Preparation method and application of negative expansion particles with inert SiO2 protective layer

By constructing an inert SiO2 protective layer on the surface of negative expansion particles, the problems of high chemical activity and uncontrollable interface reactions of negative expansion particles are solved, achieving the effect of improving retention rate and joint strength, reducing residual stress and reducing costs.

CN114905186BActive Publication Date: 2024-10-01HARBIN INST OF TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202210396183.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-15
Publication Date
2024-10-01
Estimated Expiration
2042-04-15

AI Technical Summary

Technical Problem

Existing negative expansion particles have high chemical activity and are prone to adverse chemical reactions with the base material, resulting in reaction losses and the formation of brittle compounds, which reduce the mechanical properties and service life of the components.

Method used

A uniform and dense inert SiO2 protective layer is constructed on the surface of the negative expansion particles and prepared through ultrasonic vibration, stirring reaction and sintering steps to avoid direct contact between the negative expansion particles and the base material and inhibit adverse interface reactions.

Benefits of technology

It effectively suppresses adverse interface reactions, improves the retention rate and joint strength of negative expansion particles, reduces residual stress, has low cost and simple operation, and is suitable for most negative expansion particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114905186B_ABST
    Figure CN114905186B_ABST
Patent Text Reader

Abstract

A preparation method and application of negative expansion particles with an inert SiO2 protective layer. The present invention aims to solve the problems of high chemical activity and uncontrollable interface reaction of existing negative expansion particles. Preparation method: 1. Add negative expansion particle powder to a mixed solution of deionized water and alcohol, and obtain a suspension after ultrasonic vibration; 2. Add concentrated ammonia water to the suspension, stir evenly, and then add tetraethyl orthosilicate to carry out stirring reaction; 3. After stirring, centrifuge to collect the solid phase; 4. Place the particle reactants in a muffle furnace for sintering treatment to obtain negative expansion particles with an inert SiO2 protective layer. The present invention avoids direct contact between the negative expansion particles and the parent material by constructing a uniform and dense inert SiO2 protective layer on the surface of the negative expansion particles. On the one hand, it suppresses the adverse reaction between the negative expansion particles and the parent material, and on the other hand, it improves the retention rate of the negative expansion particles in the parent material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and particularly relates to an inert SiO 2 The invention discloses a preparation method and application of negative expansion particles of a protective layer. Background Art

[0002] For components or members made of dissimilar materials, the difference in linear expansion coefficients between different components will lead to the generation of large residual stress, thereby reducing the mechanical properties of the components / members and shortening their service life. A common solution currently used is to reduce the linear expansion coefficient by adding negative expansion coefficient particles to materials with high linear expansion coefficients, thereby reducing the thermal mismatch between components and relieving residual stress.

[0003] However, this method has great limitations: negative expansion particles usually have high chemical activity and can easily undergo violent chemical reactions with the base material. On the one hand, the reaction consumes a large number of negative expansion particles, reducing the retention rate of the particles and resulting in the inability to fully exert the negative expansion effect. On the other hand, the reaction may generate a large number of brittle compounds, resulting in a serious decrease in the mechanical properties of the components / members. Therefore, it is necessary to develop a new method to obtain negative expansion particles with stable chemical properties and controllable interface reactions. Summary of the invention

[0004] The present invention aims to solve the problems of high chemical activity and uncontrollable interface reaction of existing negative expansion particles, and provide an inert SiO 2 The invention discloses a preparation method and application of negative expansion particles of a protective layer.

[0005] The present invention has inert SiO 2 The preparation method of the negative expansion particles of the protective layer is achieved by the following steps:

[0006] 1. Add the negative expansion particle powder into a mixed solution of deionized water and alcohol (anhydrous ethanol), and obtain a suspension after ultrasonic vibration;

[0007] 2. Add concentrated ammonia water to the suspension, stir evenly, then add ethyl orthosilicate and stir to react;

[0008] 3. After the stirring is completed, the solid phase is collected by centrifugation and washed to obtain a granular reactant;

[0009] Fourth, the pelletized reactants are placed in a muffle furnace for sintering at a holding temperature of 100-600°C. After the holding temperature is completed, they are naturally cooled to room temperature to obtain inert SiO 2 Negative expansion particles for the protective layer;

[0010] The negative expansion particle powder in step 1 is ZrW 2 O8 , HfW 2 O 8 、ZrMo 2 O 8 , ZrV 2 O 8 ,ThP 2 O 8 、CeP 2 O 8 Sc 2 W 3 O 12 、Dy 2 W 3 O 12 , Y 2 W 3 O 12 , Er 2 W 3 O 12 , Yb 2 W 3 O 12 、Lu 2 W 3 O 12 , Y 2 Mo 3 O 12 , Er 2 Mo 3 O 12 , Yb 2 Mo 3 O 12 、Lu 2 Mo 3 O 12 Sc 2 Mo 3 O 12 、TaVO 5 、NbVO 5 、CaZrF 6 MgZrF 6 、FeZrF 6 ,CaNbF 6 、TiZrF 6 、LiAlSiO 4 One or more mixed powders.

[0011] The present invention has inert SiO 2 The negative expansion particles of the protective layer are used as auxiliary materials in the solder.

[0012] The present invention proposes a method of preparing an inert SiO 2 The preparation method of the negative expansion particles of the protective layer is to construct a uniform and dense inert SiO2 The protective layer is used to avoid direct contact between the negative expansion particles and the base material. On the one hand, it inhibits the adverse reaction between the negative expansion particles and the base material, and on the other hand, it improves the retention rate of the negative expansion particles in the base material.

[0013] The inert SiO 2 The preparation method of the negative expansion particles of the protective layer mainly includes the following beneficial effects:

[0014] 1. SiO prepared by the present invention 2 The protective layer avoids direct contact between the negative expansion particles and the base material, inhibits adverse interface reactions, avoids the formation of brittle compounds, and improves the strength of the joint.

[0015] 2. SiO 2 The protective layer greatly reduces the reaction loss of the negative expansion particles, improves their retention rate, can give full play to their negative expansion capacity, and reduce residual stress.

[0016] 3. This preparation method has low cost, simple operation, and SiO 2 The layer thickness is controllable and suitable for most negative expansion particles. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 In the first embodiment, Y 2 W 3 O 12 Inert SiO prepared on particle surface 2 High-resolution transmission electron microscopy photograph of the protective layer;

[0018] Figure 2 In Example 1, 5 wt.% Y 2 W 3 O 12 Granular Ag-based solder for joining BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ Backscattered photographs of the joints obtained with AISI 441 stainless steel;

[0019] Figure 3 In Example 1, a 20 wt.% SiO 2 Protective layer Y 2 W 3 O 12 Granular Ag-based solder for joining BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ Backscattered photograph of the joint obtained with AISI 441 stainless steel. DETAILED DESCRIPTION

[0020] Specific implementation method 1: This implementation method has an inert SiO 2 The preparation method of the negative expansion particles of the protective layer is implemented according to the following steps:

[0021] 1. Add the negative expansion particle powder into a mixed solution of deionized water and alcohol, and obtain a suspension after ultrasonic vibration;

[0022] 2. Add concentrated ammonia water to the suspension, stir evenly, then add ethyl orthosilicate and stir to react;

[0023] 3. After the stirring is completed, the solid phase is collected by centrifugation and washed to obtain a granular reactant;

[0024] Fourth, the pelletized reactants are placed in a muffle furnace for sintering at a holding temperature of 100-600°C. After the holding temperature is completed, they are naturally cooled to room temperature to obtain inert SiO 2 Negative expansion particles for the protective layer;

[0025] The negative expansion particle powder in step 1 is ZrW 2 O 8 , HfW 2 O 8 、ZrMo 2 O 8 , ZrV 2 O 8 ,ThP 2 O 8 、CeP 2 O 8 Sc 2 W 3 O 12 、Dy 2 W 3 O 12 , Y 2 W 3 O 12 , Er 2 W 3 O 12 , Yb 2 W 3 O 12 、Lu 2 W 3 O 12 , Y 2 Mo 3 O 12 , Er 2 Mo 3 O 12 , Yb 2 Mo 3 O12 、Lu 2 Mo 3 O 12 Sc 2 Mo 3 O 12 、TaVO 5 、NbVO 5 、CaZrF 6 MgZrF 6 、FeZrF 6 ,CaNbF 6 、TiZrF 6 、LiAlSiO 4 One or more mixed powders.

[0026] In this embodiment, a uniform and dense inert SiO2 is formed on the surface of the negative expansion particles. 2 The protective layer is used to avoid direct contact between the negative expansion particles and the base material. On the one hand, it inhibits the adverse reaction between the negative expansion particles and the base material, and on the other hand, it improves the retention rate of the negative expansion particles in the base material.

[0027] Specific implementation method 2: The difference between this implementation method and specific implementation method 1 is that the average particle size of the negative expansion particle powder described in step 1 is 0.1-10 μm.

[0028] Specific implementation method three: This implementation method is different from specific implementation methods one or two in that the mixed solution described in step one is prepared from anhydrous ethanol and deionized water in a mass ratio of 60:40 to 90:10.

[0029] Specific implementation method 4: This implementation method is different from any one of specific implementation methods 1 to 3 in that the mass ratio of the negative expansion particle powder to the mixed solution in step 1 is (0.2-2):100.

[0030] Specific implementation method five: This implementation method is different from specific implementation methods one to four in that the duration of ultrasonic vibration in step one is 2 to 15 minutes.

[0031] Specific implementation method 6: This implementation method is different from specific implementation methods 1 to 5 in that the volume ratio of concentrated ammonia water to the mixed solution used in step 2 is (1-5):100, and the mass concentration of the concentrated ammonia water is 25%.

[0032] Specific embodiment 7: The difference between this embodiment and any one of specific embodiments 1 to 6 is that in step 2, the volume ratio of ethyl orthosilicate to the mixed solution is (1-5):100.

[0033] Specific implementation eight: This implementation is different from specific implementations one to seven in that the stirring time in step two is 1 to 10 hours.

[0034] Specific embodiment 9: This embodiment is different from any one of specific embodiments 1 to 8 in that in step 4, the temperature is kept at 500° C. for 2 to 3 hours.

[0035] Specific embodiment ten: This embodiment has an inert SiO 2 The negative expansion particles of the protective layer are used as auxiliary materials in the solder.

[0036] Specific embodiment 11: This embodiment uses the inert SiO 2 Negative expansion of protective layer of BaZr particles brazing 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ And the method for stainless steel is as follows:

[0037] According to the mass ratio of (15-25): (75-85), the inert SiO 2 The negative expansion particles of the protective layer are mixed with Ag powder, and the mixed powder is pressed into an Ag-based solder sheet. The Ag-based solder sheet is sandwiched between BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ Between the steel and the stainless steel, a pressure of 0.3 to 0.6 MPa is applied and the brazing connection is performed at a temperature of 900 to 950°C.

[0038] Example: This example has inert SiO 2 The preparation method of the negative expansion particles of the protective layer is implemented according to the following steps:

[0039] 1. Prepare 84g of mixed solution of anhydrous ethanol and deionized water in a mass ratio of 76:24, and add negative expansion particles Y 2 W 3 O 12 The powder was added to the mixed solution, and a suspension was obtained after 5 min of ultrasonic vibration;

[0040] 2. Add 2 mL of concentrated ammonia (mass concentration is 25%) to the suspension, stir evenly, then add 2 mL of ethyl orthosilicate, and stir and react at room temperature for 3 hours;

[0041] 3. After stirring, the particles were separated by centrifuge (3000r / min), and the particle reactants were obtained after washing with alcohol three times;

[0042] Fourth, the pelletized reactants were placed in a muffle furnace for sintering at a holding temperature of 500°C for 2 hours. After the holding period, they were naturally cooled to room temperature to obtain inert SiO 2Negative expansion particles for the protective layer.

[0043] In this embodiment, Y 2 W 3 O 12 The dense SiO prepared on the powder surface 2 coating, which then inhibits the Y 2 W 3 O 12 Reaction of powder with base material.

[0044] pass Figure 1 It can be found that in Y 2 W 3 O 12 A layer of SiO is formed on the powder surface 2 The protective layer is SiO obtained by the method of this embodiment. 2 The protective layer thickness is about 35nm, dense and uniform, and 2 W 3 O 12 Good combination.

[0045] In order to verify that SiO 2 The role of the protective layer is to first remove the unprotected Y 2 W 3 O 12 The particles were mixed with Ag powder in a mass ratio of 5:95 to obtain a Y 2 W 3 O 12 Ag-based solder particles are then pressed into Ag-based solder sheets (solder sheet thickness is 100 microns), and the Ag-based solder sheets are sandwiched between BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ The pressure of 0.4 MPa was applied between the stainless steel and the brazing connection was performed at a connection temperature of 950°C and a holding time of 30 min (the heating and cooling rate was 3°C / min). 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ and AISI 441 stainless steel. Figure 2 It can be found that there is no SiO 2 Protective layer Y 2 W 3 O 12 The powder will be mixed with BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δThe violent reaction generates a brittle compound layer, which directly leads to cracking and failure of the joint.

[0046] Then the SiO 2 Protective layer Y 2 W 3 O 12 The particles were mixed with Ag powder in a mass ratio of 20:80 to obtain the corresponding Ag-based solder, which was pressed into Ag-based solder sheets (the thickness of the solder sheet was 100 μm). The Ag-based solder sheets were sandwiched between BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ The pressure of 0.4 MPa was applied between the stainless steel and the brazing connection was performed at a connection temperature of 950°C and a holding time of 30 min (the heating and cooling rate was 3°C / min). 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ and AISI 441 stainless steel. Figure 3 It can be found that the joint is well formed and no cracks are generated. 2 The protective layer avoids Y 2 W 3 O 12 Powder and BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ The direct contact inhibits the violent interface reaction and avoids the formation of brittle compound layer.

Claims

1. Application of negative expansion particles with an inert SiO2 protective layer, characterized in that The negative expansion particles with an inert SiO2 protective layer are used as auxiliary materials in the brazing material, and the negative expansion particles with an inert SiO2 protective layer are used to braze BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ And the method for stainless steel is as follows: The negative expansion particles with an inert SiO2 protective layer are mixed with Ag powder in a mass ratio of (15-25): (75-85), and the mixed powder is pressed into an Ag-based solder sheet. The Ag-based solder sheet is sandwiched between BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ Between the steel and stainless steel, apply a pressure of 0.3~0.6MPa and perform brazing connection at a temperature of 900~950℃; The preparation method of the negative expansion particles having an inert SiO2 protective layer is achieved by the following steps:

1. Add the negative expansion particle powder into a mixed solution of deionized water and alcohol, and obtain a suspension after ultrasonic vibration; 2. Add concentrated ammonia water to the suspension, stir evenly, then add ethyl orthosilicate and stir to react; 3. After the stirring is completed, the solid phase is collected by centrifugation and washed to obtain a granular reactant; Fourth, the particle reactants are placed in a muffle furnace for sintering at a holding temperature of 100-600°C, and naturally cooled to room temperature after the holding is completed to obtain negative expansion particles with an inert SiO2 protective layer; The negative expansion particle powder in step 1 is ZrW2O8, HfW2O8, ZrMo2O8, ZrV2O8, ThP2O8, CeP2O8, Sc2W3O 12 、Dy2W3O 12 、Y2W3O 12 、Er2W3O 12 、Yb2W3O 12 、Lu2W3O 12 、Y2Mo3O 12 、Er2Mo3O 12 、Yb2Mo3O 12 、Lu2Mo3O 12 Sc2Mo3O 12 , TaVO5, NbVO5, CaZrF6, MgZrF6, FeZrF6, CaNbF6, TiZrF6, LiAlSiO4 or a mixed powder of more than one.

2. The use according to claim 1, characterized in that The average particle size of the negative expansion particle powder described in step 1 is 0.1-10 μm.

3. The use according to claim 1, characterized in that The mass ratio of the negative expansion particle powder to the mixed solution described in step 1 is (0.2~2):

100.

4. The use according to claim 1, characterized in that The duration of ultrasonic vibration in step 1 is 2 to 15 minutes.

5. The use according to claim 1, characterized in that The volume ratio of the concentrated ammonia water used in step 2 to the mixed solution is (1-5):100, and the mass concentration of the concentrated ammonia water is 25%.

6. The use according to claim 1, characterized in that In step 2, the volume ratio of ethyl orthosilicate to the mixed solution is (1-5):

100.

7. The use according to claim 1, characterized in that The stirring time in step 2 is 1 to 10 hours.

8. The use according to claim 1, characterized in that In step 4, keep the temperature at 500°C for 2 to 3 hours.

Citation Information

Patent Citations

  • Method for preparing nano SiO2 hollow ball composite materials based on polyimide base body

    CN103923332A

  • Preparation method of SiO2-coated core-shell structure catalyst

    CN104056633A

  • Preparation method of self-lubricating ceramic cutting tool material comprising spherical nanometer silicon dioxide coated hexagonal boron nitride composite powder

    CN104844178A

  • Method for preparing graphene toughened silicon carbide ceramic composite material

    CN105801154A

  • Silicon / titanium dioxide / carbon composite material for negative electrode of lithium-ion battery and preparation method of silicon / titanium dioxide / carbon composite material

    CN108598416A