A LCP film and its preparation method and application

Through the combined process of blow molding film formation method and annealing treatment, the problem of insufficient toughness of LCP films was solved, and a high-rigid and high-toughness LCP film was prepared for use in the earphone diaphragm, which improved the sound quality and processing efficiency.

CN114889174BActive Publication Date: 2024-11-22ZHUHAI WANTONG SPECIAL ENG PLASTICS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210240758.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-10
Publication Date
2024-11-22
Estimated Expiration
2042-03-10

AI Technical Summary

Technical Problem

The films made of existing LCP materials have poor toughness and are difficult to be used in earphone diaphragms, especially during the pressing process, and heat treatment leads to a decrease in Young's modulus, making it difficult to have both high rigidity and good toughness.

Method used

The LCP material is extruded by blow molding film formation method and annealed at a specific temperature. Combined with blow molding and annealing process, the elongation of breaking and maintaining high Young's modulus is improved, and the LCP with high rigidity and toughness is prepared. film.

Benefits of technology

The LCP film prepared by this method has a Young's modulus ≥7.8 GPa and an elongation rate of break of ≥10%. It is suitable for earphone diaphragms, which improves sound quality and processing yield, and avoids the problems of excessive heat treatment time and material softening.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003541181400000031
    Figure BDA0003541181400000031
  • Figure BDA0003541181400000041
    Figure BDA0003541181400000041
  • Figure BDA0003541181400000051
    Figure BDA0003541181400000051
Patent Text Reader

Abstract

The present invention discloses an LCP film and a preparation method and application thereof. The preparation method of the LCP film of the present invention comprises the following steps: adding an LCP material to an extruder, extruding through a die head, blow-molding into a film, and then annealing to obtain the LCP film; the process of the annealing treatment is: placing the film at a temperature of Tc‑20 to Tc+15°C for 1 to 30 minutes, and then cooling it to room temperature at a cooling rate of 1 to 10°C / min under the protection of an inert gas. Combining the processes of blow molding and annealing, the LCP material is blown into a film, and then heat-insulated and cooled at a specific temperature, so that an LCP film with good elongation at break can be obtained, and the LCP film still maintains excellent rigidity. The LCP film is applied to the diaphragm of an earphone to make the sound quality of the earphone better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of liquid crystal macromolecular polymer films, and more specifically to an LCP film and a preparation method and application thereof. Background Art

[0002] With the development of mobile communication technology, consumers are increasingly using mobile communication devices with voice functions, and headphones have become an indispensable device in daily life and work. As the sound-generating unit of headphones, the diaphragm has a decisive influence on the sound quality of headphones. Generally speaking, the diaphragm needs to have extremely high rigidity (Young's modulus ≥ 6GPa) and a high loss factor. Among them, a diaphragm with a high Young's modulus can ensure the consistency of the diaphragm movement, and a high loss factor is less likely to cause resonance. A diaphragm with high rigidity and high loss factor makes the headphones sound better.

[0003] Common diaphragm materials include paper diaphragms, wooden diaphragms, metal diaphragms, and plastic diaphragms. Plastic diaphragms are the most commonly used diaphragm materials due to their good plasticity, easy processing, and low cost. LCP materials (liquid crystal polymers) have the advantages of high rigidity, high heat resistance, corrosion resistance, and low moisture absorption, and have a relatively high loss factor and are not prone to resonance, which provides the theoretical basis for becoming an excellent diaphragm material.

[0004] However, LCP films made from LCP materials generally have poor toughness, especially low elongation at break, and are easily crushed during the lamination process when preparing diaphragms. The prior art discloses a method for improving the mechanical properties of liquid crystal polymer products, which treats the LCP film by multiple long-term heating to increase the elongation at break. However, due to the long heat treatment time, the film softens during the heat treatment process, and two layers of PI film are required to protect the LCP film. The processing process is difficult, and only LCP sheet films can be prepared, not LCP roll films. Moreover, due to the long heat treatment time and high temperature, the Young's modulus of the material is greatly reduced, generally ≤3GPa, which makes it difficult to apply to diaphragms.

[0005] Therefore, it is necessary to develop an LCP film that has both high rigidity and good toughness. Summary of the invention

[0006] In order to overcome the defect of insufficient toughness described in the above-mentioned prior art, the present invention provides a method for preparing an LCP film, wherein the LCP material is extruded by a blow molding method and then annealed to obtain an LCP film with high Young's modulus and high elongation at break.

[0007] Another object of the present invention is to provide an LCP film obtained by the above preparation method.

[0008] Another object of the present invention is to provide application of the above LCP film in earphone diaphragms.

[0009] Another object of the present invention is to provide a method for preparing the above-mentioned headphone diaphragm.

[0010] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0011] A method for preparing an LCP film comprises the following steps:

[0012] The LCP material is added to a single screw extruder, melt-mixed, extruded through a die head, blown into a film, and then annealed to obtain the LCP film;

[0013] The annealing process is as follows: heat-treating the film at a temperature of Tc-20 to Tc+15°C for 1 to 30 minutes, and then cooling the film to room temperature at a cooling rate of 1 to 10°C / min under the protection of an inert gas;

[0014] The Tc refers to the crystallization temperature of the LCP material.

[0015] The inventors have found that by combining the blow molding and annealing processes, after the LCP material is blown into a film, it is kept warm at a specific temperature and cooled at a specific speed, so that an LCP film with good elongation at break can be obtained, and the LCP film still maintains excellent rigidity.

[0016] In the preparation method of the present invention, the heat temperature in the annealing treatment is Tc-20 to Tc+15°C, that is, the heat treatment is performed near the crystallization temperature of the LCP film, the LCP molecular chain segments relax and cold crystallize, the crystallization of the molecular chain segments is more perfect, and its elongation at break is improved. By setting a specific annealing treatment procedure, the adhesion between LCP films can be effectively prevented, so the LCP film coil can be directly processed, and the annealing treatment time is greatly shortened, effectively improving the preparation efficiency of the LCP film.

[0017] The inventors have found that during the annealing process, the heat treatment temperature should not be too high or too low. If the temperature is too low, there will be no improvement in the elongation at break; if the temperature is too high, the LCP film will be severely softened and the layers will stick together.

[0018] Preferably, the extrusion temperature is Tm to Tm+20° C., wherein Tm is the melting point of the LCP material.

[0019] The detection method of Tm and Tc is as follows: the LCP material is detected by differential scanning calorimeter, the temperature is increased from room temperature to 30°C above the melting point at a heating rate of 20°C / min, the temperature is then decreased to 25°C at 20°C / min, and finally the temperature is increased to 30°C above the melting point at 20°C / min; the lowest point of the crystallization peak in the first cooling curve is taken as the crystallization temperature Tc, and the highest point of the melting peak in the second heating curve is taken as the melting point Tm.

[0020] Preferably, the melting point of the LCP material is 250-350°C.

[0021] More preferably, the melting point of the LCP material is 235-325°C.

[0022] Preferably, the blow molding process is: inflation ratio 5-8, stretching ratio 3-8.

[0023] Preferably, the inert gas is nitrogen and / or argon.

[0024] Preferably, the annealing process is: placing the film at a temperature of Tc-10 to Tc+10°C for 5 to 20 minutes, and then cooling it to room temperature at a cooling rate of 3 to 8°C / min under inert gas protection.

[0025] The present invention also protects the LCP film prepared by the above preparation method.

[0026] The Young's modulus of the LCP film is ≥7.8 GPa, and the elongation at break is ≥10%.

[0027] The LCP film prepared by the preparation method of the present invention has a high Young's modulus and a suitable elongation at break.

[0028] Generally speaking, the Young's modulus of LCP material is inversely proportional to the elongation at break. The higher the modulus, the harder the material and the smaller the elongation at break. The diaphragm requires the material to have a high modulus and a suitable elongation at break in order to obtain excellent sound quality and a good processing yield.

[0029] Therefore, the present invention is not intended to obtain an LCP film with extremely high elongation at break, but to improve the elongation at break without reducing the Young's modulus of the LCP film.

[0030] The present invention also protects the application of the above LCP film in earphone diaphragms.

[0031] The present invention also protects a method for preparing the above-mentioned earphone diaphragm, comprising the following steps:

[0032] The LCP film is placed in two layers of protective films, pressed into shape, and the protective films are removed to obtain the earphone diaphragm.

[0033] Preferably, the material of the protective film is one or more of PET, PI, PTFE or PEEK.

[0034] Preferably, the temperature of the compression molding is 130-200° C., the pressure is 0.1-0.3 MPa, and the time is 20-100 s.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] The present invention develops a method for preparing an LCP film and the prepared LCP film. By combining the blow molding and annealing processes, the LCP material is blown into a film, and then the film is kept warm and cooled at a specific temperature, so that an LCP film with good elongation at break can be obtained, and the LCP film still maintains excellent rigidity. The LCP film is applied to the diaphragm of earphones to improve the sound quality of the earphones. DETAILED DESCRIPTION

[0037] The present invention will be further described below in conjunction with specific implementation modes.

[0038] The raw materials in the embodiments and comparative examples can be obtained from commercial sources, as follows:

[0039]

[0040] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the present technical field.

[0041] Examples 1 to 11

[0042] Examples 1 to 11 provide an LCP film and an earphone diaphragm made using the same. The LCP material used in Examples 1 to 11 is LCP-1, and the LCP film preparation method is as follows:

[0043] LCP-1 is added to a single screw extruder, melt-mixed, extruded through a die head, blown into a film of a certain thickness, rolled up after cooling, and then annealed to obtain an LCP film;

[0044] The thickness of Examples 1 to 10 is 25 μm, and the thickness of Example 11 is 38 μm;

[0045] The process of blow molding is: melt extrusion temperature is A, blow ratio is B, stretch ratio is C;

[0046] The annealing process is as follows: the film is placed under the protection of an inert gas (nitrogen) at a temperature D for a time E, and then cooled to room temperature 25°C at a cooling rate F;

[0047] The specific parameter values ​​of A to F are shown in Table 1.

[0048] Table 1 Parameters of the preparation method of LCP films of Examples 1 to 11

[0049]

[0050] The preparation methods of the earphone diaphragms of Examples 1 to 11 are as follows:

[0051] The LCP films of Examples 1 to 11 were placed in two layers of protective films (made of PET) and pressed together at a temperature of 150° C., a pressure of 0.2 MPa, and a time of 50 seconds. The protective films were then removed to obtain headphone diaphragms.

[0052] Embodiments 12 to 13

[0053] Examples 12 to 13 respectively provide an LCP film, the LCP material used in Example 12 is LCP-2, and the LCP material used in Example 13 is LCP-3. The steps of the preparation method are the same as those in Example 1, wherein the parameter values ​​of A to F are specifically shown in Table 2.

[0054] Table 1 Parameters of the preparation method of LCP films of Examples 12 to 13

[0055]

[0056] The preparation method of the earphone diaphragm of Examples 12 to 13 is as follows:

[0057] The LCP films of Examples 12 and 13 were placed in two layers of protective films (made of PET) respectively, and pressed into shape at a temperature of 150° C., a pressure of 0.2 MPa, and a time of 50 seconds. After removing the protective films, the headphone diaphragms were obtained.

[0058] Comparative Examples 1 to 6

[0059] Comparative Examples 1 to 6 provide a LCP film respectively, and the LCP material used is LCP-1;

[0060] The preparation method of Comparative Example 1 is as follows: LCP-1 is added to a single screw extruder, extruded through a die head, and blown into a film with a thickness of 25 μm, wherein the melt extrusion temperature is 300° C., the blow-up ratio is 5.5, and the stretching ratio is 7.8; after cooling, the film is rolled up to obtain an LCP film, i.e., without annealing treatment;

[0061] The steps of the preparation method of Comparative Examples 2 to 6 are the same as those of Example 1, wherein the parameter values ​​of A to F are specifically shown in Table 3.

[0062] Table 3 Parameters of the preparation method of LCP films of Comparative Examples 1 to 6

[0063]

[0064] The preparation methods of the headphone diaphragms of Comparative Examples 1 to 6 are as follows:

[0065] The LCP films of comparative examples 1 to 6 were respectively placed in two layers of protective films (made of PET), and pressed into shape at a temperature of 150° C., a pressure of 0.2 MPa, and a time of 50 seconds. After the protective films were removed, headphone diaphragms were obtained.

[0066] Performance Testing

[0067] The performance of the LCP films prepared in the above embodiments and comparative examples was tested, and the specific method is as follows:

[0068] Young's modulus: ASTM-D4092-2007 method, using TA's DMA instrument, test temperature 30 ° C, variable frequency scanning, scanning frequency 1 ~ 100 Hz, the storage modulus G' at 1 Hz is the Young's modulus of the material;

[0069] Elongation at break: Using the ASTM D882-2018 method, 10 mm × 15 cm specimens were cut from the LCP film and measured using a universal tensile tester at a tensile speed of 10 mm / min.

[0070] Pressing molding effect: observe the appearance and groove depth of the prepared headphone diaphragm; if the headphone diaphragm is intact and the groove depth is consistent with the mold, the pressing effect is good; if the headphone diaphragm is intact, but the groove depth is shallower than the mold, the pressing effect is average; if the headphone diaphragm is damaged, the pressing effect is poor.

[0071] The test results of Examples 1 to 13 are shown in Table 4, and the test results of Comparative Examples 1 to 6 are shown in Table 5.

[0072] Table 4 Test results of Examples 1 to 13

[0073]

[0074] According to the test results in Table 3, the LCP films prepared in each embodiment of the present invention have good rigidity. Compared with the comparative example 1 which has not been annealed, the degree of rigidity degradation is less. The Young's modulus of the LCP films prepared in each embodiment is ≥7.8 GPa, which is within an acceptable range and can be applied to diaphragms; the toughness is better, the elongation at break is ≥10%, and the pressing effect is good during the preparation of the headphone diaphragm.

[0075] Among Examples 1 to 6, the elongation at break of Example 5 is relatively low, and the Young's modulus of Example 6 is relatively low. Taking into account the rigidity and toughness of the LCP film, the LCP films of Examples 1 to 4 have relatively better comprehensive performance.

[0076] In Examples 1 and 7 to 9, the annealing temperatures during the preparation of the LCP film are different. It can be seen that when the annealing temperature is high (Example 1), the rigidity of the LCP film is deteriorated to a certain extent, and the Young's modulus decreases; when the annealing temperature is low (Example 9), the toughness of the LCP film is improved to a limited extent, and the elongation at break is relatively low.

[0077] Therefore, the annealing process is preferably: placing the film at a temperature of Tc-10 to Tc+10°C for 5 to 20 minutes, and then cooling it to room temperature at a cooling rate of 3 to 8°C / min under inert gas protection.

[0078] According to Example 1 and Examples 10 to 13, within the extrusion temperature range of Tm to Tm+20°C, under different blowing ratios and stretching ratios, or for different LCP materials, the LCP films prepared using the preparation method of the present invention all have good rigidity and toughness.

[0079] Table 5 Test results of comparative examples 1 to 6

[0080]

[0081] In Comparative Example 1, the preparation process of the LCP film does not include annealing treatment, and the toughness of the obtained LCP film is very poor, and the elongation at break is only 6.7%. The obtained diaphragm is damaged during the lamination process, and the lamination effect is poor.

[0082] In Comparative Example 2, the annealing time was too short, and the toughness of the LCP film was not significantly improved. In Comparative Example 3, the annealing time was too long, and although the elongation at break of the LCP film reached 13.7%, the rigidity was seriously deteriorated, and the Young's modulus was only 5.8 GPa.

[0083] According to the test results of Comparative Example 4 and Comparative Example 5, if the cooling rate in the annealing treatment is too fast or the temperature of the heat treatment is too low, an LCP film with good toughness cannot be obtained.

[0084] In Comparative Example 6, the heat treatment temperature in the annealing treatment was too high, resulting in adhesion between the LCP films, making it impossible to unfold the rolled LCP film.

[0085] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A LCP film, characterized in that: The LCP film is made of LCP material, and the Young's modulus of the LCP film is ≥7.8 GPa, and the elongation at break is ≥10%. The preparation method of the LCP film comprises the following steps: The LCP material is added to a single screw extruder, melt-mixed, extruded through a die head, blown into a film, and then annealed to obtain the LCP film; The annealing process is as follows: heat-treating the film at a temperature of Tc-20 to Tc+15°C for 1 to 30 minutes, and then cooling the film to room temperature at a cooling rate of 1 to 10°C / min under the protection of an inert gas; The Tc is the crystallization temperature of the LCP material.

2. The LCP film according to claim 1, characterized in that: The extrusion temperature is Tm~Tm+20°C, where Tm is the melting point of the LCP material.

3. The LCP film according to claim 1, characterized in that: The melting point of the LCP material is 250-350°C.

4. The LCP film according to claim 1, characterized in that: The blow molding process is as follows: the blow ratio is 5-8, and the stretch ratio is 3-8.

5. The LCP film according to claim 1, characterized in that: The annealing process is as follows: placing the film at a temperature of Tc-10 to Tc+10°C for 5 to 20 minutes, and then cooling the film to room temperature at a cooling rate of 3 to 8°C / min under the protection of an inert gas.

6. The LCP film according to claim 1, characterized in that: The inert gas is nitrogen and / or argon.

7. Application of the LCP film according to claim 1 in earphone diaphragms.

8. The method for preparing the earphone diaphragm according to claim 7, characterized in that: The steps include: The LCP film of claim 1 is placed in two layers of protective films, pressed into shape, and then the protective films are removed to obtain the earphone diaphragm.

9. The preparation method according to claim 8, characterized in that: The material of the protective film is one or more of PET, PI, PTFE or PEEK.