A kind of anti-ultraviolet thermal insulation glass and preparation method thereof

Porous with high compressive strength, good thermal insulation and UV resistance are prepared by melting tris(phthalate ethoxysilane) phosphate with aluminum glycine with base glass powder and scraping specific compounds on the surface. 保温玻璃,解决了现有技术中性能兼顾难的问题。

CN114956590BActive Publication Date: 2024-11-05HENAN XINZHENGFANG ELECTRONIC TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210482518.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-05
Publication Date
2024-11-05
Estimated Expiration
2042-05-05

AI Technical Summary

Technical Problem

In the prior art, when preparing porous insulation glass, it is difficult to take into account both the compressive strength and the insulation performance, and the installation process consumes a lot of manpower and material resources, which affects the appearance.

Method used

Insulating glass is prepared by mixing tris(phthalate ethoxysilane) phosphate with aluminum glycine and melting it with basic glass powder, and the surface is scraped with butanoketone formamide phenylethanol and chloroacetone o-hydroxybenzene Amidine, an ultraviolet insulation glass is formed by using electrically assisted steam scraping.

Benefits of technology

It improves the compressive strength and thermal insulation performance of the glass, while enhancing the UV resistance and corrosion resistance, forming a uniform pore structure and metal film layer, improving the overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003628139050000121
    Figure BDA0003628139050000121
Patent Text Reader

Abstract

The invention discloses an anti-ultraviolet thermal insulation glass and a preparation method thereof, and relates to the technical field of glass. When preparing the anti-ultraviolet thermal insulation glass, the invention first mixes tris(phthalylethoxysilane) phosphate and aluminum glycinate, and melts them together with basic glass powder to form an aluminum phosphate network and polyimide, and the polyimide is decomposed at high temperature to form a large number of uniform pores to prepare the thermal insulation glass; then, butyric acid formamide phenylethanol and chloroacetone-based o-hydroxybenzene formamidine are mixed and scraped on the upper surface of the thermal insulation glass, and electrically assisted steam scraping is used to form o-hydroxyphenyl triazine compounds and metal porphyrin films to prepare the anti-ultraviolet thermal insulation glass; the anti-ultraviolet thermal insulation glass prepared by the invention has good compressive strength, thermal insulation, anti-ultraviolet performance and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass, in particular to an anti-ultraviolet thermal insulation glass and a preparation method thereof. Background Art

[0002] Glass is the most common material in our daily life and is closely related to people's production activities. With the development of modern science and technology, glass technology and the improvement of people's living standards, the function of architectural glass is no longer just to meet the lighting requirements, but also to have the characteristics of light regulation, thermal insulation, bulletproof, anti-theft, fire prevention, radiation protection, anti-electromagnetic interference, artistic decoration, etc.

[0003] With the development of science and technology and the improvement of the quality of life, people have more and more demands for the thermal insulation of glass as a home decoration material. People also solve this problem by preparing vacuum glass. Vacuum glass is to seal two pieces of flat glass on all sides, evacuate the gap between them and seal the exhaust holes. The gap between the two pieces of glass is 0.1-0.2mm, which makes the thickness of the thermal insulation glass thicker, which consumes a lot of manpower and material resources during installation, and often affects the overall aesthetics of home decoration after installation. Therefore, porous thermal insulation glass came into being. In the prior art, porous thermal insulation glass is generally prepared by acid immersion or alkali immersion to form a large number of channels in the glass, which leads to a sharp decrease in the compressive strength of the glass. Therefore, preparing glass with good thermal insulation and good compressive strength has become a major problem in the current glass manufacturing industry.

[0004] The present invention pays attention to this problem and solves this problem by preparing UV-proof thermal insulation glass. Summary of the invention

[0005] The object of the present invention is to provide an anti-ultraviolet thermal insulation glass and a preparation method thereof, so as to solve the problems existing in the prior art.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A method for preparing an anti-ultraviolet thermal insulation glass. The anti-ultraviolet thermal insulation glass is prepared by mixing butyric acid carboxamidophenylethanol and chloroacetone-based o-hydroxybenzamide and applying the mixture on the upper surface of the thermal insulation glass, and then applying the mixture by electrically assisted steam. The thermal insulation glass is prepared by mixing tri(phthaloylethoxysilane) phosphate and aluminum glycinate, and then melting the mixture with basic glass powder.

[0008] Furthermore, the preparation method of the anti-ultraviolet thermal insulation glass comprises the following preparation steps:

[0009] (1) At 24-26°C, tri(phthalylethoxysilane) phosphate and ethanol are mixed in a mass ratio of 1:3-1:5, stirred at 1200-1300 r / min for 20-30 min, then 0.6-0.8 times the mass of tri(phthalylethoxysilane) phosphate and a 3-5% ethanol aqueous solution are added dropwise at 60-80 drops / min, the stirring is continued at 60-80°C for 2-4 h, 3-4 times the mass of tri(phthalylethoxysilane) phosphate aluminum glycinate is added, and then 20% sodium hydroxide solution is added dropwise at 60-80 drops / min to adjust the pH to 8-10, the stirring is continued for 3-4 h, and 1-3 times the mass of tri(phthalylethoxysilane) phosphate N,N-dihydrochloric acid is added dropwise at -16--14°C under argon protection at 40-60 drops / min. Methylacetamide, continue stirring for 1 to 3 hours, then heat to -1 to 1 ° C at 2 to 4 ° C, continue stirring for 0.8 to 1.2 hours, continue to heat to 14 to 16 ° C, continue stirring for 1 to 3 hours, and age at room temperature for 23 to 25 hours. Then, add 0.05 to 0.07 times the mass of tri(phthalylethoxysilane) phosphate basic glass powder, stir at 2200 to 2300 r / min for 2 to 4 hours, and put it into a quartz crucible. , in a box-type resistance furnace, heating to 100-300°C at 4-6°C / min, keeping the temperature for 1.5-2.5h, continuing to heating to 400-600°C, keeping the temperature for 20-40min, cooling to 100-300°C at 10-20°C / min, keeping the temperature for 1-3h, continuing to cool to room temperature, washing with deionized water 2-4 times, drying at 40-60°C for 1-3h, and naturally cooling to room temperature to prepare thermal insulation glass;

[0010] (2) at room temperature, mixing butyric acid methylaminophenyl ethanol, chloroacetonyl o-hydroxybenzamide and dimethyl sulfoxide in a mass ratio of 1:0.3:4 to 1:0.5:6, stirring at 500 to 700 r / min for 20 to 40 min, adding 0.001 to 0.002 times the mass of butyric acid methylaminophenyl ethanol, adding cesium carbonate to adjust the pH to 7 to 9, then heating to 100 to 130° C. at 3 to 5° C. / min, and continuing stirring for 15 to 17 h to prepare a scraping solution;

[0011] (3) Place the insulating glass in a sealed container at room temperature for 2 to 4 minutes. 3 / min, pass 100-120℃ steam for 5-7min, then use a scraper to scrape 60-80nm thick scraping liquid on the upper surface of the insulation glass at 30-40℃, add 0.1-0.3 times the mass of the insulation glass dichlorothionyl at 40-60 drops / min, treat for 40-60min under 2400-2500MHz and 700-900W microwave conditions, then add 10-20% mass fraction of sodium hydroxide solution at 40-60 drops / min, adjust pH to 7-9, continue microwave treatment for 80-120min, continue to add 0.03-0.05 times the mass of the insulation glass sulfur trioxide, continue microwave for 60-80min, then corona treat for 2-3 times at a speed of 6-8m / s, cool naturally to room temperature, wash with deionized water for 2-4 times, and bake at 40-60℃ for 1-3h to prepare UV-proof insulation glass.

[0012] Further, the preparation method of the basic glass powder in step (1) is as follows: cullet, lead tetroxide, zirconium oxide and lime are mixed in a mass ratio of 1:0.5:0.15:0.15 to 1:0.7:0.25:0.25, stirred at 100 to 300 r / min for 10 to 20 min, then dried at 40 to 60° C. for 1 to 3 h, put into a ball mill for 23 to 25 h, and passed through a 180 to 220 mesh sieve. , put it into a quartz crucible, heat it to 400-500℃ in a box-type resistance furnace at 4-6℃ / min, keep it warm for 1.5-2.5h, continue to heat it to 700-800℃, keep it warm for 3-5h, take it out and quickly pour it into 10-20℃ cold water to cool for 40-60min, then bake it at 40-60℃ for 1-3h, put it into a ball mill and mill it for 23-25h, pass it through a 180-220 mesh sieve, and prepare basic glass powder.

[0013] Furthermore, the preparation method of tri(ethoxysilylphthalate) phosphate in step (1) is as follows: at room temperature and under argon protection conditions, tri(ethoxychlorosilane) phosphate and phthalic anhydride are mixed in a mass ratio of 1:0.8 to 1:1, stirred at 500 to 700 r / min for 15 to 25 min, and then aluminum chloride with a mass of 0.02 to 0.04 times that of chlorobutyric acid formamide is added, the temperature is reduced from 3 to 5°C to 0 to 4°C, and stirring is continued for 7 to 9 hours to prepare tri(ethoxysilylphthalate) phosphate.

[0014] Furthermore, the preparation method of tri(ethoxychlorosilane) phosphate is as follows: phosphorus oxychloride and dihydroxyethoxychlorosilane are mixed in a mass ratio of 1:5 to 1:7 at 30 to 40°C and 10 to 20Pa, stirred at 500 to 700 r / min for 30 to 50 min, and dichlorosulfuryl with a mass of 0.1 to 0.3 times the mass of phosphorus oxychloride is added at 40 to 60 drops / min, and stirring is continued for 2 to 4 hours to prepare tri(ethoxychlorosilane) phosphate.

[0015] Furthermore, the preparation method of the ketobutyric acid methylaminophenylethanol in step (2) is as follows: at room temperature and under argon protection, chlorobutyric acid methylaminophenylethanol and phenylethanol are mixed in a mass ratio of 1:0.6 to 1:0.8, stirred at 500 to 700 r / min for 15 to 25 min, and then 0.01 to 0.03 times the mass of chlorobutyric acid methylaminophenylethanol is added, and the temperature is reduced from 3 to 5°C to 0 to 4°C, and stirring is continued for 7 to 9 hours to prepare ketobutyric acid methylaminophenylethanol.

[0016] Furthermore, the preparation method of the chlorobutyric acid formamide is as follows: at 25 to 27° C. and under argon protection conditions, 4-chloro-3-carbonylbutyric acid and formamide are mixed in a mass ratio of 1:0.5 to 1:0.7, stirred at 500 to 700 r / min for 20 to 30 min, then nano-titanium dioxide with a mass of 0.07 to 0.09 times that of 4-chloro-3-carbonylbutyric acid is added, the temperature is raised to 80 to 100° C. at 9 to 10° C. / min, and stirring is continued for 2 to 4 h to prepare chlorobutyric acid formamide.

[0017] Furthermore, the preparation method of the chloroacetone-based o-hydroxybenzamidine in step (2) is as follows: at room temperature and under argon protection, dichloroacetone and o-hydroxybenzamidine are mixed in a mass ratio of 1:0.5 to 1:0.7, stirred at 500 to 700 r / min for 20 to 30 min, and then 0.01 to 0.03 times the mass of dichloroacetone is added with aluminum chloride, the temperature is reduced from 3 to 5°C to 0 to 4°C, and stirring is continued for 7 to 9 hours to prepare chloroacetone-based o-hydroxybenzamidine.

[0018] Furthermore, the preparation method of the o-hydroxybenzamide is as follows: at 30-40° C., salicylaldehyde oxime, ethanol, and deionized water are mixed in a mass ratio of 1:8:3-1:10:5, stirred at 500-700 r / min for 30-50 min, then nickel powder of 0.002-0.004 times the mass of salicylaldehyde oxime is added, put into a reactor at 0.6-0.8 MPa, heated to 60-80° C. at 3-5° C. / min, and stirred for 8-10 h under argon protection to prepare o-hydroxybenzamide.

[0019] Furthermore, the current intensity of the corona treatment in step (3) is 7 to 9A.

[0020] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0021] When preparing the anti-ultraviolet thermal insulation glass, the present invention firstly mixes tri(phthalylethoxysilane) phosphate and aluminum glycinate, and melts the mixture with basic glass powder to prepare the thermal insulation glass; then, butyric acid formamide phenylethanol and chloroacetone-based o-hydroxybenzene formamidine are mixed and scraped on the upper surface of the thermal insulation glass, and electrically assisted steam scraping is used to prepare the anti-ultraviolet thermal insulation glass.

[0022] Firstly, tri(ethoxysilylphthalate) phosphate is hydrolyzed and condensed to form phosphoric acid and silica gel, aluminum glycinate is hydrolyzed to form aluminum hydroxide gel and glycine, part of the phosphoric acid reacts with the aluminum hydroxide gel to form an aluminum phosphate network in the insulating glass, thereby enhancing the compressive strength of the insulating glass; the phthalic acid on the tri(ethoxysilyl) phosphate reacts with the amino group on the aluminum glycinate to form polyimide, which carbonizes and decomposes to form carbon dioxide, thereby forming a large number of carbon dioxide bubbles, which escape to form a large number of pores, and part of the phosphoric acid is dehydrated to form phosphorus pentoxide, which can reduce the surface tension of the batch material, effectively prevent the bursting of bubbles, and form a large number of uniform pore structures inside the insulating glass, thereby enhancing the thermal insulation performance of the insulating glass.

[0023] Secondly, butyric acid formamide phenylethanol is hydrolyzed to form formamide and butyric acid phenylethanol, chloroacetone o-hydroxybenzamide reacts and polymerizes with the aldehyde group in part of the formamide to form o-hydroxyphenyl triazine compounds and ammonia. When irradiated with ultraviolet rays of a certain wavelength, the o-hydroxyphenyl triazine compounds absorb light energy, break the hydrogen bonds and open the chelate rings, and then convert the absorbed energy into the form of fluorescence, phosphorescence or heat, and release or consume it in a non-radiative manner, thereby enhancing the anti-ultraviolet performance of the anti-ultraviolet thermal insulation glass; part of the phosphorus pentoxide on the surface of the thermal insulation glass is combined to form phosphoric acid, which reacts with the hydroxyl group in butyric acid phenylethanol to form phosphate ester, and the butyric acid phenylethanol is firmly grafted on the surface of the thermal insulation glass. At the same time, ammonia reacts with butyric acid phenylethanol and chloroacetone o-hydroxybenzamide to form benzopyrrole, and part of the formamide reacts with benzopyrrole to form porphyrin, which quickly captures free aluminum ions in the glass to form a metal film layer, thereby enhancing the corrosion resistance of the anti-ultraviolet thermal insulation glass. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0025] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the UV-proof thermal insulation glass prepared in the following examples as follows:

[0026] Compressive strength: The compressive strength of the UV-proof thermal insulation glass prepared in the embodiment and the comparative example of the same length and width was measured according to GB / T6552 standard.

[0027] Thermal insulation: The thermal insulation properties of the anti-ultraviolet thermal insulation glasses prepared in the embodiment and the comparative example of the same mass were measured by testing the heat transfer coefficient according to GB / T8484.

[0028] Anti-ultraviolet performance: The anti-ultraviolet thermal insulation glass prepared in the embodiment and the comparative example of the same length and width was irradiated with 365nm ultraviolet light for 8 hours continuously, with an interval of 10 hours. After 5 cycles, the compressive strength after ultraviolet aging was measured according to GB / T6552 standard to determine the anti-ultraviolet performance.

[0029] Corrosion resistance: Take the same mass of the anti-ultraviolet thermal insulation glass prepared in the embodiment and the comparative example and mix it with 98% concentrated sulfuric acid in a mass ratio of 1:10 and soak it for 2 days. After taking it out, wash it with deionized water 3 times, put it into a 40°C oven for 0.5h, and naturally cool it to room temperature to obtain acid-immersed anti-ultraviolet thermal insulation glass. Weigh the mass of the acid-immersed anti-ultraviolet thermal insulation glass, and the corrosion rate = 100% * (mass of the anti-ultraviolet thermal insulation glass - mass of the acid-immersed anti-ultraviolet thermal insulation glass) / mass of the anti-ultraviolet thermal insulation glass.

[0030] Example 1

[0031] A method for preparing ultraviolet-proof thermal insulation glass, the method for preparing ultraviolet-proof thermal insulation glass comprising the following preparation steps:

[0032] (1) Cullet glass, lead tetroxide, zirconium oxide and lime are mixed in a mass ratio of 1:0.5:0.15:0.15, stirred at 100 r / min for 10 min, then dried at 40°C for 1 h, put into a ball mill for 23 h, passed through a 180-mesh sieve, put into a quartz crucible, heated to 400°C at 4°C / min in a box-type resistance furnace, kept warm for 1.5 h, continued to heat to 700°C, kept warm for 3 h, taken out and quickly poured into 10°C cold water for cooling for 40 min, dried at 40°C for 1 h, put into a ball mill for 23 h, passed through a 180-mesh sieve, and prepared basic glass powder;

[0033] (2) Phosphorus oxychloride and dihydroxyethoxysilyl chloride were mixed at a mass ratio of 1:5 at 30°C and 10Pa, stirred at 500r / min for 30min, and dichlorothioyl (0.1 times the mass of phosphorus oxychloride) was added dropwise at 40 drops / min, and stirring was continued for 2h to prepare tri(ethoxysilyl chloride) phosphate; at room temperature and under argon protection, tri(ethoxysilyl chloride) phosphate and phthalic anhydride were mixed at a mass ratio of 1:0.8, stirred at 500r / min for 15min, and then methyl chlorobutyrate was added. The mixture was stirred at 1200 r / min for 20 min, and then a 3% aqueous ethanol solution with a mass fraction of 0.6 times that of tri(phthalylethoxysilane) phosphate was added at a rate of 60 drops / min, and stirring was continued at 60°C for 2 h. Add aluminum glycinate with a mass of 3 times that of tri(phthaloylethoxysilyl) phosphate, then add a 20% sodium hydroxide solution at a rate of 60 drops / min to adjust the pH to 8, continue stirring for 3 hours, and at -16°C and argon protection, add N,N-dimethylacetamide with a mass of 1 times that of tri(phthaloylethoxysilyl) phosphate at a rate of 40 drops / min, continue stirring for 1 hour, then heat up to -1°C at 2°C, continue stirring for 0.8 hours, continue heating to 14°C, continue stirring for 1 hour, and store at room temperature. After 23 hours of melting, add basic glass powder with a mass of 0.05 times of tri(phthalylethoxysilane) phosphate, stir at 2200r / min for 2 hours, put into a quartz crucible, heat to 100°C at 4°C / min in a box-type resistance furnace, keep warm for 1.5 hours, continue to heat to 400°C, keep warm for 20 minutes, cool to 100°C at 10°C / min, keep warm for 1 hour, continue to cool to room temperature, wash twice with deionized water, bake at 40°C for 1 hour, and naturally cool to room temperature to prepare thermal insulation glass;

[0034] (3) At 30°C, salicylaldehyde oxime, ethanol and deionized water were mixed in a mass ratio of 1:8:3, stirred at 500 r / min for 30 min, then nickel powder (0.002 times the mass of salicylaldehyde oxime) was added, put into a 0.6MPa reactor, heated to 60°C at 3°C / min, and stirred for 8 h under argon protection to prepare o-hydroxybenzamide; at room temperature and argon protection, dichloroacetone and o-hydroxybenzamide were mixed in a mass ratio of 1:0.5, stirred at 500 r / min for 20 min, then aluminum chloride (0.01 times the mass of dichloroacetone) was added, cooled to 0°C at 3°C, and stirred for 7 h to prepare chloroacetonyl o-hydroxybenzamide; at 25°C and argon protection, 4-chloro-3-carbonylbutyric acid and formamide were mixed in a mass ratio of 1:0.5, stirred at 500 r / min for 20 min, then 4-chloro- -3-carbonylbutyric acid mass 0.07 times of nano titanium dioxide, 9 ℃ / min to 80 ℃, continue to stir for 2h, prepare chlorobutyric acid formamide; at room temperature and argon protection conditions, chlorobutyric acid formamide and phenylethanol are mixed in a mass ratio of 1: 0.6, stirred at 500r / min for 15min, then added with aluminum chloride 0.01 times the mass of chlorobutyric acid formamide, cooled to 0 ℃ at 3 ℃, and continued to stir for 7h to prepare butyric acid formamide phenylethanol; at room temperature, butyric acid formamide phenylethanol, chloroacetonyl o-hydroxybenzamide and dimethyl sulfoxide are mixed in a mass ratio of 1: 0.3: 4, stirred at 500r / min for 20min, 0.001 times the mass of butyric acid formamide phenylethanol rubidium chloride is added, cesium carbonate is added to adjust the pH to 7, then heated to 100 ℃ at 3 ℃ / min, and continued to stir for 15h to prepare a scraping liquid;

[0035] (4) At room temperature, place the insulating glass in a sealed container at 2m 3 / min, pass 100°C steam for 5min, then use a scraper to scrape a 60nm thick scraping liquid on the upper surface of the insulating glass at 30°C, add dichlorothionyl in an amount of 0.1 times the mass of the insulating glass at 40 drops / min, treat at 2400MHz and 700W microwave conditions for 40min, then add 10% sodium hydroxide solution in an amount of 40 drops / min, adjust the pH to 7, continue microwave treatment for 80min, continue to add sulfur trioxide in an amount of 0.03 times the mass of the insulating glass, continue microwave treatment for 60min, then corona treat twice at a speed of 6m / s and a current intensity of 7A, cool naturally to room temperature, wash twice with deionized water, and bake at 40°C for 1h to prepare UV-proof insulating glass.

[0036] Example 2

[0037] A method for preparing ultraviolet-proof thermal insulation glass, the method for preparing ultraviolet-proof thermal insulation glass comprising the following preparation steps:

[0038] (1) Cullet glass, lead tetroxide, zirconium oxide and lime are mixed in a mass ratio of 1:0.6:0.2:0.2, stirred at 200 r / min for 15 min, then dried at 50° C. for 2 h, put into a ball mill for 24 h, passed through a 200-mesh sieve, put into a quartz crucible, heated to 450° C. at 5° C. / min in a box-type resistance furnace, kept warm for 2 h, continued to heat to 750° C., kept warm for 4 h, taken out and quickly poured into 15° C. cold water for cooling for 50 min, dried at 50° C. for 2 h, put into a ball mill for 24 h, passed through a 200-mesh sieve, and prepared basic glass powder;

[0039] (2) Phosphorus oxychloride and dihydroxyethoxysilyl chloride were mixed at a mass ratio of 1:6 at 35°C and 15 Pa, stirred at 600 r / min for 40 min, and dichlorosulfuryl (0.2 times the mass of phosphorus oxychloride) was added at 50 drops / min, and stirring was continued for 3 h to prepare tri(ethoxysilyl chloride) phosphate; at room temperature and under argon protection, tri(ethoxysilyl chloride) phosphate and phthalic anhydride were mixed at a mass ratio of 1:0.9, stirred at 600 r / min for 20 min, and then methyl chlorobutyrate was added. The mixture was stirred at 1250r / min for 25 min, and then a 4% aqueous ethanol solution with a mass fraction of 0.7 times the mass of tri(phthalylethoxysilane) phosphate was added at a rate of 70 drops / min, and stirring was continued at 70°C for 3 hours. Add aluminum glycinate with a mass of 3.5 times that of tri(phthaloylethoxysilyl) phosphate, then add a 20% sodium hydroxide solution at a rate of 70 drops / min to adjust the pH to 9, continue stirring for 3.5 hours, and at -15°C and argon protection, add N,N-dimethylacetamide with a mass of 2 times that of tri(phthaloylethoxysilyl) phosphate at a rate of 50 drops / min, continue stirring for 2 hours, then heat up to 0°C at a rate of 3°C, continue stirring for 1 hour, continue heating to 15°C, continue stirring for 2 hours, and cool to room temperature. After aging for 24 hours, add basic glass powder with a mass of 0.06 times of tri(phthalylethoxysilane)phosphate, stir at 2250r / min for 3 hours, put into a quartz crucible, heat to 200°C at 5°C / min in a box-type resistance furnace, keep warm for 2 hours, continue to heat to 500°C, keep warm for 30 minutes, cool to 200°C at 15°C / min, keep warm for 2 hours, continue to cool to room temperature, wash 3 times with deionized water, bake at 50°C for 2 hours, and naturally cool to room temperature to prepare thermal insulation glass;

[0040] (3) At 35°C, salicylaldehyde oxime, ethanol, and deionized water were mixed in a mass ratio of 1:9:4, stirred at 600 r / min for 40 min, and then 0.003 times the mass of salicylaldehyde oxime nickel powder was added, placed in a 0.7 MPa reactor, heated to 70°C at 4°C / min, and stirred for 9 h under argon protection to prepare o-hydroxybenzamide; dichloroacetone and o-hydroxybenzamide were mixed at room temperature and under argon protection. The amidines were mixed in a mass ratio of 1:0.6, stirred at 600r / min for 25min, and then 0.02 times the mass of dichloroacetone was added with aluminum chloride, cooled from 4°C to 2°C, and stirred for 8h to prepare chloroacetonyl o-hydroxybenzamidine; at 26°C and argon protection, 4-chloro-3-carbonylbutyric acid and formamide were mixed in a mass ratio of 1:0.6, stirred at 600r / min for 25min, and then 4-chloro-3 -0.08 times the mass of carbonyl butyric acid nano-titanium dioxide, heated to 90°C at 9.5°C / min, and continued to stir for 3h to prepare chlorobutyric acid formamide; at room temperature and argon protection conditions, chlorobutyric acid formamide and phenylethanol were mixed in a mass ratio of 1:0.7, stirred at 600r / min for 20min, and then aluminum chloride with a mass of 0.02 times the mass of chlorobutyric acid formamide was added, cooled to 2°C at 4°C, and continued to stir for 8h to prepare butyric acid formamide phenylethanol; at room temperature, butyric acid formamide phenylethanol, chloroacetonyl o-hydroxybenzamide and dimethyl sulfoxide were mixed in a mass ratio of 1:0.5:5, stirred at 600r / min for 30min, rubidium chloride with a mass of 0.0015 times the mass of butyric acid formamide phenylethanol was added, cesium carbonate was added to adjust the pH to 8, and then the temperature was raised to 115°C at 4°C / min, and continued to stir for 16h to prepare a scraping liquid;

[0041] (4) At room temperature, place the insulating glass in a sealed container and 3 / min, pass 110℃ steam for 6min, then use a scraper to scrape 70nm thick scraping liquid on the upper surface of the insulating glass at 35℃, add dichlorothionyl in an amount of 0.2 times the mass of the insulating glass at 50 drops / min, treat at 2450MHz and 800W microwave conditions for 50min, then add 15% mass fraction of sodium hydroxide solution at 50 drops / min, adjust the pH to 8, continue microwave treatment for 100min, continue to add 0.04 times the mass of the insulating glass sulfur trioxide, continue microwave for 70min, then corona treat twice at a speed of 7m / s and a current intensity of 8A, cool naturally to room temperature, wash three times with deionized water, and bake at 50℃ for 2h to prepare UV-proof insulating glass.

[0042] Example 3

[0043] A method for preparing ultraviolet-proof thermal insulation glass, the method for preparing ultraviolet-proof thermal insulation glass comprising the following preparation steps:

[0044] (1) Cullet glass, lead tetroxide, zirconium oxide and lime are mixed in a mass ratio of 1:0.7:0.25:0.25, stirred at 300 r / min for 20 min, then dried at 60° C. for 3 h, put into a ball mill for 25 h, passed through a 220-mesh sieve, put into a quartz crucible, heated to 500° C. at 6° C. / min in a box-type resistance furnace, kept warm for 2.5 h, continued to heat to 800° C., kept warm for 5 h, taken out and quickly poured into 20° C. cold water for cooling for 60 min, then dried at 60° C. for 3 h, put into a ball mill for 25 h, passed through a 220-mesh sieve, and prepared basic glass powder;

[0045] (2) Phosphorus oxychloride and dihydroxyethoxysilyl chloride were mixed at a mass ratio of 1:7 at 40°C and 20Pa, stirred at 700 r / min for 50 min, and dichlorosulfuryl (0.3 times the mass of phosphorus oxychloride) was added at 60 drops / min, and stirring was continued for 4 h to prepare tri(ethoxysilyl chloride) phosphate; at room temperature and under argon protection, tri(ethoxysilyl chloride) phosphate and phthalic anhydride were mixed at a mass ratio of 1:1, stirred at 700 r / min for 25 min, and then chlorobutyric acid formyl was added. The mixture was stirred at 1300 r / min for 30 min, and then a 5% aqueous ethanol solution with a mass fraction of 0.8 times that of the phosphate tris(o-phthaloylethoxysilane) was added at a rate of 80 drops / min, and stirring was continued at 80°C for 4 h. Aluminum glycinate with a mass of 4 times that of tri(phthaloethoxysilyl) phosphate was added, and then a 20% sodium hydroxide solution was added at a rate of 80 drops / min to adjust the pH to 10, and stirring was continued for 4 hours. At -14°C and argon protection, N,N-dimethylacetamide with a mass of 3 times that of tri(phthaloethoxysilyl) phosphate was added at a rate of 60 drops / min, and stirring was continued for 3 hours. The mixture was then heated from 4°C to 1°C, and stirring was continued for 1.2 hours. The mixture was then heated to 16°C, and stirring was continued for 3 hours. The mixture was aged at room temperature. After 25 hours, add basic glass powder with a mass of 0.07 times of tri(phthalylethoxysilane)phosphate, stir at 2300r / min for 4 hours, put into a quartz crucible, heat to 300°C at 6°C / min in a box-type resistance furnace, keep warm for 2.5 hours, continue to heat to 600°C, keep warm for 40 minutes, cool to 300°C at 20°C / min, keep warm for 3 hours, continue to cool to room temperature, wash 4 times with deionized water, bake at 60°C for 3 hours, and naturally cool to room temperature to prepare insulating glass;

[0046] (3) At 40°C, salicylaldehyde oxime, ethanol, and deionized water were mixed in a mass ratio of 1:10:5, stirred at 700 r / min for 50 min, and then 0.004 times the mass of salicylaldehyde oxime nickel powder was added, placed in a 0.8 MPa reactor, heated to 80°C at 5°C / min, and stirred for 10 h under argon protection to prepare o-hydroxybenzamide; dichloroacetone and o-hydroxybenzamide were mixed at room temperature and under argon protection. Benzamidine was mixed in a mass ratio of 1:0.7, stirred at 700r / min for 30min, and then 0.03 times the mass of dichloroacetone was added with aluminum chloride, cooled from 5°C to 4°C, and stirred for 9h to prepare chloroacetonyl o-hydroxybenzamidine; 4-chloro-3-carbonylbutyric acid and formamide were mixed in a mass ratio of 1:0.7 at 27°C and argon protection, stirred at 700r / min for 30min, and then 4-chloro- -3-carbonylbutyric acid mass 0.09 times of nano titanium dioxide, 10 ℃ / min to 100 ℃, continue stirring for 4h, prepare chlorobutyric acid formamide; at room temperature and argon protection conditions, chlorobutyric acid formamide and phenylethanol are mixed in a mass ratio of 1: 0.8, stirred at 700r / min for 25min, then added with aluminum chloride 0.03 times the mass of chlorobutyric acid formamide, cooled to 4 ℃ at 5 ℃, continued stirring for 9h, and prepared ketoacetic acid formamidophenylethanol; at room temperature, ketoacetic acid formamidophenylethanol, chloroacetonyl o-hydroxybenzamide and dimethyl sulfoxide are mixed in a mass ratio of 1: 0.5: 6, stirred at 700r / min for 40min, 0.002 times the mass of ketoacetic acid formamidophenylethanol rubidium chloride is added, cesium carbonate is added to adjust the pH to 9, then heated to 130 ℃ at 5 ℃ / min, continued stirring for 17h, and prepared a scraping liquid;

[0047] (4) At room temperature, place the insulating glass in a sealed container at 4m 3 / min, pass 120℃ steam for 7min, then use a scraper to scrape 80nm thick scraping liquid on the upper surface of the insulating glass at 40℃, add dichlorothionyl in an amount of 0.3 times the mass of the insulating glass at 60 drops / min, treat at 2500MHz and 900W microwave conditions for 60min, then add 20% sodium hydroxide solution in an amount of 60 drops / min, adjust the pH to 9, continue microwave treatment for 120min, continue to add sulfur trioxide in an amount of 0.05 times the mass of the insulating glass, continue microwave treatment for 80min, then corona treat 3 times at a speed of 8m / s and a current intensity of 9A, cool naturally to room temperature, wash 4 times with deionized water, and bake at 60℃ for 3h to prepare UV-proof insulating glass.

[0048] Comparative Example 1

[0049] The difference between Comparative Example 1 and Example 2 is only the difference in step (2). Step (2) is modified as follows: at 25°C, ethyl silicate and ethanol are mixed in a mass ratio of 1:4, stirred at 1250r / min for 25min, then 0.7 times the mass of ethyl silicate and a 4% ethanol aqueous solution are added at 70 drops / min, stirring is continued at 70°C for 3h, 3.5 times the mass of ethyl silicate aluminum glycinate is added, and then 20% sodium hydroxide solution is added at 70 drops / min to adjust the pH to 9, stirring is continued for 3.5h, and ethyl silicate is added at 50 drops / min at -15°C and under argon protection. 2 times of N, N-dimethylacetamide, continue stirring for 2h, then heat to 0℃ at 3℃, continue stirring for 1h, continue heating to 15℃, continue stirring for 2h, age at room temperature for 24h, put in basic glass powder with 0.06 times the mass of ethyl silicate, stir at 2250r / min for 3h, put in a quartz crucible, heat to 200℃ at 5℃ / min in a box-type resistance furnace, keep warm for 2h, continue heating to 500℃, keep warm for 30min, cool to 200℃ at 15℃ / min, keep warm for 2h, continue cooling to room temperature, wash 3 times with deionized water, bake at 50℃ for 2h, cool naturally to room temperature, and prepare thermal insulation glass. The remaining preparation steps are the same as those in Example 2.

[0050] Comparative Example 2

[0051] The difference between Comparative Example 2 and Example 2 is only the difference in step (2). Step (2) is modified as follows: at 35° C. and 15 Pa, phosphorus oxychloride and dihydroxyethoxychlorosilane are mixed in a mass ratio of 1:6, stirred at 600 r / min for 40 min, dichlorosulfuryl with a mass of 0.2 times that of phosphorus oxychloride is added dropwise at 50 drops / min, and stirring is continued for 3 h to prepare tri(ethoxychlorosilane) phosphate; at room temperature and under argon protection, tri(ethoxychlorosilane) phosphate and phthalic anhydride are mixed in a mass ratio of 1:0 .9, stirred at 600r / min for 20min, then added aluminum chloride with a mass of 0.03 times that of chlorobutyric acid formamide, cooled from 4°C to 2°C, and continued stirring for 8h to prepare tri(phthalylethoxysilane) phosphate; at 25°C, tri(phthalylethoxysilane) phosphate and ethanol were mixed in a mass ratio of 1:4, stirred at 1250r / min for 25min, and then 0.7 times the mass of tri(phthalylethoxysilane) phosphate was added at 70 drops / min. times the mass fraction of 4% ethanol aqueous solution, continue stirring at 70°C for 3h, then add 20% mass fraction of sodium hydroxide solution at 70 drops / min to adjust the pH to 9, continue stirring for 3.5h, at -15°C and argon protection conditions, add N,N-dimethylacetamide twice the mass of tri(phthalylethoxysilane) phosphate at 50 drops / min, continue stirring for 2h, then heat to 0°C at 3°C, continue stirring for 1h, continue to heat to 15°C, continue stirring for 2h, and cool to room temperature. After aging for 24 hours, add basic glass powder with a mass of 0.06 times of tri(phthalylethoxysilane)phosphate, stir at 2250r / min for 3 hours, put into a quartz crucible, heat to 200°C at 5°C / min in a box-type resistance furnace, keep warm for 2 hours, continue to heat to 500°C, keep warm for 30 minutes, cool to 200°C at 15°C / min, keep warm for 2 hours, continue to cool to room temperature, wash 3 times with deionized water, bake at 50°C for 2 hours, and naturally cool to room temperature to prepare thermal insulation glass. The remaining preparation steps are the same as in Example 2.

[0052] Comparative Example 3

[0053] The difference between Comparative Example 3 and Example 2 is only the difference in step (3). Step (3) is modified as follows: at 26°C and argon protection conditions, 4-chloro-3-carbonylbutyric acid and formamide are mixed in a mass ratio of 1:0.6, stirred at 600 r / min for 25 min, then 0.08 times the mass of 4-chloro-3-carbonylbutyric acid The nano-titanium dioxide is added, the temperature is raised to 90°C at 9.5°C / min, and stirring is continued for 3h to prepare chlorobutyric acid formamide; at room temperature and argon protection conditions, chlorobutyric acid formamide and phenylethanol are mixed in a mass ratio of 1:0.7, Stir at 600r / min for 20min, then add aluminum chloride with a mass of 0.02 times of chlorobutyric acid formamide, cool to 2°C at 4°C, continue stirring for 8h, and prepare ketoacetic acid formamide phenylethanol; at room temperature, ketoacetic acid formamide phenylethanol and dimethyl sulfoxide are mixed in a mass ratio of 1:5, stirred at 600r / min for 30min, rubidium chloride with a mass of 0.0015 times of ketoacetic acid formamide phenylethanol is added, cesium carbonate is added to adjust the pH to 8, then the temperature is raised to 115°C at 4°C / min, and stirring is continued for 16h to prepare a scraping liquid. The remaining preparation steps are the same as in Example 2.

[0054] Comparative Example 4

[0055] The difference between Comparative Example 4 and Example 2 is only the difference in step (3). Step (3) is modified as follows: at 35°C, salicylaldehyde oxime, ethanol, and deionized water are mixed in a mass ratio of 1:9:4, stirred at 600r / min for 40min, then 0.003 times the mass of salicylaldehyde oxime nickel powder is added, put into a 0.7MPa reactor, heated to 70°C at 4°C / min, and stirred for 9h under argon protection to prepare o-hydroxybenzamide; at room temperature and under argon protection, dichloroacetone and o-hydroxybenzamide are mixed in a mass ratio of 1:0.6 , stirring at 600r / min for 25min, then adding aluminum chloride with a mass of 0.02 times of dichloroacetone, cooling at 4°C to 2°C, and continuing stirring for 8h to prepare chloroacetone-based o-hydroxybenzamide; at room temperature, chloroacetone-based o-hydroxybenzamide and dimethyl sulfoxide were mixed at a mass ratio of 0.5:5, stirred at 600r / min for 30min, 0.0015 times of the mass of chloroacetone-based o-hydroxybenzamide rubidium chloride was added, cesium carbonate was added to adjust the pH to 8, then the temperature was raised to 115°C at 4°C / min, and stirring was continued for 16h to prepare a scraping liquid. The remaining preparation steps are the same as in Example 2.

[0056] Comparative Example 5

[0057] The difference between Comparative Example 5 and Example 2 is only the difference in step (4), which is modified as follows: at room temperature, place the insulating glass in a sealed container and heat it for 3 minutes. 3 / min, 110°C steam was introduced for 6min, then at 35°C, a scraping liquid with a thickness of 70nm was scraped on the upper surface of the insulation glass using a scraper, 0.2 times the mass of the insulation glass was added with dichlorothionyl at 50 drops / min, and the glass was treated for 50min under microwave conditions of 2450MHz and 800W, then 15% sodium hydroxide solution was added at 50 drops / min, the pH was adjusted to 8, the microwave treatment was continued for 100min, 0.04 times the mass of the insulation glass was added with sulfur trioxide, the microwave treatment was continued for 70min, the glass was naturally cooled to room temperature, washed with deionized water for 3 times, and baked at 50°C for 2h to prepare the UV-proof insulation glass. The remaining preparation steps are the same as those in Example 2.

[0058] Effect example

[0059] Table 1 below shows the analysis results of the compressive strength, thermal insulation, UV protection and corrosion resistance of the UV-proof thermal insulation glass prepared by Examples 1 to 3 of the present invention and Comparative Examples 1 to 5.

[0060] Table 1

[0061]

[0062] It can be found from Table 1 that the compressive strength, thermal insulation, UV protection and corrosion resistance of the UV-proof thermal insulation glass prepared in Examples 1, 2 and 3 are relatively strong; from the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 1, it can be found that the use of tri(phthalylethoxysilane) phosphate to prepare thermal insulation glass can form an aluminum phosphate network and polyimide, and the polyimide is decomposed at high temperature to form a large number of uniform pores, and the compressive strength and thermal insulation of the prepared UV-proof thermal insulation glass are relatively strong; from the experimental data of Examples 1, 2, 3 and Comparative Example 2, it can be found that the use of aluminum glycinate to prepare thermal insulation glass can form an aluminum phosphate network and polyimide, and the polyimide is decomposed at high temperature to form a large number of uniform pores, and the UV-proof thermal insulation glass prepared later can form a metal film layer, and the compressive strength of the prepared UV-proof thermal insulation glass is relatively strong. , thermal insulation and corrosion resistance are strong; from the experimental data of Examples 1, 2, 3 and Comparative Example 3, it can be found that the use of chloroacetone-based o-hydroxybenzenecarboxamidine to prepare UV-proof thermal insulation glass can form o-hydroxyphenyl triazine compounds and a metal film layer, and the prepared UV-proof thermal insulation glass has strong UV protection and corrosion resistance; from the experimental data of Examples 1, 2, 3 and Comparative Example 4, it can be found that the use of butyric acid carboxamide-phenylethanol to prepare UV-proof thermal insulation glass can form o-hydroxyphenyl triazine compounds and a metal film layer, and the prepared UV-proof thermal insulation glass has strong UV protection and corrosion resistance; from the experimental data of Examples 1, 2, 3 and Comparative Example 5, it can be found that the use of electric-assisted steam scraping to prepare UV-proof thermal insulation glass can form a metal film layer, and the prepared UV-proof thermal insulation glass has strong corrosion resistance.

[0063] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing UV-proof thermal insulation glass, characterized in that: The preparation method of the anti-ultraviolet thermal insulation glass comprises the following preparation steps: (1) At 24-26°C, tri(phthaloylethoxysilyl) phosphate and ethanol were mixed in a mass ratio of 1:3-1:5, stirred at 1200-1300 r / min for 20-30 min, then a 3-5% aqueous ethanol solution with a mass fraction of 0.6-0.8 times the mass of tri(phthaloylethoxysilyl) phosphate was added dropwise at 60-80 drops / min, the mixture was stirred at 60-80°C for 2-4 h, aluminum glycinate with a mass fraction of 3-4 times the mass of tri(phthaloylethoxysilyl) phosphate was added, and then a 20% sodium hydroxide solution with a mass fraction of 60-80 drops / min was added to adjust the pH to 8-10, the mixture was stirred for 3-4 h, and N,N-dimethylethyl ether with a mass fraction of 1-3 times the mass of tri(phthaloylethoxysilyl) phosphate was added dropwise at 40-60 drops / min under argon protection. amide, continue stirring for 1~3h, then heat to -1~1℃ at 2~4℃ / min, continue stirring for 0.8~1.2h, continue heating to 14~16℃, continue stirring for 1~3h, after aging at room temperature for 23~25h, add basic glass powder with a mass of 0.05~0.07 times that of tri(phthalylethoxysilane)phosphate, stir at 2200~2300r / min for 2~4h, and put it into a quartz crucible. , in a box-type resistance furnace, the temperature is raised to 100-300°C at 4-6°C / min, kept at this temperature for 1.5-2.5h, then the temperature is further raised to 400-600°C, kept at this temperature for 20-40min, then the temperature is lowered to 100-300°C at 10-20°C / min, kept at this temperature for 1-3h, then the temperature is further lowered to room temperature, then the glass is washed 2-4 times with deionized water, and then the glass is dried at 40-60°C for 1-3h, and then naturally cooled to room temperature to obtain the heat-insulating glass; The preparation method of the basic glass powder is as follows: mixing broken glass, lead tetroxide, zirconium oxide and lime in a mass ratio of 1:0.5:0.15:0.15-1:0.7:0.25:0.25, stirring at 100-300 r / min for 10-20 min, then drying at 40-60° C. for 1-3 h, putting into a ball mill for 23-25 ​​h, passing through a 180-220 mesh sieve, putting into a quartz crucible, heating to 400-500° C. at 4-6° C. / min in a box-type resistance furnace, keeping the temperature for 1.5-2.5 h, continuing to heat to 700-800° C., keeping the temperature for 3-5 h, taking out and quickly pouring into 10-20° C. cold water to cool for 40-60 m in, and then dried at 40-60°C for 1-3h, put into a ball mill for 23-25h, and passed through a 180-220 mesh sieve to prepare a basic glass powder; the preparation method of tri(ethoxysilyl phthalate) phosphate is as follows: at room temperature and under argon protection conditions, tri(ethoxychlorosilane) phosphate and phthalic anhydride are mixed in a mass ratio of 1:0.8-1:1, stirred at 500-700r / min for 15-25min, and then aluminum trichloride with a mass of 0.02-0.04 times of chlorobutyric acid formamide is added, and the temperature is reduced to 0-4°C at 3-5°C / min, and stirring is continued for 7-9h to prepare tri(ethoxysilyl phthalate) phosphate; (2) At room temperature and under argon protection, dichloroacetone and o-hydroxybenzamide were mixed in a mass ratio of 1:0.5-1:0.7, stirred at 500-700 r / min for 20-30 min, and then 0.01-0.03 times the mass of dichloroacetone of aluminum chloride was added, the temperature was lowered to 0-4°C at 3-5°C / min, and stirring was continued for 7-9 h to prepare chloroacetonyl o-hydroxybenzamide; at room temperature and under argon protection, chlorobutyric acid formamide and phenylethanol were mixed in a mass ratio of 1:0.6-1:0.8, stirred at 500-700 r / min for 15-25 min, and then 0.01 times the mass of chlorobutyric acid formamide was added. ~0.03 times of aluminum trichloride, cooling to 0~4°C at 3~5°C / min, continuing stirring for 7~9h to prepare butyric acid formamidophenylethanol; at room temperature, butyric acid formamidophenylethanol, chloroacetone-based o-hydroxybenzamide and dimethyl sulfoxide are mixed in a mass ratio of 1:0.3:4~1:0.5:6, stirring at 500~700r / min for 20~40min, adding rubidium chloride with a mass of 0.001~0.002 times of butyric acid formamidophenylethanol, adding cesium carbonate to adjust the pH to 7~9, then heating to 100~130°C at 3~5°C / min, continuing stirring for 15~17h to prepare a scraping liquid; (3) At room temperature, place the insulating glass in a sealed container, and pass 100-120°C steam at 2-4 m³ / min for 5-7 min. Then, at 30-40°C, use a scraper to scrape a 60-80 nm thick scraping solution on the surface of the insulating glass. Add 0.1-0.3 times the mass of the insulating glass with dichlorothionyl at 40-60 drops / min. Treat the glass with a microwave at 2400-2500 MHz and 700-900 W for 40-60 min. Then, heat the glass with 400-2500 MHz microwave. A sodium hydroxide solution with a mass fraction of 10-20% was added at 0-60 drops / min, the pH was adjusted to 7-9, the microwave treatment was continued for 80-120 min, sulfur trioxide in an amount of 0.03-0.05 times the mass of the insulating glass was continued to be added, the microwave was continued for 60-80 min, and then corona treatment was performed at a speed of 6-8 m / s for 2-3 times. After naturally cooling to room temperature, the solution was washed with deionized water for 2-4 times, and dried at 40-60°C for 1-3 h to prepare UV-proof insulating glass.

2. The method for preparing the UV-proof thermal insulation glass according to claim 1, characterized in that: The preparation method of tri(ethoxychlorosilane) phosphate in step (1) is as follows: phosphorus oxychloride and dihydroxyethoxychlorosilane are mixed in a mass ratio of 1:5-1:7 at 30-40°C and 10-20Pa, stirred at 500-700r / min for 30-50min, dichlorosulfuryl in an amount of 0.1-0.3 times the mass of phosphorus oxychloride is added dropwise at 40-60 drops / min, and stirring is continued for 2-4h to prepare tri(ethoxychlorosilane) phosphate.

3. The method for preparing the UV-proof thermal insulation glass according to claim 1, characterized in that: The preparation method of chlorobutyric acid formamide in step (2) is as follows: at 25-27° C. and argon protection conditions, 4-chloro-3-carbonylbutyric acid and formamide are mixed in a mass ratio of 1:0.5-1:0.7, stirred at 500-700 r / min for 20-30 min, then 0.07-0.09 times the mass of 4-chloro-3-carbonylbutyric acid of nano-titanium dioxide is added, the temperature is raised to 80-100° C. at 9-10° C. / min, and stirring is continued for 2-4 h to prepare chlorobutyric acid formamide.

4. The method for preparing the UV-proof thermal insulation glass according to claim 1, characterized in that: The preparation method of the o-hydroxybenzamide described in step (2) is as follows: at 30-40° C., salicylaldehyde oxime, ethanol and deionized water are mixed in a mass ratio of 1:8:3-1:10:5, stirred at 500-700 r / min for 30-50 min, then nickel powder of 0.002-0.004 times the mass of salicylaldehyde oxime is added, put into a reactor at 0.6-0.8 MPa, and heated to 60-80° C. at 3-5° C. / min. Under argon protection, stirring is continued for 8-10 h to prepare o-hydroxybenzamide.

5. The method for preparing the UV-proof thermal insulation glass according to claim 1, characterized in that: The current intensity of the corona treatment in step (3) is 7-9A.

Citation Information

Patent Citations

  • Porcelain film composition based on siloxane and preparation method thereof

    CN101343428A

  • Ultraviolet light curing glass paint and preparation method thereof

    CN101514274A

  • Anti-frost cold and heat-resistant heat preservation anti ultraviolet glass used for high-rise building and preparation method thereof

    CN103043923A

  • Coated substrate and process of preparation

    CN112119049A

  • Ultraviolet-shielding glass and method for producing the same

    JP2005263513A