A natural plant fiber / waterborne epoxy resin composite material and a manufacturing method thereof

By combining natural plant fibers with aqueous epoxy resin in an aqueous medium and using hot pressing forming technology, the problem of poor compatibility between fiber and resin interface is solved, and the high mechanical properties and environmentally friendly manufacturing process of composite materials are achieved, and the Pollution and performance problems in traditional methods.

CN114854172BActive Publication Date: 2024-11-12INST OF CHEM IND OF FOREST PROD CHINESE ACAD OF FORESTRY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210283184.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-22
Publication Date
2024-11-12
Estimated Expiration
2042-03-22

AI Technical Summary

Technical Problem

Due to poor interfacial compatibility and safety and environmental pollution problems caused by the use of organic cosolvents, natural plant fibers and epoxy resin composites have poor mechanical properties and durability, making it difficult to achieve large-scale industrial manufacturing.

Method used

The natural plant fibers and aqueous epoxy resin are directly combined in the aqueous medium, and the composite material is made by hot pressing, and the compatibility between the fiber and the resin is improved by using a curing agent with a certain polarity.

Benefits of technology

The fibers and resins are achieved with good compatibility, and the composite materials produced have excellent mechanical properties, and are simple in process and environmentally friendly, which have important practical application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114854172B_ABST
    Figure CN114854172B_ABST
Patent Text Reader

Abstract

The invention discloses a natural plant fiber / waterborne epoxy resin composite material and a manufacturing method thereof. The main components of the composite material are natural plant fiber, waterborne epoxy resin and curing agent. The natural plant fiber, waterborne epoxy resin and curing agent are uniformly mixed, dried, dehydrated and pre-cured to prepare a prepreg, and then hot-pressed to obtain a composite material. The present invention utilizes the porosity and hydrophilicity of natural plant fibers to composite the plant fibers with waterborne epoxy resin, and the manufactured plant fiber / epoxy resin composite material has excellent mechanical properties. The present invention effectively solves the problems of poor interface compatibility and low mechanical properties of the composite material when the plant fiber is directly composited with the epoxy resin, the manufacturing method is simple, and the manufacturing and use processes do not release organic solvents and volatile organic compounds (VOC), which is green and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a natural fiber / epoxy resin composite material and a manufacturing method thereof, in particular to a natural plant fiber / waterborne epoxy resin composite material and a manufacturing method thereof, belonging to the field of organic polymer composite materials. Background Art

[0002] Natural plant fiber reinforced epoxy resin composites have the advantages of abundant and renewable raw material sources, strong designability, high specific strength and specific modulus, and biodegradability. They are environmentally friendly green composites and are widely used in aerospace, rail transportation and other fields.

[0003] Natural plant fibers are hydrophilic because they contain a large number of hydroxyl groups on their surfaces, while epoxy resin matrices are usually hydrophobic. When fibers and resins are directly compounded, there are problems such as poor interface compatibility and weak bonding, which leads to poor mechanical properties and durability of the composite materials. At present, physical and chemical methods are commonly used to modify the fiber surface to improve the interfacial compatibility between the fiber and the resin. However, the existing fiber modification methods generally have problems such as poor physical modification effects and relatively complex chemical modification processes. At the same time, organic cosolvents such as ethanol, acetone and toluene are usually required in the manufacturing process of composite materials to improve the wettability of fibers and resins, which poses safety and environmental pollution problems and makes it difficult to achieve large-scale industrial manufacturing. Therefore, green and environmentally friendly composite material interface modification and manufacturing technology is a key technical bottleneck in the development and application of natural plant fiber reinforced epoxy resin composite materials.

[0004] The present invention utilizes the polarity of natural plant fiber and waterborne epoxy resin to directly compound the plant fiber and waterborne epoxy resin in an aqueous medium to prepare a composite material. The manufacturing process of the present invention is simple and environmentally friendly; at the same time, the interface compatibility between the natural plant fiber and the waterborne epoxy resin matrix is ​​good, and the manufactured composite material has excellent mechanical properties and has important practical application value. Summary of the invention

[0005] The purpose of the present invention is to provide a natural plant fiber / waterborne epoxy resin composite material and a method for manufacturing the same. The polarity of natural plant fiber and waterborne epoxy resin is utilized to achieve the compatible composite of the two in an aqueous medium, and a green composite material is manufactured by hot pressing.

[0006] The technical solution of the present invention is: a natural plant fiber / waterborne epoxy resin composite material, the main components of the composite material are natural plant fiber, waterborne epoxy resin and curing agent. The natural plant fiber is a fiber or a derivative thereof obtained by processing and separating natural plant resources and their residues, and the curing agent is a small molecule compound, oligomer or polymer with a certain polarity that can be cured and cross-linked with epoxy resin.

[0007] The natural plant fiber is any one or more of wood fiber, bamboo fiber, bast fiber, cotton fiber, straw fiber, hemp fiber, palm fiber, and husk fiber. The fiber accounts for 20% to 90% of the composite material by mass.

[0008] The waterborne epoxy resin is a water-soluble or water-dispersible epoxy resin or a compound, oligomer or polymer containing epoxy groups.

[0009] The waterborne epoxy resin is an emulsion or water dispersion based on epoxy resin.

[0010] The water-based epoxy resin is a bisphenol A epoxy resin emulsion or water dispersion.

[0011] The curing agent is any one or more of anhydride, amine compound or its derivatives.

[0012] The curing agent is any one or more of methyltetrahydrophthalic anhydride, diethyltoluenediamine, triethanolamine and ethylenediamine.

[0013] The method for manufacturing the natural plant fiber / waterborne epoxy resin composite material is achieved by the following steps:

[0014] In the first step, natural plant fibers, water-based epoxy resin and curing agent are uniformly mixed, and then dried, dehydrated and pre-cured to obtain prepreg;

[0015] In the second step, the prepreg is evenly laid, hot-pressed to obtain a composite material, and then post-cured to obtain a natural plant fiber / epoxy resin composite material.

[0016] The drying, dehydration and pre-curing process described in the first step is carried out at a temperature of 50° C. to 150° C. and for a time of 0.5 h to 8 h.

[0017] The hot pressing process described in the second step is divided into hot pressing and post-curing stages. In the hot pressing stage, the hot pressing temperature is 140℃~170℃, and the pressure is 0.05MPa~10MPa for 0min~20min, and then the pressure is 7MPa~35MPa for 30min~60min; in the post-curing stage, the curing temperature is 140℃~170℃, and the curing time is 5h~10h.

[0018] Beneficial Effects

[0019] 1. Make the epoxy resin water-based, improve its compatibility with natural plant fibers, achieve compatible composites of natural plant fibers and water-based epoxy resin, and manufacture composite materials with excellent mechanical properties.

[0020] 2. Directly use natural plant fibers and water-based epoxy resin in water-phase medium to compound and hot-press to make composite materials. The manufacturing process is simple and green. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The present invention is a process flow chart of the composite material manufacturing process.

[0022] Figure 2 This is a scanning electron microscope image of a cross section of the composite material of Example 2 of the present invention. DETAILED DESCRIPTION

[0023] A natural plant fiber / waterborne epoxy resin composite material mainly comprises natural plant fiber, waterborne epoxy resin and curing agent.

[0024] The natural plant fiber / waterborne epoxy resin composite material is manufactured by the following steps:

[0025] In the first step, natural plant fibers, water-based epoxy resin and curing agent are uniformly mixed, and then dried, dehydrated and pre-cured to obtain prepreg;

[0026] In the second step, the prepreg is evenly laid, hot-pressed to obtain a composite material, and then post-cured to obtain a natural plant fiber / epoxy resin composite material.

[0027] In the first step, the natural plant fiber is the fiber and its derivatives obtained by processing and separating natural plant resources and their residues, including any one or more of wood fiber, bamboo fiber, bast fiber, cotton fiber, straw fiber, hemp fiber, palm fiber, husk fiber and their derivatives, and the mass percentage of the fiber in the composite material is 20% to 90%; the water-based epoxy resin is a water-soluble or water-dispersible epoxy resin or a compound, oligomer and polymer containing epoxy groups, and the water-based epoxy resin is a bisphenol A epoxy resin emulsion or water dispersion; the curing agent is a small molecule compound, oligomer or polymer with a certain polarity that can be cured and cross-linked with the epoxy resin, including any one or more of anhydrides, amine compounds and their derivatives, and the curing agent is any one or more of methyltetrahydrophthalic anhydride, diethyltoluenediamine, triethanolamine and ethylenediamine.

[0028] In the first step, the temperature of the drying, dehydration and pre-curing process is 50° C. to 150° C. and the time is 0.5 h to 8 h.

[0029] In the second step, the hot pressing process is divided into hot pressing and post-curing stages. In the hot pressing stage, the hot pressing temperature is 140°C to 170°C, the pressure is 0.05MPa to 10MPa, and the pressure is maintained for 0min to 20min, and then the pressure is maintained for 30min to 60min at 7MPa to 35MPa; in the post-curing stage, the curing temperature is 140°C to 170°C, and the curing time is 5h to 10h.

[0030] Example 1

[0031] 60g of wood fiber, 180g of aqueous epoxy resin emulsion with a solid content of 13% (aqueous epoxy resin emulsion prepared according to the method of patent CN202110214043.X) and 17g of methyltetrahydrophthalic anhydride were added to a kneader, kneaded at room temperature for 30min, and then heated to 100°C and kneaded for 30min; then, the material was dried at 80°C for 2h; then, the material was dispersed with a disperser to obtain a prepreg.

[0032] The prepreg was laid in the mold and hot pressed to obtain the wood fiber / epoxy composite material. In the prepressing stage, the hot pressing temperature was 165°C, the pressure was 8MPa, and the time was 3min; in the curing stage, the temperature was 165°C, the pressure was 13MPa, and the time was 40min.

[0033] The composite material after demoulding was post-cured at 150° C. for 8 h. The tensile strength, flexural strength and flexural modulus of the composite material were measured to be 68 MPa, 138 MPa and 8.31 GPa.

[0034] Example 2

[0035] Add 60g of wood fiber, 180g of aqueous epoxy resin emulsion with a solid content of 18% (aqueous epoxy resin emulsion prepared according to the method of patent CN202110214043.X) and 7g of diethyltoluenediamine into a kneader, knead at room temperature for 30min, then heat to 100°C and knead for 30min; then, dry the material at 80°C for 2h; then disperse the material with a disperser to obtain a prepreg.

[0036] The prepreg was laid in the mold and hot pressed to obtain the wood fiber / epoxy composite material. In the prepressing stage, the hot pressing temperature was 165°C, the pressure was 8MPa, and the time was 3min; in the curing stage, the temperature was 165°C, the pressure was 13MPa, and the time was 40min.

[0037] The composite material after demoulding was post-cured at 150° C. for 8 h. The tensile strength, flexural strength and flexural modulus of the composite material were measured to be 73 MPa, 145 MPa and 8.91 GPa.

[0038] Example 3

[0039] Add 60g of hemp fiber, 180g of water-based epoxy resin emulsion with a solid content of 18% (Anbang New Material AB-EP-51) and 7g of diethyltoluenediamine into a kneader, knead at room temperature for 30 minutes, then heat to 100°C and knead for 30 minutes; then, dry the material at 90°C for 2 hours; then disperse the material with a disperser to obtain a prepreg.

[0040] The prepreg was laid in a mold and hot pressed to obtain a hemp fiber / epoxy composite material. In the prepressing stage, the hot pressing temperature was 165°C, the pressure was 8MPa, and the time was 5min; in the curing stage, the temperature was 165°C, the pressure was 13MPa, and the time was 40min.

[0041] The composite material after demoulding was post-cured at 150° C. for 8 h. The tensile strength, flexural strength and flexural modulus of the composite material were measured to be 79 MPa, 183 MPa and 10.27 GPa.

[0042] Example 4

[0043] Add 60g of wood fiber, 180g of water-based epoxy resin emulsion with a solid content of 15% (Anbang New Material AB-EP-51) and 3g of triethanolamine into a kneader, knead at room temperature for 30 minutes, then heat to 100°C and knead for 30 minutes; then, dry the material at 90°C for 2 hours; then disperse the material with a disperser to obtain a prepreg.

[0044] The prepreg was laid in the mold and hot pressed to obtain the wood fiber / epoxy composite material. In the prepressing stage, the hot pressing temperature was 165°C, the pressure was 8MPa, and the time was 5min; in the curing stage, the temperature was 165°C, the pressure was 13MPa, and the time was 40min.

[0045] The composite material after demoulding was post-cured at 150° C. for 8 h. The tensile strength, flexural strength and flexural modulus of the composite material were measured to be 62 MPa, 143 MPa and 9.07 GPa.

[0046] Example 5

[0047] 60g of bamboo fiber, 180g of waterborne epoxy resin emulsion (Huntsman Araldite PZ3961) with a solid content of 15% and 3g of triethanolamine were added to a kneader, kneaded at room temperature for 30min, and then heated to 100°C and kneaded for 30min; then, the material was dried at 80°C for 3h; and then the material was dispersed with a disperser to obtain a prepreg.

[0048] The prepreg was laid in the mold and hot pressed to obtain the bamboo fiber / epoxy composite material. In the prepressing stage, the hot pressing temperature was 165°C, the pressure was 8MPa, and the time was 5min; in the curing stage, the temperature was 165°C, the pressure was 9MPa, and the time was 40min.

[0049] The composite material after demoulding was post-cured at 150° C. for 8 h. The tensile strength, flexural strength and flexural modulus of the composite material were measured to be 85 MPa, 172 MPa and 11.03 GPa.

[0050] Example 6

[0051] 60g of wood fiber, 180g of waterborne epoxy resin emulsion (Huntsman Araldite PZ3961) with a solid content of 16% and 2g of ethylenediamine were added to a kneader, kneaded at room temperature for 30min, and then heated to 100°C and kneaded for 30min; then, the material was dried at 80°C for 3h; and then the material was dispersed with a disperser to obtain a prepreg.

[0052] The prepreg was laid in the mold and hot pressed to obtain the wood fiber / epoxy composite material. In the prepressing stage, the hot pressing temperature was 165°C, the pressure was 8MPa, and the time was 5min; in the curing stage, the temperature was 165°C, the pressure was 13MPa, and the time was 40min.

[0053] The composite material after demoulding was post-cured at 150° C. for 8 h. The tensile strength, flexural strength and flexural modulus of the composite material were measured to be 65 MPa, 143 MPa and 8.36 GPa.

[0054] Example 7

[0055] Add 80g of wood fiber, 240g of aqueous epoxy resin emulsion with a solid content of 7% (aqueous epoxy resin emulsion prepared according to the method of patent CN202110214043.X) and 3.2g of diethyltoluenediamine into a kneader, knead at room temperature for 30min, and then heat to 100°C and knead for 30min; then, dry the material at 80°C for 2h; then disperse the material with a disperser to obtain a prepreg.

[0056] The prepreg was laid in the mold and hot pressed to obtain the wood fiber / epoxy composite material. In the prepressing stage, the hot pressing temperature was 165°C, the pressure was 8MPa, and the time was 5min; in the curing stage, the temperature was 165°C, the pressure was 15MPa, and the time was 40min.

[0057] The composite material after demoulding was post-cured at 150° C. for 8 h. The tensile strength, flexural strength and flexural modulus of the composite material were measured to be 53 MPa, 156 MPa and 8.07 GPa.

[0058] Comparison example

[0059] 60 g of wood fiber, 23 g of epoxy resin (E51), 400 ml of acetone and 17 g of methyltetrahydrophthalic anhydride were added into a kneader, kneaded at room temperature for 30 min, and then heated to 60° C. and kneaded for 30 min to obtain a prepreg.

[0060] The prepreg was laid in the mold and hot pressed to obtain the wood fiber / epoxy composite material. In the prepressing stage, the hot pressing temperature was 165°C, the pressure was 8MPa, and the time was 3min; in the curing stage, the temperature was 165°C, the pressure was 13MPa, and the time was 40min.

[0061] The composite material after demoulding was post-cured at 150° C. for 8 h. The tensile strength, flexural strength and flexural modulus of the composite material were measured to be 39 MPa, 55 MPa and 7.22 GPa.

Claims

1. A natural plant fiber / waterborne epoxy resin composite material, characterized in that: The composite material is composed of natural plant fiber, water-based epoxy resin and curing agent; the natural plant fiber is any one or more of wood fiber, bamboo fiber and hemp fiber; the mass percentage of the natural plant fiber in the composite material is 20% to 90%; the water-based epoxy resin is bisphenol A epoxy resin emulsion; The preparation method is as follows: natural plant fiber, water-based epoxy resin and curing agent are mixed evenly, and a prepreg is obtained by drying, dehydrating and precuring; the prepreg is evenly laid, a composite material is obtained by hot pressing, and a natural plant fiber / epoxy resin composite material is obtained by post-curing.

2. The natural plant fiber / waterborne epoxy resin composite material according to claim 1, characterized in that: The curing agent is any one or more of methyltetrahydrophthalic anhydride, diethyltoluenediamine, triethanolamine and ethylenediamine.

3. The method for producing the natural plant fiber / waterborne epoxy resin composite material according to any one of claims 1 to 2, characterized in that: This is accomplished by following these steps: In the first step, natural plant fibers, water-based epoxy resin and curing agent are uniformly mixed, and then dried, dehydrated and pre-cured to obtain prepreg; In the second step, the prepreg is evenly laid, hot-pressed to obtain a composite material, and then post-cured to obtain a natural plant fiber / epoxy resin composite material.

4. The method for producing the natural plant fiber / waterborne epoxy resin composite material according to claim 3, characterized in that: The temperature of the drying, dehydration and pre-curing process described in the first step is 50 ℃ ~ 150 ℃, and the time is 0.5 h ~ 8 h.

5. The method for producing the natural plant fiber / waterborne epoxy resin composite material according to claim 3, characterized in that: The hot pressing process described in the second step is divided into hot pressing and post-curing stages; in the hot pressing stage, the hot pressing temperature is 140 ℃ ~ 170 ℃, and the pressure is 0.05 MPa ~ 10 MPa maintained for 3 min ~ 20 min, and then maintained at a pressure of 7 MPa ~ 35 MPa for 30 min ~ 60 min; in the post-curing stage, the curing temperature is 140 ℃ ~ 170 ℃, and the curing time is 5 h ~ 10 h.