A bipolar membrane based on in-situ grown nanosheets and a method for preparing the same

By using in-situ growth nanosheet technology in the bipolar membrane, a dense iron oxyhydroxide nanosheet array interface layer is formed, which solves the problems of catalyst leakage and instability, improves water dissociation performance and stability, and expands the bipolar Membrane application range.

CN114855217BActive Publication Date: 2024-10-18UNIV OF SCI & TECH OF CHINA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202210652117.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-10
Publication Date
2024-10-18
Estimated Expiration
2042-06-10

AI Technical Summary

Technical Problem

In practical applications of bipolar membranes, due to the loose connection between the interface layer catalyst and the anion and cation exchange membrane layers, catalyst leakage and instability in the water electrolysis device affect its water dissociation performance and stability, limiting its application scope and industrial development.

Method used

Using a bipolar membrane preparation method based on in-situ growth of nanosheets, the sulfonic acid polyphenylene ether cation exchange membrane solution is cast and heated for cross-linking, and soaked in an alkaline potassium ferrate solution to form an iron oxyhydroxide nanosheet array interface layer. Then spray the quaternary ammonium polyphenylene ether anion exchange membrane liquid to form a dense bipolar membrane structure and improve the interfacial bonding force between the catalytic layer and the membrane layer.

Benefits of technology

It significantly reduces the water dissociation voltage and improves the performance and stability of acid and alkali production. The bipolar membrane shows good operating stability and high efficiency in electrolytic water devices under acid and alkali systems, and extends the galvanostatic test time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003688104830000011
    Figure HDA0003688104830000011
  • Figure HDA0003688104830000021
    Figure HDA0003688104830000021
  • Figure HDA0003688104830000022
    Figure HDA0003688104830000022
Patent Text Reader

Abstract

The present invention provides a method for preparing a bipolar membrane based on in-situ grown nanosheets, comprising the following steps: casting a sulfonic acid type polyphenylene ether cation exchange membrane liquid on a substrate, and heating the substrate cast with the membrane liquid until some sulfonic acid groups in the membrane liquid are cross-linked to obtain a cross-linked cation exchange membrane layer; soaking one side of the cross-linked cation exchange membrane layer in an alkaline potassium ferrate solution to obtain a bipolar membrane interface layer of a hydroxyl iron nanosheet array; spraying a quaternary amine type polyphenylene ether anion exchange membrane liquid on the bipolar membrane interface layer, and drying to obtain a bipolar membrane. The water flux of the bipolar membrane prepared by the present invention is increased. The hydroxyl iron nanosheet array is fixed in the bipolar membrane interface layer by in-situ growth to improve the hydrophilicity of the interface layer, and the in-situ growth technology significantly improves the interface bonding force between the catalyst layer and the membrane layer, greatly reduces the water dissociation voltage, and significantly improves the acid and alkali production performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material technology, and in particular to a bipolar membrane based on in-situ grown nanosheets and a preparation method thereof. Background Art

[0002] The bipolar membrane is a special new type of composite ion exchange membrane, which is generally composed of an anion exchange membrane layer, a cation exchange membrane layer and an interface layer. When a reverse bias is applied to both sides of the bipolar membrane, under the action of the external electric field, the water molecules in the interface layer undergo a water dissociation reaction to generate hydrogen ions and hydroxide ions. Further, under the action of the electric field, the hydrogen ions and hydroxides move to the electrode chambers on both sides of the bipolar membrane, converting the salt solution in the electrode chamber feed liquid into the corresponding acid and base. Since the acid and alkali production process of the bipolar membrane does not involve the generation of harmful gases, it has been combined with a variety of chemical processes and invested in energy conversion and storage, clean production, and wastewater resource treatment. For example, bipolar membrane water electrolysis produces hydrogen, bipolar membrane flow batteries, and bipolar membrane combined with biological anodes for wastewater treatment.

[0003] Since hydrogen has a high calorific value and meets the conditions of being clean and renewable, it has been widely used as a new energy source. At present, conventional hydrogen production technology still relies on water electrolysis reaction. Its cathode hydrogen evolution reaction has a low overpotential under acidic conditions, and the anode oxygen evolution reaction has a low overpotential under alkaline conditions. The bipolar membrane is introduced into the water electrolysis device as a diaphragm, and the water dissociation reaction at the interface layer under reverse bias is used to generate hydrogen ions and hydroxide ions. The pH gradient on both sides is maintained so that the hydrogen evolution and oxygen evolution reactions at the cathode and anode can be in the optimal pH environment. At the same time, it is also beneficial to expand the selection of electrode reaction catalysts, such as a large number of non-precious metal catalysts on the earth, avoiding the cost increase caused by the use of precious metal catalysts.

[0004] However, in the actual application of bipolar membranes, the catalyst leakage occurs due to the loose bonding between the interface layer catalyst and the anion and cation exchange membrane layers on both sides, or the instability of the cation exchange membrane layers and anion exchange membrane layers on both sides of the bipolar membrane in the water electrolysis device under acid and alkaline systems, resulting in an increase in the water dissociation voltage of the bipolar membrane, a decrease in the water dissociation performance, and a decrease in the acid and alkali production efficiency, which affects the stability of the bipolar membrane, limits the further expansion of the application of the bipolar membrane, and hinders the large-scale application and industrial development of the bipolar membrane. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a method for preparing a bipolar membrane based on in-situ grown nanosheets. The bipolar membrane prepared by the present invention is tightly combined with the anion and cation exchange membrane layers on both sides, the water dissociation voltage of the bipolar membrane does not increase, the water dissociation performance is good, the acid and alkali production efficiency is high, and the stability is good. At the same time, the bipolar membrane is applied to a water electrolysis device under an acid and alkali system. The bipolar membrane has good operating stability, further expanding the application range of the bipolar membrane.

[0006] The present invention provides a method for preparing a bipolar membrane based on in-situ grown nanosheets, comprising the following steps:

[0007] A) casting a sulfonic acid type polyphenylene ether cation exchange membrane liquid on a substrate, and heating the substrate on which the membrane liquid is cast, until part of the sulfonic acid groups in the membrane liquid are cross-linked, thereby obtaining a cross-linked cation exchange membrane layer;

[0008] B) soaking one side of the cross-linked cation exchange membrane layer in an alkaline potassium ferrate solution to obtain an iron oxyhydroxide nanosheet array bipolar membrane interface layer;

[0009] C) spraying quaternary amine type polyphenylene ether anion exchange membrane liquid on the interface layer of the bipolar membrane, and drying to obtain the bipolar membrane.

[0010] Preferably, the sulfonic acid polyphenylene ether cation exchange membrane liquid comprises sulfonic acid polyphenylene ether powder particles and an organic solvent; the mass concentration of the sulfonic acid polyphenylene ether powder particles in the sulfonic acid polyphenylene ether cation exchange membrane liquid is 3% to 9%.

[0011] Preferably, the heating temperature in step A) is 60-90° C. and the heating time is 15-96 hours.

[0012] Preferably, the thickness of the cross-linked cation exchange membrane layer in step A) is 30 to 70 μm.

[0013] Preferably, the alkaline potassium permanganate solution in step B) is prepared by centrifuging potassium ferrate and an alkali solution; the concentration of the alkali solution is 1 to 12 mol / L; the centrifugal speed is 3000 to 12000 rpm, and the centrifugal time is 3 to 10 min.

[0014] Preferably, the mass concentration of potassium ferrate in the alkaline potassium permanganate solution in step B) is 0.001 to 0.05 mol / L;

[0015] The soaking time is 0.5 to 24 hours.

[0016] Preferably, the method for preparing the quaternary amine type polyphenylene ether anion exchange membrane liquid in step C) is specifically as follows:

[0017] The brominated polyphenylene ether reacts with an amine organic substance to undergo a quaternization reaction, and the solution after the reaction is precipitated in a precipitant, and the precipitate is dissolved again to obtain a quaternized polyphenylene ether anion exchange membrane liquid;

[0018] The amine organic matter is a tertiary amine organic matter; the bromination degree of the brominated polyphenylene ether is 20% to 50%.

[0019] Preferably, the mass concentration of quaternary ammonium polyphenylene in the quaternary ammonium polyphenylene ether anion exchange membrane liquid in step C) is 2% to 7%.

[0020] Preferably, in step C), the thickness of the quaternized polyphenylene ether anion exchange membrane layer is 8 to 45 μm.

[0021] The present invention provides a bipolar membrane based on in-situ grown nanosheets, which is prepared by the preparation method described in any one of the above technical solutions.

[0022] Compared with the prior art, the present invention provides a method for preparing a bipolar membrane based on in-situ grown nanosheets, comprising the following steps: A) casting a sulfonic acid type polyphenylene ether cation exchange membrane liquid on a substrate, and heating the substrate cast with the membrane liquid until part of the sulfonic acid groups in the membrane liquid are cross-linked to obtain a cross-linked cation exchange membrane layer; B) soaking one side of the cross-linked cation exchange membrane layer in an alkaline potassium ferrate solution to obtain a bipolar membrane interface layer of a hydroxy iron oxide nanosheet array; and C) spraying a quaternary amine type polyphenylene ether anion exchange membrane liquid on the bipolar membrane interface layer, and drying to obtain a bipolar membrane.

[0023] The anion exchange membrane layer and cation exchange membrane layer selected by the present invention are both densely structured and have good hydrophilicity, so that the water flux of the prepared bipolar membrane is increased; potassium ferrate is hydrolyzed to generate Fe(OH)3 colloid, and the alkaline environment promotes the coagulation of the positively charged Fe(OH)3 colloid, so the Fe(OH)3 colloid is successfully adsorbed on the surface of the negatively charged cation exchange membrane layer, and further converted into an array of hydroxyl iron nanosheets. The array of hydroxyl iron nanosheets is fixed in the interface layer of the bipolar membrane by in-situ growth. The nanosheet material is beneficial to increase the reactive area and the number of catalytic active sites, improve the hydrophilicity of the interface layer, and the in-situ growth technology significantly improves the interfacial bonding force between the catalytic layer and the membrane layer. Therefore, the bipolar membrane prepared by this technology not only achieves a significant reduction in the water dissociation voltage, but also significantly improves the acid and alkali production performance, and further enhances the stability of the bipolar membrane. Experimental results show that when 0 to 100 mA / cm is applied 2 At a current density of 1.5 volts, the voltage required for water dissociation by the bipolar membrane was less than 1 V. After 3 hours of electrodialysis, the concentration of acid and alkali produced by the bipolar membrane reached 0.39 mol / L. Compared with the blank sample, the voltage of the bipolar membrane acid and alkali production device was significantly reduced. 2 ) During the test, the water dissociation voltage was stable between 0.74-0.77 V. The bipolar membrane was applied to the water electrolysis device in acid and alkali systems. At a current density of 100, the bipolar membrane was able to achieve constant current stability for 27 hours, and the voltage was stable at about 1 V. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1A schematic flow chart of an embodiment of a method for preparing a bipolar membrane based on in-situ growth of nanosheets according to the present invention;

[0025] Figure 2 A transmission electron microscope image of an iron oxyhydroxide nanosheet powder according to an embodiment of a method for preparing a bipolar membrane based on in-situ growth of nanosheets of the present invention;

[0026] Figure 3 This is a scanning electron microscope image of a dense cross-linked cation exchange membrane layer of an embodiment of a method for preparing a bipolar membrane based on in-situ growth of nanosheets of the present invention;

[0027] Figure 4 This is a scanning electron microscope image of a dense cross-linked cation exchange membrane layer carrying an array of iron oxyhydroxide nanosheets according to an embodiment of a method for preparing a bipolar membrane based on in-situ growth of nanosheets of the present invention;

[0028] Figure 5 A scanning electron microscope morphology image of a cross section of a bipolar membrane of a method for preparing a bipolar membrane based on in-situ growth of nanosheets according to the present invention;

[0029] Figure 6 The current-voltage curve of a bipolar membrane of a bipolar membrane preparation method based on in-situ growth of nanosheets of the present invention;

[0030] Figure 7 A schematic diagram of the electrodialysis performance of a bipolar membrane according to a method for preparing a bipolar membrane based on in-situ growth of nanosheets of the present invention;

[0031] Figure 8 It is a schematic diagram of the water dissociation stability test performance under constant current density of a bipolar membrane of a bipolar membrane preparation method based on in-situ growth of nanosheets of the present invention.

[0032] Fig. 9 It is a schematic diagram of the performance of a bipolar membrane prepared by a method for preparing a bipolar membrane based on in-situ grown nanosheets in the present invention, in a water dissociation stability test at a constant current density in an acid and base system. DETAILED DESCRIPTION

[0033] The present invention provides a bipolar membrane based on in-situ grown nanosheets and a method for preparing the same. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and they all fall within the scope of protection of the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0034] The present invention provides a method for preparing a bipolar membrane based on in-situ grown nanosheets, comprising the following steps:

[0035] A) casting a sulfonic acid type polyphenylene ether cation exchange membrane liquid on a substrate, and heating the substrate on which the membrane liquid is cast, until part of the sulfonic acid groups in the membrane liquid are cross-linked, thereby obtaining a cross-linked cation exchange membrane layer;

[0036] B) soaking one side of the cross-linked cation exchange membrane layer in an alkaline potassium ferrate solution to obtain an iron oxyhydroxide nanosheet array bipolar membrane interface layer;

[0037] C) spraying quaternary amine type polyphenylene ether anion exchange membrane liquid on the interface layer of the bipolar membrane, and drying to obtain the bipolar membrane.

[0038] The invention provides a method for preparing a bipolar membrane based on in-situ grown nanosheets. Firstly, a sulfonic acid type polyphenylene ether cation exchange membrane liquid is cast on a substrate.

[0039] The sulfonic acid polyphenylene ether cation exchange membrane liquid comprises sulfonic acid polyphenylene ether powder particles and an organic solvent; the mass concentration of the sulfonic acid polyphenylene ether powder particles in the sulfonic acid polyphenylene ether cation exchange membrane liquid is preferably 3% to 9%, and more preferably 4% to 8%.

[0040] Furthermore, the sulfonic acid type polyphenylene ether cation exchange membrane is uniformly cast on the substrate, and the substrate cast with the cation exchange membrane liquid is placed on a heating plate for heating until the sulfonic acid groups in the cation exchange membrane liquid are partially cross-linked, the heating temperature is 60 to 90°C, and the heating time is 15 to 96 hours; more preferably, the heating temperature is 65 to 85°C, and the heating time is 20 to 80 hours.

[0041] The thickness of the cationic membrane layer of the bipolar membrane preparation method based on in-situ growth of nanosheets is 30 to 70 μm.

[0042] One side of the cross-linked cation exchange membrane layer is immersed in an alkaline potassium ferrate solution to obtain an iron oxyhydroxide nanosheet array bipolar membrane interface layer.

[0043] The alkaline potassium permanganate solution of the present invention is specifically obtained by mixing potassium ferrate with an alkaline solution and centrifuging; the concentration of the alkaline solution is preferably 1-12 mol / L; more preferably 2-10 mol / L; the centrifugal speed is 3000 to 12000 rpm, and the centrifugal time is 3 to 10 min; more preferably, the speed is 4000 to 10000 rpm, and the centrifugal time is 4 to 8 min.

[0044] Furthermore, an alkaline potassium ferrate solution is immersed on one side of the obtained dense cross-linked cation exchange membrane layer to in situ grow an iron oxide hydroxide nanosheet array on the dense cross-linked cation exchange membrane layer as a bipolar membrane interface layer, and the immersion time of the alkaline potassium ferrate solution is 0.5 to 24 hours; more preferably 2 to 16 hours; most preferably 3 to 12 hours.

[0045] In the present invention, the mass concentration of potassium ferrate in the alkaline potassium permanganate solution is preferably 0.001 to 0.05 mol / L; more preferably 0.002 to 0.04 mol / L; most preferably 0.003 to 0.03 mol / L.

[0046] The bipolar membrane is obtained by spraying a quaternary amine type polyphenylene ether anion exchange membrane liquid on the interface layer of the bipolar membrane and drying the liquid.

[0047] In some preferred embodiments of the present invention, the preparation method of the quaternary amine type polyphenylene ether anion exchange membrane liquid is specifically as follows:

[0048] The brominated polyphenylene ether reacts with an amine organic substance to undergo a quaternization reaction, and the solution after the reaction is precipitated in a precipitant, and the precipitate is dissolved again to obtain a quaternized polyphenylene ether anion exchange membrane liquid;

[0049] In some preferred embodiments of the present invention, a brominated polyphenylene ether solution with a certain degree of bromination is subjected to a quaternary amination reaction with an amine organic substance at 15 to 55° C. for 15 to 96 hours. After the reaction, the solution is precipitated in a precipitant, and the product is dissolved again to obtain a quaternary polyphenylene ether anion exchange membrane liquid. The amine organic substance selected for the quaternary amination reaction is a tertiary amine organic substance.

[0050] It should be noted that the tertiary amine organic substance used in this embodiment is trimethylamine. It should be understood that the tertiary amine organic substance used in the bipolar membrane preparation method based on in situ growth of nanosheets of the present invention can be one or more of trimethylamine, triethylamine or N-methylpiperidine.

[0051] The bromination degree of the brominated polyphenylene ether of the present invention is 20% to 50%.

[0052] The precipitant of the present invention is preferably ether or ethyl acetate.

[0053] Specifically, the mass concentration of quaternary amine polyphenylene in the quaternary amine polyphenylene ether anion exchange membrane liquid is preferably 2% to 7%; more preferably 3% to 6%; and most preferably 4% to 6%.

[0054] The thickness of the quaternized polyphenylene ether anion exchange membrane layer of the present invention is 8-45 μm.

[0055] The present invention provides a bipolar membrane based on in-situ grown nanosheets, which is prepared by the preparation method described in any one of the above technical solutions.

[0056] The invention provides a method for preparing a bipolar membrane based on in-situ grown nanosheets, comprising the following steps: A) casting a sulfonic acid type polyphenylene ether cation exchange membrane liquid on a substrate, and heating the substrate cast with the membrane liquid until part of the sulfonic acid groups in the membrane liquid are cross-linked to obtain a cross-linked cation exchange membrane layer; B) soaking one side of the cross-linked cation exchange membrane layer in an alkaline potassium ferrate solution to obtain a bipolar membrane interface layer of an iron oxide hydroxide nanosheet array; and C) spraying a quaternary amine type polyphenylene ether anion exchange membrane liquid on the bipolar membrane interface layer, and drying to obtain a bipolar membrane.

[0057] The anion exchange membrane layer and the cation exchange membrane layer selected by the present invention are both densely structured and have good hydrophilicity, so that the water flux of the prepared bipolar membrane is increased; potassium ferrate is hydrolyzed to generate Fe(OH)3 colloid, and the alkaline environment promotes the coagulation of the positively charged Fe(OH)3 colloid, so the Fe(OH)3 colloid is successfully adsorbed on the surface of the negatively charged cation exchange membrane layer, and further converted into an array of hydroxyl iron nanosheets. The array of hydroxyl iron nanosheets is fixed in the interface layer of the bipolar membrane by in-situ growth. The nanosheet material is beneficial to increase the reaction active area and the number of catalytic active sites, improve the hydrophilicity of the interface layer, and the in-situ growth technology significantly improves the interfacial bonding force between the catalytic layer and the membrane layer. Therefore, the bipolar membrane prepared by this technology not only achieves a significant reduction in the water dissociation voltage and a significant improvement in the acid and alkali production performance, but also further enhances the stability of the bipolar membrane. At the same time, the bipolar membrane is applied to the electrolytic water device under the acid and alkali system, further expanding the application of the bipolar membrane. The experimental results show that when 0 to 100 mA / cm is applied 2 At a current density of 1.5 volts, the voltage required for water dissociation by the bipolar membrane was less than 1 V. After 3 hours of electrodialysis, the concentration of acid and alkali produced by the bipolar membrane reached 0.39 mol / L. Compared with the blank sample, the voltage of the bipolar membrane acid and alkali production device was significantly reduced. 2 ) During the test, the water dissociation voltage was stable between 0.74-0.77 V. The bipolar membrane was applied to the water electrolysis device in acid and alkali systems. 2 At a current density of , the bipolar membrane can achieve constant current stability for 27 hours, and the voltage is stable at around 1V.

[0058] In order to further illustrate the present invention, a bipolar membrane based on in-situ grown nanosheets and a preparation method thereof provided by the present invention are described in detail below in conjunction with embodiments.

[0059] Example 1

[0060] Please refer to Figure 1 , Figure 1 It is a schematic flow chart of the first embodiment of the method for preparing a bipolar membrane by in-situ growth of nanosheets according to the present invention.

[0061] The present invention provides an embodiment of a method for preparing a bipolar membrane based on in-situ grown nanosheets. It should be understood that the schematic diagram is presented in a logical order. However, in some cases, the devices and steps shown or described may be implemented in a different order than that described here.

[0062] Specifically, for example, a sulfonic acid polyphenylene ether polymer is dissolved in an organic solvent to prepare a sulfonic acid polyphenylene ether cation exchange membrane liquid with a mass fraction of 5%, a glass plate is placed on a hot plate at 80°C for heating, an appropriate amount of the sulfonic acid polyphenylene ether cation exchange membrane liquid is evenly coated, and the heating is continued for 24 hours so that the sulfonic acid groups in the sulfonic acid polyphenylene ether cation exchange membrane liquid are partially cross-linked, and a cross-linked cation exchange membrane layer with a dense structure can be obtained. The glass plate carrying the sulfonic acid polyphenylene ether cation exchange membrane is placed in a container filled with deionized water for soaking, and the sulfonic acid polyphenylene ether cation exchange membrane can fall off the glass plate.

[0063] It is particularly noted that the substrate used in the method for preparing a bipolar membrane based on in-situ grown nanosheets of the present invention can be a glass plate or a polytetrafluoroethylene plastic plate. It should be understood that the method for preparing a bipolar membrane based on in-situ grown nanosheets of the present invention does not limit the substrate used for preparing a dense cation exchange membrane.

[0064] Specifically, for example, a sodium hydroxide solution with a concentration of 2 mol / L is prepared, potassium ferrate is added to form an alkaline potassium ferrate dispersion of 0.007 mol / L, the dispersion is ultrasonically dissolved for 40 minutes, the sodium hydroxide solution of potassium ferrate after ultrasonic dissolution is centrifuged in a centrifuge at a speed of 5000 rpm / min for 5 minutes, and the supernatant is the reaction solution.

[0065] Specifically, for example, a dense cation exchange membrane that has fallen off a glass plate is fixed in a device, 30 mL of centrifuged alkaline potassium ferrate solution is added to the device, and the potassium ferrate in the alkaline potassium ferrate solution is slowly hydrolyzed at 25°C under alkaline conditions to in situ grow an array of hydroxyl iron oxide nanosheets on the dense cation exchange membrane. After 8 hours, the sulfonic acid polyphenylene ether cation exchange membrane is removed from the device, and the surface of the sulfonic acid polyphenylene ether cation exchange membrane is rinsed with deionized water until the pH of the washing solution is neutral.

[0066] The concentration of 5% polyphenylene ether bromide solution is measured, trimethylamine solution is added to the polyphenylene ether bromide solution, reacted at 25°C for 24 hours, the solution after the reaction is dripped into ether for precipitation, washed multiple times, filtered and dried to obtain a quaternary polyphenylene ether polymer. The quaternary polyphenylene ether polymer is configured into a solution with a mass concentration of 5%, a dense cation exchange membrane carrying an in-situ grown hydroxyl iron nanosheet array as an interface layer is placed in a precision ultrasonic spraying device, 3mL of the quaternary polyphenylene ether solution with a mass concentration of 5% is ultrasonically atomized and evenly sprayed on one side of the dense cation exchange membrane carrying an in-situ grown hydroxyl iron nanosheet array as an interface layer to prepare an anion exchange membrane layer, and after the spraying is completed, it is dried for a period of time to obtain a bipolar membrane with an intermediate layer of the hydroxyl iron nanosheet array.

[0067] In this embodiment, a sulfonic acid polyphenylene ether cation exchange membrane is uniformly cast on a substrate, and the substrate with the cast membrane liquid is placed on a heating plate for heating until the sulfonic acid groups in the cation exchange membrane liquid are partially cross-linked to obtain a cross-linked cation exchange membrane layer with a dense structure; one side of the obtained dense cross-linked cation exchange membrane layer is immersed in an alkaline potassium ferrate solution to in-situ grow an iron hydroxide nanosheet array on the dense cross-linked cation exchange membrane layer as a bipolar membrane interface layer; the in-situ grown iron hydroxide nanosheet array is used as an interfacial layer, and a quaternary amine polyphenylene ether anion exchange membrane liquid is sprayed on one side of the dense cross-linked cation exchange membrane layer carrying the in-situ grown iron hydroxide nanosheet array, and after drying the anion exchange membrane liquid, a bipolar membrane with the iron hydroxide nanosheet array as the interface layer is obtained. The anion exchange membrane layer and the cation exchange membrane layer selected by the present invention are both dense in structure and have good hydrophilicity, so that the water flux of the prepared bipolar membrane is increased; and the iron oxyhydroxide nanosheet array is fixed on the dense cation exchange membrane by in-situ growth, which is beneficial to increase the reaction active area, increase the active sites of the catalyst and enhance the binding force with the membrane layer, so that the water dissociation voltage of the bipolar membrane is reduced and the stability of the bipolar membrane is improved.

[0068] The experimental results show that applying 0 to 100 mA / cm 2 At a current density of 1.5 volts, the voltage required for water dissociation by the bipolar membrane was less than 1 V. After 3 hours of electrodialysis, the concentration of acid and alkali produced by the bipolar membrane reached 0.39 mol / L. The bipolar membrane was tested at a constant current of 50 mA / cm 2 ) During the test, the water dissociation voltage was stable at about 0.74 V. The bipolar membrane was applied to the water electrolysis device in acid and alkali systems. 2 At a current density of , the bipolar membrane can achieve constant current stability for 20 hours, and the voltage is stable at around 1V.

[0069] Example 2

[0070] Furthermore, a second embodiment of the method for preparing a bipolar membrane based on in-situ grown nanosheets of the present invention is proposed. In this embodiment, a sulfonic acid type polyphenylene ether cationic polymer is uniformly configured into a solution with a mass fraction of 7%, an appropriate amount of polyphenylene ether cation exchange membrane liquid is dripped on a glass plate, and the solution is heated on a hot plate at 70°C for 48 hours to partially cross-link the sulfonic acid groups in the sulfonic acid type polyphenylene ether cation exchange membrane liquid. After the cross-linking is completed, the glass plate with the dense cross-linked cation exchange membrane is removed and cooled to room temperature, and then immersed in deionized water until the dense cross-linked cation exchange membrane naturally falls off the glass plate.

[0071] A potassium hydroxide solution with a concentration of 3 mol / L is prepared, and potassium ferrate is added to prepare a 0.01 mol / L alkaline potassium ferrate dispersion. The above dispersion is stirred and dissolved for 30 minutes. After the stirring is completed, high-speed centrifugation is performed at a speed of 5000 rpm for 5 minutes. After the completion, the supernatant is taken to obtain an alkaline potassium ferrate solution. The dense cation exchange membrane that has fallen off the glass plate is fixed in the device, and 60 mL of the alkaline potassium ferrate solution after centrifugation is added to the device, so that the alkaline potassium ferrate solution is slowly hydrolyzed at 35°C and alkaline conditions to in-situ grow hydroxyl iron oxide nanosheet arrays on the dense cation exchange membrane. After 4 hours, the dense cation exchange membrane is taken out from the device, and the surface of the sulfonic acid polyphenylene ether cation exchange membrane is rinsed with deionized water until the pH of the washing liquid is neutral.

[0072] A polyphenylene ether bromide solution with a mass concentration of 5% is prepared, a triethylamine solution is measured and added to the polyphenylene ether bromide solution, and the reaction is carried out at 25°C for 48 hours. The solution after the reaction is dripped into ether for precipitation, and after multiple washings, suction filtration and drying are performed to obtain a quaternary polyphenylene ether polymer. The quaternary polyphenylene ether polymer is configured into a solution with a mass fraction of 2.5%, and a dense cation exchange membrane carrying an in-situ grown hydroxyl iron nanosheet array as an interface layer is moved into a precision ultrasonic spraying device, and the quaternary polyphenylene ether solution is ultrasonically atomized and uniformly sprayed on one side of the dense cation exchange membrane carrying an in-situ grown hydroxyl iron nanosheet array as an interface layer to prepare an anion exchange membrane layer. After the spraying is completed, the anion exchange membrane liquid is dried to obtain a bipolar membrane with an oxyhydroxide iron nanosheet array as an interface layer.

[0073] The experimental results show that applying 0 to 100 mA / cm 2 At a current density of 1.5 volts, the voltage required for water dissociation by the bipolar membrane was less than 1 V. After 3 hours of electrodialysis, the concentration of acid and alkali produced by the bipolar membrane reached 0.37 mol / L. The bipolar membrane was tested at a constant current of 50 mA / cm 2 ) During the test, the water dissociation voltage was stable at about 0.76 V. The bipolar membrane was applied to the water electrolysis device in acid and alkali systems.2 At a current density of , the bipolar membrane can achieve constant current stability for 18 hours, and the voltage is stable at around 1V.

[0074] Example 3

[0075] Furthermore, a third embodiment of the method for preparing a bipolar membrane based on in-situ grown nanosheets of the present invention is proposed. In this embodiment, a sulfonic acid type polyphenylene ether cationic polymer is uniformly configured into a solution with a mass fraction of 8%, an appropriate amount of sulfonic acid type polyphenylene ether cation exchange membrane liquid is dripped on a polytetrafluoroethylene plastic plate, and the solution is heated on a hot plate at 80°C for 72 hours to partially cross-link the sulfonic acid groups in the sulfonic acid type polyphenylene ether cation exchange membrane liquid. After the cross-linking is completed, the solution is removed and cooled to room temperature, and then the glass plate with the dense cross-linked cation exchange membrane is immersed in deionized water until the dense cross-linked cation exchange membrane naturally falls off the glass plate.

[0076] A sodium hydroxide solution with a concentration of 6 mol / L was prepared, potassium ferrate was added, and a 0.02 mol / L alkaline potassium ferrate dispersion was prepared. The dispersion was ultrasonically dissolved for 40 minutes. After the ultrasonic dissolution was completed, high-speed centrifugation was performed at a speed of 8000 rpm for 7 minutes. After the end, the supernatant was taken to obtain an alkaline potassium ferrate solution. The dense polyphenylene ether cation exchange membrane that had fallen off the glass plate was fixed in the device, and 30 mL of the alkaline potassium ferrate solution after centrifugation was added to the device, so that the potassium ferrate in the alkaline potassium ferrate solution was slowly hydrolyzed at 30°C and alkaline conditions to in-situ grow hydroxyl iron oxide nanosheet arrays on the dense cation exchange membrane. After 2 hours, the dense cation exchange membrane was taken out from the device, and the surface of the dense cation exchange membrane was rinsed with deionized water until the pH of the washing solution was neutral.

[0077] A brominated polyphenylene ether solution with a mass concentration of 5% is prepared, a triethylamine solution is measured and added to the brominated polyphenylene ether solution, and the reaction is carried out at 50°C for 72 hours. The solution after the reaction is dripped into ether for precipitation, and the solution is filtered and dried after multiple washing to obtain a quaternary aminated polyphenylene ether polymer. The quaternary aminated polyphenylene ether polymer is configured into a solution with a mass fraction of 2.5%, and a dense cation exchange membrane carrying an in-situ grown hydroxyl iron nanosheet array as an interface layer is placed in a precision ultrasonic spraying device, and the quaternary aminated polyphenylene ether solution is evenly sprayed on one side of the dense cation exchange membrane carrying an in-situ grown hydroxyl iron nanosheet array as an interface layer through ultrasonic atomization to prepare an anion exchange membrane layer. After the spraying is completed, the anion exchange membrane liquid is dried to obtain a bipolar membrane with an interface layer of the hydroxyl iron nanosheet array.

[0078] The experimental results show that applying 0 to 100 mA / cm 2At a current density of 1.5 volts, the voltage required for water dissociation by the bipolar membrane was less than 1 V. After 3 h of electrodialysis, the concentration of acid and alkali produced by the bipolar membrane reached 0.36 mol / L. The bipolar membrane was tested at a constant current of 50 mA / cm 2 ) During the test, the water dissociation voltage was stable at about 0.78 V. The bipolar membrane was applied to the water electrolysis device in acid and alkali systems. 2 At a current density of , the bipolar membrane can achieve constant current stability for 15 hours, and the voltage is stable at around 1V.

[0079] Example 4

[0080] Furthermore, a fourth embodiment of the method for preparing a bipolar membrane based on in-situ grown nanosheets of the present invention is proposed. In this embodiment, a sulfonic acid type polyphenylene ether cationic polymer is uniformly configured into a solution with a mass fraction of 9%, an appropriate amount of sulfonic acid type polyphenylene ether cationic exchange membrane liquid is dripped on a polytetrafluoroethylene plastic plate, and the solution is heated on a hot plate at 90°C for 96 hours to partially cross-link the sulfonic acid groups in the sulfonic acid type polyphenylene ether cationic exchange membrane liquid. After the cross-linking is completed, the solution is removed and cooled to room temperature, and then the glass plate with the dense cross-linked cationic exchange membrane is immersed in deionized water until the dense cross-linked cationic exchange membrane naturally falls off the glass plate.

[0081] A sodium hydroxide solution with a concentration of 8 mol / L is prepared, potassium ferrate is added, and a 0.03 mol / L alkaline potassium ferrate dispersion is prepared. The dispersion is ultrasonically dissolved for 40 minutes. After the ultrasonic dissolution is completed, high-speed centrifugation is performed at a speed of 8000 rpm for 10 minutes. After the end, the supernatant is taken to obtain an alkaline potassium ferrate solution. The dense polyphenylene ether cation exchange membrane that has fallen off the glass plate is fixed in the device, and 30 mL of the alkaline potassium ferrate solution after centrifugation is added to the device, so that the potassium ferrate in the alkaline potassium ferrate solution is slowly hydrolyzed at 30°C and alkaline conditions to in-situ grow hydroxyl iron oxide nanosheet arrays on the dense cation exchange membrane. After 2 hours, the dense cation exchange membrane is taken out from the device, and the surface of the dense cation exchange membrane is rinsed with deionized water until the pH of the washing liquid is neutral.

[0082] A brominated polyphenylene ether solution with a mass concentration of 5% is prepared, a triethylamine solution is measured and added to the brominated polyphenylene ether solution, and the reaction is carried out at 50°C for 96 hours. The solution after the reaction is dripped into ether for precipitation, and after multiple washings, suction filtration and drying are performed to obtain a quaternized polyphenylene ether polymer. The quaternized polyphenylene ether polymer is configured into a solution with a mass fraction of 2.5%, and a dense cation exchange membrane carrying an in-situ grown hydroxyl iron nanosheet array as an interface layer is placed in a precision ultrasonic spraying device, and the quaternized polyphenylene ether solution is evenly sprayed on one side of a sulfonated dense cation exchange membrane carrying an in-situ grown hydroxyl iron nanosheet array as an interface layer through ultrasonic atomization to prepare an anion exchange membrane layer. After the spraying is completed, the anion exchange membrane liquid is dried to obtain a bipolar membrane with an interface layer of an oxyhydroxyl iron nanosheet array.

[0083] The experimental results show that applying 0 to 100 mA / cm 2 At a current density of 1.5 volts, the voltage required for water dissociation by the bipolar membrane was less than 1 V. After 3 hours of electrodialysis, the concentration of acid and alkali produced by the bipolar membrane reached 0.38 mol / L. The bipolar membrane was tested at a constant current of 50 mA / cm 2 ) During the test, the water dissociation voltage was stable at around 0.79 V. The bipolar membrane was applied to the water electrolysis device in acid and alkali systems. 2 At a current density of , the bipolar membrane can achieve constant current stability for 15 hours, and the voltage is stable at around 1V.

[0084] The iron oxyhydroxide nanosheet array obtained by the bipolar membrane preparation method based on in situ growth of nanosheets of the present invention was analyzed by transmission electron microscopy, and the dense cross-linked cation exchange membrane used in the bipolar membrane preparation method based on in situ growth of nanosheets was analyzed by scanning electron microscopy. The specific process is as follows:

[0085] The iron oxide hydroxy nanosheet powder obtained by the method for preparing a bipolar membrane based on in-situ growth of nanosheets prepared in Example 1 of the present invention is washed several times until it is neutral and dried in an oven, then an appropriate amount of the iron oxide hydroxy nanosheet powder is added to anhydrous ethanol, and ultrasonicated until the iron oxide hydroxy nanosheet powder is evenly dispersed in the anhydrous ethanol, and an appropriate amount of the anhydrous ethanol dispersion of the iron oxide hydroxy nanosheet powder is dropped on the surface of the copper mesh, and left for a period of time until the anhydrous ethanol on the copper mesh is completely evaporated, and the copper mesh with the iron oxide hydroxy nanosheet powder is sent to the sample injection chamber of a transmission electron microscope for testing to observe the morphology image of the iron oxide hydroxy nanosheet powder, as shown in FIG. Figure 2 shown.

[0086] Reference Figure 2Based on the obtained transmission electron microscope image, the multilayer structure of the iron oxyhydroxide nanosheet and the ultra-thin structure of the nanosheet layer can be intuitively seen. The iron oxyhydroxide nanosheet has a high specific surface area, which is beneficial to increase the number of catalytic active sites, increase hydrophilicity, replenish the water molecules consumed in the interface layer in time, and improve the water dissociation performance of the bipolar membrane.

[0087] The dense cross-linked cation exchange membrane layer prepared by the bipolar membrane preparation method based on in-situ growth of nanosheets and the dense cross-linked cation exchange membrane carrying the iron oxyhydroxide nanosheet array were taken out from the deionized water, and heated and dried respectively using a hot plate in a precision ultrasonic spraying device. An appropriate amount of the membrane was cut and pasted on the conductive adhesive. After gold spraying, it was moved into the sample chamber of a scanning electron microscope for testing and observation, and the surface morphology of the sulfonic acid polyphenylene ether cation exchange membrane was obtained, as shown in FIG. Figure 3 and Figure 4 As shown. Among them, Figure 3 This is a scanning electron microscope image of a dense cross-linked cation exchange membrane layer. Figure 4 This is a scanning electron microscope image of a dense cross-linked cation exchange membrane layer carrying an array of iron oxyhydroxide nanosheets.

[0088] right Figure 3 and Figure 4 Comparison of two scanning electron microscope images shows that iron oxyhydroxide nanosheet arrays were successfully introduced into the interface layer by in situ growth to catalyze the water dissociation reaction. Figure 4 It can be seen that the iron oxyhydroxide nanosheets are evenly and tightly distributed and have a large specific surface area, which is beneficial to increase the number of catalytic sites and reduce the water dissociation voltage.

[0089] The bipolar membrane prepared by the bipolar membrane preparation method based on in-situ growth of nanosheets was taken out from the precision ultrasonic spraying device, and a suitable amount of bipolar membrane was cut, clamped with tweezers and immersed in liquid nitrogen for a few seconds, and then taken out for low-temperature brittle fracture treatment. The prepared bipolar membrane cross-section sample was attached to the sample stage with conductive adhesive, and gold was sprayed, and then moved into the scanning electron microscope sample chamber for testing, and a scanning electron microscope morphology of the cross section of the bipolar membrane with the interface layer constructed based on in-situ growth of nanosheets was obtained, as shown in FIG. Figure 5 shown.

[0090] Please refer to Figure 5 ,from Figure 5 It can be seen intuitively that the anion exchange membrane layer and the anion exchange membrane layer of the bipolar membrane constructed by in-situ growth of nanosheets have uniform membrane thickness. The boundary area between the anion exchange membrane layer and the cation exchange membrane layer is the interface layer, which contains a dense array of iron oxyhydroxide nanosheets, which not only efficiently catalyzes the water dissociation reaction, but also prevents the anion exchange membrane layer from interpenetrating.

[0091] Furthermore, the bipolar membrane prepared by the bipolar membrane preparation method based on in-situ growth of nanosheets of the present invention was subjected to a current-voltage curve test (IV curve), and the specific test process is as follows:

[0092] The bipolar membrane to be tested (a bipolar membrane prepared by the bipolar membrane preparation method based on in-situ growth of nanosheets of the present invention) is placed in a bipolar chamber device for testing the current-voltage curve, and 0.5 mol / L sodium sulfate solution is respectively placed in the chambers on both sides of the bipolar membrane.

[0093] When a reverse bias of a DC electric field is applied to both sides of the bipolar membrane, that is, when the bipolar membrane is placed, the anion exchange membrane layer side faces the anode and the cation exchange membrane layer side faces the cathode, and the test is performed through the linear cyclic voltammetry test program in the electrochemical workstation. During the test, the current gradually increases. Two silver / silver chloride reference electrodes are placed on both sides close to the surface of the bipolar membrane to monitor the voltage drop across the bipolar membrane during the test. The obtained current and voltage values ​​are processed and plotted to obtain the following Figure 6 The IV curve of the bipolar membrane is shown.

[0094] like Figure 6 As shown in Figure 2, the transmembrane voltage of the bipolar membrane increases with the increase of the applied current density. When the applied current density reaches 5 mA / cm 2 When the voltage value increases rapidly, it indicates that the first limiting current density of the bipolar membrane has been reached. When the current density applied on both sides of the bipolar membrane is higher than this value, water dissociation reaction occurs in the interface layer of the bipolar membrane.

[0095] By comparing the IV curves of bipolar membranes, at the same current density (100mA / cm 2 ), for the blank sample (bipolar membrane without in situ growth of nanosheets to construct the interface layer), the voltage required for water dissociation is 2.03V, and for the bipolar membrane of 8h-iron hydroxide (bipolar membrane with 8h in situ growth of nanosheets to construct the interface layer), the water dissociation voltage is 0.97V, indicating that the bipolar membrane prepared by the bipolar membrane preparation method based on in situ growth of nanosheets greatly reduces the voltage required for water dissociation compared with the blank sample.

[0096] Furthermore, the electrodialysis performance of the bipolar membrane prepared by the bipolar membrane preparation method based on in-situ growth of nanosheets of the present invention was tested. The specific test process is as follows:

[0097] The bipolar membrane to be tested (a bipolar membrane prepared by the bipolar membrane preparation method based on in situ grown nanosheets of the present invention) is placed in a membrane stack assembly used for electrodialysis testing. In order to detect the water dissociation performance of the bipolar membrane, the bipolar membrane is placed with its anion exchange membrane layer side facing the anode and its cation exchange membrane layer side facing the cathode during the test.

[0098] The membrane stack of the electrodialysis device is arranged in the order of "anode electrode plate / cation exchange membrane / bipolar membrane / anion exchange membrane / cathode electrode plate". The monopolar membrane (anion exchange membrane and cation exchange membrane) and the bipolar membrane are combined to form a membrane stack in order to prevent the acid and alkali solution produced by the bipolar membrane electrodialysis from leaking into the electrode chamber during the test, resulting in deviations in the calculation of acid and alkali concentrations.

[0099] The monopolar membranes used in the membrane stack of the electrodialysis device are all commercial membranes. The electrode chamber uses 1L of 0.5mol / L sodium sulfate solution, the cathode and anode chambers are connected in series, and the acid chamber and the alkali chamber use 200mL of 0.5mol / L sodium sulfate solution. The current density used in the bipolar membrane electrodialysis operation process is 100mA / cm 2 The test time is 3 hours, and sampling is carried out every 0.5 hours to test the concentration of acid and alkali produced.

[0100] According to the obtained changes in the voltage of the electrodialysis membrane stack device with the concentration of the acid chamber and the alkali chamber over time, a bipolar membrane electrodialysis performance diagram is obtained, such as Figure 7 shown.

[0101] Please refer to Figure 7 The concentrations of the acid chamber and the base chamber in the bipolar membrane electrodialysis increased with the extension of the running time, indicating that the bipolar membrane carried out the water dissociation reaction stably and efficiently during the test. Comparing the concentrations of acid and base produced by the blank sample and the 8h-iron oxyhydroxide bipolar membrane during the entire electrodialysis running time, the acid and base concentrations produced by the 8h-iron oxyhydroxide bipolar membrane were always higher than those of the blank sample, and the bipolar membrane electrodialysis membrane stack device voltage was lower than the device voltage required for the blank sample during the entire test process. After the 3h bipolar membrane electrodialysis test was completed, the concentration produced by the 8h-iron oxyhydroxide bipolar membrane was 0.39mol / L.

[0102] Furthermore, the bipolar membrane prepared by the bipolar membrane preparation method based on in-situ growth of nanosheets of the present invention was tested for water dissociation stability in a neutral system. The specific test process is as follows:

[0103] The bipolar membrane prepared by the bipolar membrane preparation method based on in-situ growth of nanosheets of the present invention is placed in a bipolar chamber glass device used for stability testing, and a 0.5 mol / L sodium sulfate solution is poured on both sides of the bipolar membrane to be tested. When a DC reverse bias is applied to both sides of the bipolar membrane to be tested, that is, the anion exchange membrane layer of the bipolar membrane to be tested is facing the anode and the cation exchange membrane layer is facing the cathode, a constant current of 50 mA / cm is applied using an electrochemical workstation. 2, the water dissociation voltage of the bipolar membrane is monitored with the silver / silver chloride reference electrode at the position near the membrane surface on both sides of the bipolar membrane to be tested. The voltage value monitored is plotted against the working time to obtain the following: Figure 8 The bipolar membrane water dissociation time-voltage curve is shown.

[0104] Please refer to Figure 8 When a constant current of 50 mA / cm is applied on both sides of the bipolar membrane 2 During the 12-hour test, the voltage required for water dissociation of the 8h-iron oxyhydroxide bipolar membrane was stable between 0.74 and 0.77 V, indicating that the bipolar membrane prepared by the bipolar membrane preparation method based on in situ grown nanosheets of the present invention has good stability. It shows that the introduction of iron oxyhydroxide nanosheet arrays into the bipolar membrane interface layer by in situ growth can make the catalyst and the membrane layer closely bonded, thereby improving the stability of the bipolar membrane during operation and avoiding the problem of increased water dissociation voltage due to catalyst shedding.

[0105] Combining all the above test results, it can be concluded that the bipolar membrane prepared by the bipolar membrane preparation method based on in situ grown nanosheets of the present invention, the hydroxyl iron oxide nanosheet array obtained by in situ growth is introduced into the interface layer as a catalyst, and the prepared bipolar membrane is characterized by scanning electron microscopy and tested for current-voltage curve performance, electrodialysis acid and alkali production performance, and water dissociation stability under constant current. According to the results, it can be obtained that the voltage required for water dissociation is significantly reduced by introducing the hydroxyl iron oxide nanosheet array obtained by in situ growth as a catalyst into the interface layer.

[0106] Compared with the same current density (100mA / cm 2 ), for the blank sample (bipolar membrane without in-situ growth of nanosheets to construct the interface layer), the voltage required for water dissociation is 2.03V, and for the 8h-iron oxyhydroxide bipolar membrane (bipolar membrane with 8h in-situ growth of nanosheets to construct the interface layer), the water dissociation voltage is 0.97V, indicating that the bipolar membrane prepared by the bipolar membrane preparation method of in-situ growth of iron oxyhydroxide nanosheets to construct the interface layer greatly reduces the voltage required for water dissociation compared with the blank sample. During the test process of up to 12 hours, the voltage required for water dissociation of the 8h-iron oxyhydroxide bipolar membrane is stable between 0.74-0.77V, indicating that the bipolar membrane prepared by the bipolar membrane preparation method based on in-situ growth of nanosheets has good stability.

[0107] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a bipolar membrane based on in-situ grown nanosheets, characterized in that: The steps include: A) casting a sulfonic acid polyphenylene ether cation exchange membrane liquid on a substrate, and heating the substrate on which the membrane liquid is cast until part of the sulfonic acid groups in the membrane liquid are cross-linked to obtain a cross-linked cation exchange membrane layer; the sulfonic acid polyphenylene ether cation exchange membrane liquid comprises sulfonic acid polyphenylene ether powder particles and an organic solvent; the mass concentration of the sulfonic acid polyphenylene ether powder particles in the sulfonic acid polyphenylene ether cation exchange membrane liquid is 3% to 9%; the heating temperature is 60 to 90° C., and the heating time is 15 to 96 hours; B) soaking one side of the cross-linked cation exchange membrane layer in an alkaline potassium ferrate solution to obtain a bipolar membrane interface layer of hydroxyl iron nanosheet arrays; the mass concentration of potassium ferrate in the alkaline potassium ferrate solution is 0.001 to 0.05 mol / L; the alkaline potassium ferrate solution is specifically obtained by mixing potassium ferrate and an alkaline solution and centrifuging; the concentration of the alkaline solution is 1 to 12 mol / L; the centrifugal speed is 3000 to 12000 rpm, and the centrifugal time is 3 to 10 min; The soaking time is 0.5 to 24 hours; C) spraying quaternary amine type polyphenylene ether anion exchange membrane liquid on the interface layer of the bipolar membrane, and drying to obtain the bipolar membrane.

2. The preparation method according to claim 1, characterized in that: Step A) The thickness of the cross-linked cation exchange membrane layer is 30-70 μm.

3. The preparation method according to claim 1, characterized in that: Step C) The method for preparing the quaternary amine type polyphenylene ether anion exchange membrane liquid is specifically as follows: The brominated polyphenylene ether reacts with an amine organic substance to undergo a quaternization reaction, and the solution after the reaction is precipitated in a precipitant, and the precipitate is dissolved again to obtain a quaternary amine type polyphenylene ether anion exchange membrane liquid; The amine organic matter is a tertiary amine organic matter; the bromination degree of the brominated polyphenylene ether is 20% to 50%.

4. The preparation method according to claim 1, characterized in that: Step C) The mass concentration of the quaternary ammonium polyphenylene ether in the quaternary ammonium polyphenylene ether anion exchange membrane liquid is 2% to 7%.

5. The preparation method according to claim 1, characterized in that: Step C) The thickness of the quaternary amine polyphenylene ether anion exchange membrane layer is 8-45 μm.

6. A bipolar membrane based on in-situ grown nanosheets, characterized in that: The method is prepared according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Preparation method of bipolar membrane and bipolar membrane

    CN110898861A

  • Bipolar membrane preparation method based on electrostatic self-assembly, and bipolar membrane

    CN110898862A

  • Synthetic method of iron oxyhydroxide nanosheet array

    CN111268740A

  • Process for oil field operation wastewater treatment and treatment system

    CN111547896A

  • Novel dipolar membrane and use thereof in electrolysis preparation of ferrate

    CN1865509A