized in that: The following steps are involved: S1, immersing wood chips in a nickel ion solution to obtain wood chips adsorbed with nickel ions; the mass volume ratio of the wood chips to the nickel ion solution is 0.002 g to 0.04 g: 1 mL; S2, calcining the wood chips adsorbed with nickel ions obtained in step S1 to obtain nickel-modified carbonized wood; S3, mixing the nickel-modified carbonized wood and the mixed solution of nickel nitrate / organic sulfur source obtained in step S2 for hydrothermal reaction to obtain a nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst; the mass volume ratio of the nickel-modified carbonized wood and the mixed solution of nickel nitrate / organic sulfur source is 0.0004g-0.013g:1mL; the mixed solution of nickel nitrate / organic sulfur source is prepared by dissolving nickel nitrate and an organic sulfur source in water; the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst The catalyst includes nickel-modified carbonized wood, on the cell wall of which a sulfide heterojunction grows; the sulfide heterojunction is a NiS / Ni3S4 heterojunction; the nickel-modified carbonized wood includes carbonized wood, on the cell wall of which nickel metal particles are embedded; the mass percentage of the sulfide heterojunction in the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst is 57% to 67%; the mass percentage of the nickel metal particles in the nickel-modified carbonized wood is 38% to 48%.
4. The preparation method according to claim 3, characterized in that In step S1, the wood chips are obtained by cutting wood along the lateral growth direction; the thickness of the wood chips is 2 mm to 5 mm; the wood chips are rectangular, square, triangle, parallelogram, trapezoid, ellipse or circular, and the length and width of the square are 1.5 cm to 2.5 cm × 0.7 cm to 1 cm; the wood is one of poplar, masson pine and fir; the concentration of the nickel ion solution is 0.15 mol / L to 0.25 mol / L; the nickel ion solution is obtained by dissolving a nickel salt in water; the nickel salt is at least one of nickel nitrate, nickel acetate and nickel chloride; the impregnation is carried out under vacuum conditions; the impregnation is carried out at a temperature of 60°C to 80°C; the impregnation time is 8h to 10h; after the impregnation is completed, the impregnated wood is dried under vacuum conditions, the drying temperature is 60°C to 80°C, and the drying time is 8h to 12h.
5. The preparation method according to claim 3 or 4, characterized in that: In step S2, the calcination is carried out under a protective gas atmosphere; the protective gas is nitrogen or argon; the calcination is first heated to 500°C for 1h to 2h, and then heated to 700°C to 900°C for 1h to 2h; the heating rate during the calcination process is 2°C / min to 5°C / min.
6. The preparation method according to claim 5, characterized in that: In step S3, after the calcination is completed, the following treatment is also included: grinding the calcined product with sandpaper of 1500-2000 mesh, washing the ground calcined product with deionized water, placing the washed calcined product in ethanol for ultrasonic treatment, and drying the calcined product after ultrasonic treatment under vacuum conditions; the number of grinding is 5-8 times; the number of washing is 2-3 times; the time of ultrasonic treatment is 3min-5min; the drying temperature is 60°C-80°C, and the drying time is 8h-12h.
7. The preparation method according to claim 3 or 4, characterized in that: In step S3, in the mixed solution of nickel nitrate / organic sulfur source, the concentration of nickel nitrate is 0.17 mol / L to 0.37 mol / L, and the concentration of the organic sulfur source is 0.77 mol / L to 0.97 mol / L; the organic sulfur source is at least one of thiourea, thioacetamide, and ethanol sulfur; the hydrothermal reaction is carried out at a temperature of 120° C. to 180° C.; and the hydrothermal reaction time is 12 h to 24 h.
8. The preparation method according to claim 3 or 4, characterized in that: In step S3, the NiS / Ni3S4 heterojunction is a nanorod with an average diameter of 50nm to 100nm and an average length of 1μm to 2μm; the nickel metal particles are nanoparticles with an average diameter of 20nm to 100nm.
9. Use of the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst as claimed in claim 1 or 2 or the nickel-modified carbonized wood / sulfide heterojunction composite electrocatalyst prepared by the preparation method of any one of claims 3 to 8 in hydrogen production by electrolysis of water.